A niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material and a preparation method thereof and a lithium-ion battery containing the same
Through ball milling and heat treatment of aluminum-based hydrotalcite nanosheets and nickel-cobalt-manganese ternary precursors, uniform doping of niobium elements is achieved, and the structural instability and circulation of niobium-doped nickel-cobalt-manganese lithium aluminate quaternary materials are solved. The problem of insufficient performance improves the cycling and electrochemical properties of the material.
Patent Information
- Application Number
- CN202111285057.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-01
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-11-01
AI Technical Summary
The existing niobium-doped nickel-cobalt-manganese-aluminate quaternary materials are difficult to achieve uniform doping of niobium elements under high pressure oxygen, resulting in unstable material structure, insufficient circulation performance and thermal stability, and it is difficult to obtain shapes in conventional spray drying methods. The spherical microparticles with uniform appearance affect the density and processing properties of the material.
Aluminum-based hydrotalcite nanosheets and nickel-cobalt-manganese ternary precursors are ball milled, followed by heat treatment under an oxygen atmosphere, and the coordinated diffusion of transition metal elements and Nb-O chemical bonds are used to achieve uniform doping and distribution of niobium elements, reducing the material The difficulty of synthesis is to regulate the proportion of four elements to improve material performance.
Through this method, niobium elements are uniformly distributed in the quaternary material, which significantly improves the cyclic performance and capacity retention of the material, ensuring the long-term stability and electrochemical properties of the material.
Smart Images

Figure CN116072858B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of preparation of positive electrode materials for lithium-ion batteries, and in particular, to a niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material, a preparation method thereof, and a lithium-ion battery comprising the same. Background Art
[0002] Since its commercialization, lithium-ion batteries have attracted widespread attention from all walks of life and are currently the main energy supplier for new energy vehicles. As the core component of the battery and the bottleneck of energy density, the performance of lithium-ion battery cathode materials directly affects the various performance indicators of lithium-ion batteries. Therefore, cathode materials with high specific capacity, good safety, and long cycle life have attracted much attention. 1-x-y-z Co x Mn y Al z As a quaternary positive electrode material, O2 (NCMA) combines some of the advantages of NCM and NCA materials, and has the advantages of high specific capacity and good safety performance. However, due to the shortcomings of the layered high-nickel material itself, such as insufficient structural stability and high surface residual alkali, high-nickel quaternary materials face shortcomings such as poor cycle stability and insufficient thermal stability. Metal ion doping is one of the effective methods to improve the structural stability of layered materials. Introducing niobium into nickel-cobalt-manganese-aluminum quaternary materials can improve the stability of positive electrode materials, expand lithium ion insertion / extraction channels, and reduce the degree of cation mixing, thereby improving material performance.
[0003] The conventional niobium doping method is to directly mix niobium compounds such as niobium oxide with the quaternary precursor, and then add a lithium source for lithium calcination. 5+ Due to the large ion radius, niobium elements are usually difficult to diffuse evenly into the quaternary material structure to achieve the ideal doping effect. Chinese patent CN111584872A discloses a method for preparing niobium-doped NCM811 ternary material. In order to achieve effective doping of niobium elements, high-temperature calcination is required under high-pressure oxygen at 20 to 100 atm, which places extremely high demands on production equipment and is not conducive to reducing production costs. Chinese patent CN111653765A discloses a method for preparing niobium-doped nickel cobalt aluminum oxide positive electrode materials by spray drying. This method uses a high-energy sand mill to grind and mix the raw materials and then spray granulate them. It is impossible to obtain spherical micron particles with uniform morphology, which is not conducive to further improving the material's tap density and processing performance. Summary of the invention
[0004] The purpose of the present disclosure is to provide a niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material, a preparation method thereof, and a lithium-ion battery containing the same. The niobium element in the quaternary material is uniformly doped, and the lithium-ion battery containing the quaternary material has good cycle performance and a high capacity retention rate after long-term cycling.
[0005] In order to achieve the above-mentioned object, the present disclosure provides a niobium-doped lithium nickel-cobalt-manganese-aluminum oxide quaternary material in the first aspect, wherein the niobium-doped lithium nickel-cobalt-manganese-aluminum oxide quaternary material comprises a chemical formula of LiNi 1-x-y-z-n Co x Mn y Al z Nb n O2 particles, 0<x≤0.2, 0<y≤0.1, 0<z≤0.05, 0.002<n≤0.02;
[0006] Among them, the ratio of A to D is 0.9-1.1;
[0007] Based on the total molar ratio of nickel, cobalt, manganese, aluminum and niobium on the surface of the particle, A represents the molar ratio of niobium on the surface of the particle;
[0008] Based on the total molar ratio of nickel, cobalt, manganese, aluminum and niobium in the particle phase, D represents the molar ratio of niobium in the particle phase.
[0009] Optionally, the median particle size D50 of the particles is 8-12 μm.
[0010] The second aspect of the present disclosure provides a method for preparing the niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material according to the first aspect of the present disclosure, the method comprising the following steps:
[0011] (1) subjecting aluminum-based hydrotalcite nanosheets, a nickel-cobalt-manganese ternary precursor, and a niobium-containing compound to a first ball milling to obtain a pre-product;
[0012] (2) subjecting the pre-product to a second ball milling with a lithium-containing compound, and then subjecting the pre-product to a heat treatment in an oxygen-containing atmosphere;
[0013] The aluminum-based hydrotalcite nanosheets contain a transition metal, the transition metal is a cobalt element or a nickel element, and the molar ratio of the transition metal element to the aluminum element is (2-5):1.
[0014] Optionally, in step (1), the molar ratio of the transition element in the aluminum-based hydrotalcite nanosheets to the niobium element in the niobium-containing compound is greater than 2:1.
[0015] Optionally, the niobium-containing compound includes one or more of niobium pentoxide, niobium oxalate and ammonium niobium oxalate;
[0016] The lithium-containing compound includes one or more of lithium hydroxide, lithium carbonate and lithium nitrate.
[0017] Optionally, the average particle size of the niobium-containing compound is 50-80 nm; the average particle size of the lithium-containing compound is 6-8 μm.
[0018] Optionally, the chemical formula of the nickel-cobalt-manganese ternary precursor is Ni 1-a-b Co a Mn b (OH)2 or Ni 1-a- b Co a Mn b CO3, where 0<a≤0.1, 0<b≤0.1;
[0019] Optionally, the median particle size D50 of the nickel-cobalt-manganese ternary precursor is 8-12 μm.
[0020] Optionally, in step (2), the molar ratio of the total molar sum of nickel, cobalt, manganese, aluminum and niobium in the pre-product to the lithium in the lithium-containing compound is 1:(1.0-1.1).
[0021] Optionally, in step (2), the heat treatment comprises the following steps:
[0022] a. Heating to 500-600°C at a first heating rate of 1-8°C / min for a first calcination for 1-3h;
[0023] b. Continue heating to 700-800°C at a second heating rate of 2-6°C / min and perform a second calcination for 10-15h.
[0024] Optionally, the first ball milling time is 1-4 hours; the second ball milling time is 1-4 hours.
[0025] A third aspect of the present disclosure provides a lithium-ion battery, comprising a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises the niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material as described in the first aspect of the present disclosure.
[0026] Through the above technical scheme, the present application first prepares aluminum-based hydrotalcite nanosheets containing cobalt or nickel elements, and then uses solid-phase ball milling to coat the aluminum-based hydrotalcite nanosheets and niobium sources on the surface of a spherical nickel-cobalt-manganese ternary precursor, and then mixes and roasts with a lithium source to obtain a niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material. The method of the present application can reduce the difficulty of material synthesis, improve the doping effect of niobium elements, and can flexibly control the ratio of the four elements in the material. The niobium element in the prepared quaternary material is evenly distributed among the particles, and the lithium-ion battery containing the quaternary material has good cycle performance and a high capacity retention rate after long-term cycling.
[0027] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0029] Figure 1 This is a scanning electron microscope image of the niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material A1 prepared in Example 1 of the present application.
[0030] Figure 2 This is a scanning electron microscope image of the undoped nickel-cobalt-manganese-aluminum-lithium quaternary material D2 prepared in Comparative Example 2 of the present application. DETAILED DESCRIPTION
[0031] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0032] The present disclosure provides a niobium-doped lithium nickel-cobalt-manganese-aluminum oxide quaternary material, wherein the niobium-doped lithium nickel-cobalt-manganese-aluminum oxide quaternary material comprises a chemical formula of LiNi 1-x-y-z-n Co x Mn y Al z Nb n O2 particles, 0<x≤0.2, 0<y≤0.1, 0<z≤0.05, 0.002<n≤0.02;
[0033] Among them, the ratio of A to D is 0.9-1.1;
[0034] Based on the total molar ratio of nickel, cobalt, manganese, aluminum and niobium on the surface of the particle, A represents the molar ratio of niobium on the surface of the particle;
[0035] Based on the total molar ratio of nickel, cobalt, manganese, aluminum and niobium in the particle phase, D represents the molar ratio of niobium in the particle phase.
[0036] In the present disclosure, "the molar proportion of niobium element on the surface of the particle" refers to the ratio of the molar number of niobium element on the surface of the particle to the total molar number of nickel element, cobalt element, manganese element, aluminum element and niobium element on the surface; "the molar proportion of niobium element in the bulk phase of the particle" refers to the ratio of the molar number of niobium element in the bulk phase of the particle to the total molar number of nickel element, cobalt element, manganese element, aluminum element and niobium element in the bulk phase.
[0037] In a preferred embodiment, the ratio of A to D is 0.95-1.05. The niobium element of the material within the above range is distributed in the bulk phase, which further optimizes the crystal structure of the material and can effectively remove residual alkali on the surface, thereby improving long-term cycle performance.
[0038] In one embodiment of the present disclosure, the median particle size D50 of the particles is 8-12 μm, preferably 9-11 μm.
[0039] In one embodiment of the present disclosure, the primary grain size of the particles is 500-1000 mm, and the testing method is scanning electron microscope ruler measurement.
[0040] The second aspect of the present disclosure provides a method for preparing the niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material according to the first aspect of the present disclosure, the method comprising the following steps:
[0041] (1) subjecting aluminum-based hydrotalcite nanosheets, a nickel-cobalt-manganese ternary precursor, and a niobium-containing compound to a first ball milling to obtain a pre-product;
[0042] (2) subjecting the pre-product to a second ball milling with a lithium-containing compound, and then subjecting the pre-product to a heat treatment in an oxygen-containing atmosphere;
[0043] The aluminum-based hydrotalcite nanosheets contain a transition metal, the transition metal is a cobalt element or a nickel element, and the molar ratio of the transition metal element to the aluminum element is (2-5):1, preferably (2-3):1.
[0044] During the heat treatment process, the cobalt or nickel elements in the aluminum-based hydrotalcite nanosheets can drive the niobium element into the interior of the material through the "synergistic diffusion effect", and can utilize the strong chemical bond of Nb-O to inhibit the structural distortion and collapse of the material during the charging and discharging process, thereby improving the cyclic stability of the material.
[0045] In the present disclosure, the oxygen-containing atmosphere is an oxygen atmosphere or an air atmosphere, preferably an oxygen atmosphere.
[0046] In one embodiment of the present disclosure, in step (1), the molar ratio of the transition metal element in the aluminum-based hydrotalcite nanosheets to the niobium element in the niobium-containing compound is greater than 2:1. Meeting the above ratio can reduce the content of niobium on the surface, so that the prepared material has better electrochemical properties.
[0047] In one embodiment of the present disclosure, the niobium-containing compound includes one or more of niobium pentoxide, niobium oxalate and ammonium niobium oxalate; the lithium-containing compound includes one or more of lithium hydroxide, lithium carbonate and lithium nitrate. Further, the average particle size of the niobium-containing compound is 50-80nm, preferably 50-60nm; the average particle size of the lithium-containing compound is 6-8μm, preferably 6-7μm.
[0048] In one embodiment of the present disclosure, the chemical formula of the nickel-cobalt-manganese ternary precursor is Ni 1-a-b Co a Mn b (OH)2 or Ni 1-a-b Co a Mn b CO3, wherein 0<a≤0.1, 0<b≤0.1.
[0049] In one embodiment of the present disclosure, the median particle size D50 of the nickel-cobalt-manganese ternary precursor is 8-12 μm, preferably 9-11 μm.
[0050] In one embodiment of the present disclosure, the molar ratio of the total molar sum of nickel, cobalt, manganese, aluminum and niobium in the pre-product to the lithium in the lithium-containing compound is (1.0-1.1):1, preferably 1:(1.02-1.08), and further preferably 1:(1.04-1.06).
[0051] In the present disclosure, in step (1), the feed amounts of aluminum-based hydrotalcite nanosheets, nickel-cobalt-manganese ternary precursor and niobium-containing compound are LiNi 1-x-y-z-a Co x Mn y Al z Nb n The molar ratio of Ni, Co, Mn, Al and Nb in the O2 material can be weighed to meet the molar content of Ni, Co, Mn, Al and Nb in the final product.
[0052] In one embodiment of the present disclosure, in step (2), the heat treatment comprises the following steps:
[0053] a. Heating to 500-600°C at a first heating rate of 1-8°C / min for a first calcination for 1-3h;
[0054] b. Continue heating to 700-800°C at a second heating rate of 2-6°C / min, and perform a second calcination for 10-15 hours. The above heat treatment method can fully decompose the nickel-cobalt-manganese ternary precursor, aluminum-based hydrotalcite nanosheets, and lithium-containing compounds into oxides in the first calcination stage, improve the solid phase reaction efficiency in the second calcination stage, and generate a quaternary material with a more complete crystal form.
[0055] In the present disclosure, both the first ball milling and the second ball milling are solid phase ball milling. Further, the first ball milling time is 1-4h, preferably 2-3h; the second ball milling time is 1-4h, preferably 2-3h. Meeting the above ball milling time can ensure sufficient coating of the nanomaterial and avoid the precursor particles from being broken due to excessive ball milling time.
[0056] In one embodiment of the present disclosure, the aluminum-based hydrotalcite nanosheets containing transition metal elements are prepared by:
[0057] S1 preparing a first solution comprising a transition metal source and an aluminum source;
[0058] S2: adding the first solution and the alkaline solution into a colloid mill at a speed of 1000-3000 r / min for 2-5 min to obtain a suspension;
[0059] S3 uses the suspension to prepare aluminum-based hydrotalcite nanosheets;
[0060] Furthermore, using the suspension to prepare aluminum-based hydrotalcite nanosheets includes: aging the suspension in a 95-98°C water bath for 2-4 hours, washing and filtering until the pH of the filtrate is lower than 7.5, and drying the filtered solid at 80-120°C for 8-12 hours to obtain aluminum-based hydrotalcite nanosheets containing transition metal elements.
[0061] In the present disclosure, the transition metal source is a soluble transition metal salt, which includes one or more of nickel sulfate, nickel chloride, nickel nitrate and nickel acetate; or, the soluble transition metal salt includes one or more of cobalt sulfate, cobalt chloride, cobalt nitrate and cobalt acetate.
[0062] In the present disclosure, the aluminum source includes one or more of aluminum sulfate, aluminum chloride, aluminum nitrate and aluminum acetate.
[0063] In the present disclosure, the alkaline solution comprises a soluble alkali and a soluble alkaline salt, wherein the soluble alkali comprises sodium hydroxide and / or potassium hydroxide; the soluble alkaline salt comprises sodium carbonate and / or potassium carbonate; specifically, the soluble alkali is sodium hydroxide, and the soluble alkaline salt is sodium carbonate. Further, the concentration of the soluble alkali is 1-2 mol / L, and the concentration of the soluble alkaline salt is 0.25-0.75 mol / L.
[0064] In the present disclosure, the volume ratio of the first solution to the alkaline solution is (0.8-1.5):1; for example, they can be mixed in equal volumes.
[0065] In the present disclosure, the molar ratio of the transition metal source calculated as transition metal element to the aluminum source calculated as aluminum element is (2-5):1; the total molar concentration of the transition metal source calculated as transition metal element and the aluminum source calculated as aluminum element is 0.5-1.25 mol / L.
[0066] A third aspect of the present disclosure is a lithium-ion battery, comprising a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises the niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material as described in the first aspect of the present disclosure.
[0067] Furthermore, the negative electrode material of the lithium ion battery may be, for example, a lithium sheet, and the electrolyte may be, for example, an alkyl carbonate solution of LiPF6. This is conventional in the art and no specific requirements are made here.
[0068] The reagents used in the examples and comparative examples of the present application are all commercially available.
[0069] The test instrument model of the scanning electron microscope is FEI Quanta 200FEG, the rated voltage of the equipment is 10kV, and the observation is performed at different magnifications;
[0070] The median particle size D50 was measured using a Mastersizer 2000 laser particle size analyzer from Malvern, UK, and the particle size of the nanomaterial was measured using SEM annotation.
[0071] Material metal element analysis: The particle surface element analysis was tested using VG Scientifc's ESCALab220i-XL X-ray photoelectron spectroscopy, and the particle bulk element analysis was tested using a Perkin-Elmer Optima 3300DV inductively coupled plasma (ICP) element analyzer.
[0072] The first discharge capacity and capacity retention rate were tested using Wuhan Blue Electric CT2001A battery tester, with a charge and discharge voltage range of 2.7-4.3V (vs.Li + / Li). After 5 cycles of charge and discharge at 0.1C, 3 cycles of charge and discharge at 0.2C were performed, and finally a long-term cycle was performed at 0.5C.
[0073] In the following examples and comparative examples, the first ball milling and the second ball milling are both solid phase ball milling.
[0074] Examples 1-6 are used to illustrate the niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material and the preparation method thereof of the present application.
[0075] Example 1
[0076] The niobium-doped lithium nickel-cobalt-manganese-aluminum oxide quaternary material A1 was prepared by the following steps.
[0077] (1) Preparation of Cobalt-Aluminum Hydrotalcite Nanosheets
[0078] Cobalt sulfate calculated as Co element and aluminum sulfate calculated as Al element were dissolved in deionized water at a molar ratio of 3:1 to prepare a first solution with a total metal ion concentration of 1.0 mol / L; an alkaline solution with a sodium hydroxide concentration of 1.6 mol / L and a sodium carbonate concentration of 0.25 mol / L was prepared. The first solution and the alkaline solution were added to a colloid mill with a rotation speed of 3000 r / min at a volume ratio of 1:1 for a mixed reaction for 3 minutes. The suspension after the mixed reaction was stirred and aged in a 98°C water bath for 3 hours, and then washed and filtered repeatedly until the pH of the filtrate was lower than 7.5. The washed filter cake was dried at 120°C for 10 hours to obtain hydrotalcite nanosheets with a molar ratio of cobalt and aluminum elements of 3:1, and the chemical formula was Co6Al2(OH) 16 CO3·6H2O.
[0079] (2) Preparation of Niobium-doped Lithium Nickel-Cobalt-Manganese-Aluminum Oxide Quaternary Materials
[0080] According to Ni 0.8 Co 0.1 Mn 0.1 The (OH)2 precursor (median particle size D50 is 9.5 μm), the cobalt aluminum hydrotalcite nanosheets prepared in step (1), and nano niobium pentoxide (average particle size is 50 nm) are weighed in a molar ratio of 100:1:0.5, and the first ball milling is performed for 2.5 hours to obtain a pre-product.
[0081] The above pre-product and lithium hydroxide (average particle size of 7 μm) were weighed according to the molar ratio of n(Ni+Co+Mn+Al+Nb):n(Li)=1:1.06, and the second ball milling was performed for 2.5 hours, and then the temperature was increased to 500°C at a first heating rate of 2°C / min in an oxygen atmosphere, and the first roasting was performed for 3 hours, and then the temperature was further increased to 750°C at a second heating rate of 2°C / min, and the second roasting was performed for 15 hours, and then cooled to room temperature to obtain niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material A1, the chemical formula of which is LiNi 0.734 Co 0.147 Mn 0.092 Al 0.018 Nb 0.009 O2. The proportion of Nb element on the particle surface and in the bulk phase in quaternary material A1 are listed in Table 1.
[0082] Scanning electron microscope test of niobium-doped nickel-cobalt-manganese-aluminum-lithium quaternary material A1. Figure 1 This is a scanning electron microscope image.
[0083] Example 2
[0084] The niobium-doped lithium nickel-cobalt-manganese-aluminum oxide quaternary material A2 was prepared by the method of Example 1, with the following differences:
[0085] (2) Preparation of Niobium-doped Lithium Nickel-Cobalt-Manganese-Aluminum Oxide Quaternary Materials
[0086] According to Ni 0.8 Co 0.1 Mn 0.1 The (OH)2 precursor (median particle size D50 is 9.5 μm), the cobalt aluminum hydrotalcite nanosheets prepared in step (1), and niobium oxalate (average particle size is 50 nm) are weighed in a molar ratio of 100:2:1, and the first ball milling is performed for 2.5 hours to obtain a pre-product.
[0087] The above pre-product and lithium carbonate (average particle size of 6 μm) were weighed according to the molar ratio of n(Ni+Co+Mn+Al+Nb):n(Li)=1:1.05, and then the temperature was raised to 500°C at a first heating rate of 4°C / min in an oxygen atmosphere, and the first calcination was performed for 3 hours. The temperature was further raised to 750°C at a second heating rate of 4°C / min, and the second calcination was performed for 15 hours. The niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material A2 was obtained, and the chemical formula was LiNi 0.678 Co 0.186 Mn 0.085 Al 0.034 Nb 0.017 O2. The proportion of Nb element on the particle surface and in the bulk phase in quaternary material A2 are listed in Table 1.
[0088] Example 3
[0089] The following steps are used to prepare niobium-doped lithium nickel-cobalt-manganese-aluminum oxide quaternary material A3.
[0090] (1) Dissolve cobalt chloride calculated as Co element and aluminum chloride calculated as Al element in a molar ratio of 2:1 in deionized water to prepare a first solution with a total metal ion concentration of 0.5 mol / L; prepare an alkaline solution with a sodium hydroxide concentration of 1.0 mol / L and a sodium carbonate concentration of 0.5 mol / L. Add the first solution and the alkaline solution at a volume ratio of 1:1 to a colloid mill at a speed of 3000 r / min for a mixed reaction for 3 minutes, stir and age the suspension after the mixed reaction in a 98°C water bath for 3 hours, then wash and filter repeatedly until the pH of the filtrate is lower than 7.5, and dry the washed filter cake at 120°C for 10 hours to obtain cobalt aluminum hydrotalcite nanosheets with a molar ratio of cobalt to aluminum elements of 2:1, with a chemical formula of Co4Al2(OH) 12 CO3·6H2O.
[0091] (2) Preparation of Niobium-doped Lithium Nickel-Cobalt-Manganese-Aluminum Oxide Quaternary Materials
[0092] According to Ni 0.8 Co 0.1 Mn 0.1The CO3 precursor (median particle size D50 is 10 μm), the cobalt aluminum hydrotalcite nanosheets prepared in step (1), and nano niobium pentoxide (average particle size is 50 nm) are weighed in a molar ratio of 100:3:1, and the first ball milling is performed for 2.5 hours to obtain a pre-product.
[0093] The above pre-product and lithium nitrate (average particle size of 6 μm) were weighed according to the molar ratio of n(Ni+Co+Mn+Al+Nb):n(Li)=1:1.04, and then the temperature was raised to 500°C at a first heating rate of 8°C / min in an oxygen atmosphere, and the first calcination was performed for 3 hours. The temperature was then further raised to 750°C at a second heating rate of 5°C / min, and the second calcination was performed for 15 hours. The niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material A3 was obtained, and the chemical formula was LiNi 0.667 Co 0.183 Mn 0.083 Al 0.050 Nb 0.017 O2. The proportion of Nb element on the particle surface and in the bulk phase in quaternary material A3 are listed in Table 1.
[0094] Example 4
[0095] (1) Preparation of NiAl-HDS nanosheets
[0096] Nickel sulfate calculated as Ni element and aluminum sulfate calculated as Al element were dissolved in deionized water at a molar ratio of 3:1 to prepare a first solution with a total metal ion concentration of 1.0 mol / L; an alkaline solution with a sodium hydroxide concentration of 1.6 mol / L and a sodium carbonate concentration of 0.25 mol / L was prepared. The first solution and the alkaline solution were added to a colloid mill with a rotation speed of 3000 r / min at a volume ratio of 1:1 for a mixed reaction for 3 minutes, and the suspension after the mixed reaction was stirred and aged in a 98°C water bath for 3 hours, and then washed and filtered repeatedly until the pH of the filtrate was less than 7.5, and the washed filter cake was dried at 120°C for 10 hours to obtain nickel-aluminum hydrotalcite nanosheets with a molar ratio of nickel and aluminum elements of 3:1, with a chemical formula of Ni6Al2(OH) 16 CO3·6H2O.
[0097] (2) Preparation of Niobium-doped Lithium Nickel-Cobalt-Manganese-Aluminum Oxide Quaternary Materials
[0098] According to Ni 0.8 Co 0.1 Mn 0.1 The (OH)2 precursor (median particle size D50 is 9.5 μm), the nickel aluminum hydrotalcite nanosheets prepared in step (1), and nano niobium pentoxide (average particle size is 50 nm) are weighed in a molar ratio of 100:1:0.5, and the first ball milling is performed for 2.5 hours to obtain a pre-product.
[0099] The above pre-product and lithium hydroxide (average particle size of 7 μm) were weighed according to the molar ratio of n(Ni+Co+Mn+Al+Nb):n(Li)=1:1.06, and the second ball milling was performed for 2.5 hours, and then the temperature was increased to 500°C at a first heating rate of 2°C / min in an oxygen atmosphere, and the first roasting was performed for 3 hours, and then the temperature was further increased to 750°C at a second heating rate of 2°C / min, and the second roasting was performed for 15 hours, and then cooled to room temperature to obtain niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material A4, the chemical formula of which is LiNi 0.789 Co 0.092 Mn 0.092 Al 0.018 Nb 0.009 O2. The proportion of Nb element on the particle surface and in the bulk phase in the quaternary material A4 are listed in Table 1.
[0100] Example 5
[0101] The niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material A5 was prepared by the method of Example 3, except that Ni 0.8 Co 0.1 Mn 0.1 The molar ratio of the CO3 precursor, the cobalt aluminum hydrotalcite nanosheets prepared in step (1), and nano niobium pentoxide is 100:0.5:1.
[0102] The chemical formula of quaternary material A5 is LiNi 0.762 Co 0.114 Mn 0.095 Al 0.010 Nb 0.019 O2. The proportion of Nb element on the particle surface and in the bulk phase in quaternary material A5 are listed in Table 1.
[0103] Comparative Example 1
[0104] In this comparative example, a conventional solid phase coating method was used to prepare niobium-doped lithium nickel cobalt manganese aluminum oxide positive electrode material D1.
[0105] (1) Preparation of Cobalt-Aluminum Hydrotalcite Nanosheets
[0106] Cobalt sulfate calculated as Co element and aluminum sulfate calculated as Al element were dissolved in deionized water at a molar ratio of 3:1 to prepare a first solution with a total metal ion concentration of 1.0 mol / L; an alkaline solution with a sodium hydroxide concentration of 1.6 mol / L and a sodium carbonate concentration of 0.25 mol / L was prepared. The first solution and the alkaline solution were added to a colloid mill with a rotation speed of 3000 r / min at a volume ratio of 1:1 for a mixed reaction for 3 minutes, and the suspension after the mixed reaction was stirred and aged in a 98°C water bath for 3 hours, and then washed and filtered repeatedly until the pH of the filtrate was less than 7.5, and the washed filter cake was dried at 120°C for 10 hours to obtain a cobalt aluminum hydrotalcite nanosheet with a molar ratio of cobalt and aluminum elements of 3:1, and the chemical formula was Co6Al2(OH) 16 CO3·6H2O.
[0107] (2) Preparation of nickel-cobalt-manganese-aluminum-lithium quaternary materials
[0108] According to Ni 0.8 Co 0.1 Mn 0.1 The (OH)2 precursor (median particle size D50 is 9.5 μm) and the cobalt aluminum hydrotalcite nanosheets prepared in step (1) are weighed in a molar ratio of 100:1, the two are mixed and solid-phase ball milled for 2.5 hours, and the first ball milling is performed for 2.5 hours to obtain a pre-product.
[0109] The above pre-product and lithium hydroxide (average particle size is 7 μm) are weighed according to the molar ratio of n(Ni+Co+Mn+Al+Nb):n(Li)=1:1.06, and the second ball milling is carried out for 2.5 hours. Then, the temperature is increased to 500°C in an oxygen atmosphere at a first heating rate of 2°C / min, and the first calcination is carried out for 3 hours. Then, the temperature is continued to be increased to 750°C at a second heating rate of 2°C / min, and the second calcination is carried out for 15 hours. After cooling to room temperature, a nickel-cobalt-manganese-aluminum lithium oxide quaternary material is obtained.
[0110] (3) Doping with niobium
[0111] The nickel-cobalt-manganese-aluminum lithium quaternary material and nano-niobium pentoxide in step (2) were weighed in a molar ratio of 100:0.5, solid-phase ball milled for 2.5 hours, and calcined at 750° C. for 5 hours in an oxygen atmosphere to obtain niobium-doped nickel-cobalt-manganese-aluminum lithium positive electrode material D1. The chemical formula of the quaternary material D1 is LiNi 0.734 Co 0.147 Mn 0.092 Al 0.018 Nb 0.009 O2, among which, the proportion of Nb element on the particle surface and in the bulk phase in the quaternary material D1 are listed in Table 1.
[0112] Comparative Example 2
[0113] In this comparative example, steps (1) and (2) of comparative example 1 are used to prepare niobium-free nickel-cobalt-manganese-aluminum-lithium quaternary material D2, without performing niobium doping in step (3).
[0114] The chemical formula of the quaternary material D2 is LiNi 0.741 Co 0.148 Mn 0.093 Al 0.018 O2, the proportion of Nb element on the particle surface and in the whole in the quaternary material D2 are listed in Table 1.
[0115] Scanning electron microscope test of the nickel-cobalt-manganese-aluminum-oxide positive electrode material D2 without niobium doping. Figure 2 This is a scanning electron microscope image.
[0116] Comparative Example 3
[0117] The niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material D3 was prepared by the method of Example 1, except that the aluminum-based hydrotalcite used was magnesium-aluminum hydrotalcite Mg4Al2(OH) 12 CO3·6H2O.
[0118] The chemical formula of the quaternary material D3 is LiNi 0.748 Co 0.093 Mn 0.093 Mg 0.037 Al 0.019 Nb 0.010 O2, among which, the proportion of Nb element on the particle surface and in the bulk phase in the quaternary material D3 are listed in Table 1.
[0119] Test Example 1-8
[0120] The quaternary materials of Examples 1-5 and Comparative Examples 1-3 were used as positive electrode materials, mixed with acetylene black conductive agent and polyvinylidene fluoride binder in a mass ratio of 94:3:3, coated on the surface of aluminum foil current collector, dried at 110°C and pressed into sheets, and electrode sheets with a diameter of 1 cm were obtained by a punching machine. The sheets were vacuum dried in a vacuum oven at 120°C for 24 hours as positive electrodes, metal lithium sheets were used as negative electrodes, polyethylene films were used as separators, 1 mol / L LiPF6 / (ethylene carbonate + dimethyl carbonate) was used as electrolyte, wherein the volume ratio of ethylene carbonate to dimethyl carbonate was 1:1, and button batteries were assembled in a glove box.
[0121] The Wuhan Blue Electric CT2001A battery tester was used to test the electrochemical performance, and the charge and discharge voltage range was 2.7-4.3V (vs.Li + / Li). After 5 cycles of charge and discharge at 0.1C, 3 cycles of charge and discharge at 0.2C, and finally long-term cycle at 0.5C. The results are listed in Table 1.
[0122] Table 1
[0123]
[0124] In Table 1, A represents the molar ratio of niobium on the surface of the particle, and D represents the molar ratio of niobium in the particle bulk phase. The molar ratio of niobium refers to the stoichiometric number of niobium after the normalized contents of the four elements Ni, Co, Mn, Al and Nb in the material are calculated.
[0125] According to the data in Table 1, the molar ratios of niobium elements on the surface and bulk phase of the nickel-cobalt-manganese-aluminum-lithium-aluminate quaternary materials A1-A4 prepared by the method disclosed in the present invention and D1 prepared by the traditional coating doping method are basically the same, indicating that the niobium element is evenly distributed in the material and the doping effect is good; while the niobium element in D1 is enriched on the surface of the material particles, indicating that it is difficult to achieve uniform doping of elements with large ion diameters after the quaternary material structure is formed. Although its first discharge capacity does not change significantly, its capacity retention rate after 200 cycles is significantly lower than that of the uniformly doped embodiment. In embodiment A5, the ratio of cobalt element in cobalt-aluminum hydrotalcite to niobium element in niobium pentoxide is 1:1, and the cobalt element is not enough to drive the niobium element of equal moles to diffuse in coordination during the solid phase reaction. Therefore, part of niobium is still enriched on the surface of the material in A5, and effective uniform doping is not achieved, and its capacity retention rate is significantly lower than that of A1-A4. Compared with the quaternary material D1 prepared by the conventional solid phase method, the ratio of A to D is significantly larger than that of A1-A5, indicating that the conventional solid phase method cannot achieve effective and uniform doping of Ni elements, and the capacity retention rate is low. Compared with the undoped quaternary material D2, although the first discharge capacity of the material A1 doped with niobium element has a small decrease, after 200 cycles, a higher capacity retention rate can be obtained, indicating that its long-term cycle performance is good. Relative to the quaternary material D3, the quaternary material is prepared using aluminum-based hydrotalcite nanosheets that do not contain transition metals, and the niobium element is enriched on the surface of the material particles, which shows that the transition metal in the aluminum-based hydrotalcite nanosheets can drive the niobium element into the interior of the material, so that the niobium element in the prepared material is evenly distributed, thereby obtaining a higher first discharge capacity and good long-term cycle performance. At the same time, the method disclosed in the present invention can flexibly control the ratio of the four elements in the material by changing the type of aluminum-based hydrotalcite nanosheets and the ratio of metal elements to meet the needs of improving the electrical properties of the material.
[0126] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0127] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0128] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A method for preparing niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material, It is characterized in that The method comprises the following steps: (1) performing a first ball milling on aluminum-based hydrotalcite nanosheets, a nickel-cobalt-manganese ternary precursor, and a niobium-containing compound to obtain a pre-product; (2) subjecting the pre-product to a second ball milling with a lithium-containing compound, and then subjecting the pre-product to a heat treatment in an oxygen-containing atmosphere; Wherein, the aluminum-based hydrotalcite nanosheets contain a transition metal, the transition metal is a cobalt element or a nickel element, and the molar ratio of the transition metal element to the aluminum element is (2-5):1; In step (1), the molar ratio of the transition element in the aluminum-based hydrotalcite nanosheets to the niobium element in the niobium-containing compound is 2:1 or more; The niobium-containing compound includes one or more of niobium pentoxide, niobium oxalate and ammonium niobium oxalate; In step (2), the heat treatment comprises the following steps: a. Heating to 500-600°C at a first heating rate of 1-8°C / min for a first calcination for 1-3h; b. Continue heating to 700-800°C at a second heating rate of 2-6°C / min for a second calcination for 10-15h; The niobium-doped lithium nickel-cobalt-manganese-aluminum oxide quaternary material comprises a chemical formula of LiNi 1-x-y-z-n Co x Mn y Al z Nb n O 2 Particles, 0<x≤0.2, 0<y≤0.1, 0<z≤0.05, 0.002<n≤0.02; Among them, the ratio of A to D is 0.9-1.1; Based on the total molar ratio of nickel, cobalt, manganese, aluminum and niobium on the surface of the particle, A represents the molar ratio of niobium on the surface of the particle; Based on the total molar ratio of nickel, cobalt, manganese, aluminum and niobium in the particle phase, D represents the molar ratio of niobium in the particle phase.
2. The method according to claim 1, in, The lithium-containing compound includes one or more of lithium hydroxide, lithium carbonate and lithium nitrate.
3. The method according to claim 1, in, The average particle size of the niobium-containing compound is 50-80 nm; the average particle size of the lithium-containing compound is 6-8 μm.
4. The method according to claim 1, in, The chemical formula of the nickel-cobalt-manganese ternary precursor is Ni 1-a-b Co a Mn b (OH) 2 Or Ni 1-a-b Co a Mn b CO 3 , where 0<a≤0.1, 0<b≤0.
1.
5. The method according to claim 4, in, The median particle size D50 of the nickel-cobalt-manganese ternary precursor is 8-12 μm.
6. The method according to claim 1, in, The molar ratio of the total mole of nickel element, cobalt element, manganese element, aluminum element and niobium element in the pre-product to the mole of lithium element in the lithium-containing compound is 1:(1.0-1.1).
7. The method according to claim 1, in, The first ball milling time is 1-4 hours; the second ball milling time is 1-4 hours.
8. The method according to claim 1, in, The median particle size D50 of the particles is 8-12 μm.
9. A lithium ion battery, It is characterized in that The lithium-ion battery comprises a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises a niobium-doped nickel-cobalt-manganese-aluminum lithium quaternary material prepared by the method described in any one of claims 1 to 8.