High-boron-content polymer as well as preparation method and application thereof
By conducting liquid-assisted reaction between polysilazane and ammonia borane under low temperature conditions, high boron content polymer is prepared, which solves the problems of boron source toxicity and low boron content, improves synthesis efficiency and purity, and is suitable for high-temperature ceramics Preparation of materials.
Patent Information
- Application Number
- CN202411125574.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-16
AI Technical Summary
In the prior art, the boron source reactants are toxic, have low boron content and difficult synthesis, resulting in low synthesis efficiency and reduced purity.
Under the protection of nitrogen or argon, polysilazane is dissolved in an organic solvent, and ammonia borane is added at a temperature of -10°C to 0°C. The polymer with high boron content is prepared by low-temperature liquid phase assisted reaction, which avoids the The influence of chlorine and sulfur in traditional boron sources improves synthesis efficiency and safety.
It realizes efficient preparation of high boron content polymers, improves synthesis efficiency and purity, reduces synthesis difficulty, and ammonia borane is non-toxic and safe, suitable for large-scale generation.
Smart Images

Figure CN118994595A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer materials, and in particular to a high-boron content polymer and a preparation method and application thereof. Background Art
[0002] At present, the preparation of boron-containing polymers mainly uses borane chlorosilane, borane dimethyl sulfide and boron trichloride as boron sources, and prepares boron-containing polymers through multiple high-temperature and long-term reactions. The disadvantage is that the boron content in this type of boron source reactant is too low, and excessive boron source reactants need to be added to increase the boron content in the polymer. At the same time, inorganic elements such as chlorine and sulfur are increased in the reactants, thereby reducing the purity of the polymer and making it difficult to mass produce; on the other hand, this type of boron source reactant containing inorganic elements has certain toxicity; on the other hand, multiple steps of high-temperature and long-term reactions are required to synthesize the polymer, which increases the difficulty of synthesizing the boron-containing polymer and reduces the synthesis efficiency. Summary of the invention
[0003] The problem solved by the invention is how to solve the problems of toxicity of boron source reactants, low boron content of boron source reactants and great synthesis difficulty in the process of preparing boron-containing polymers.
[0004] In order to solve the above problems, the present invention provides a high-boron content polymer and a preparation method and application thereof.
[0005] In a first aspect, the present invention provides a method for preparing a high boron content polymer, comprising the following steps:
[0006] S1: Under the protection of nitrogen or argon, dissolving polysilazane in an organic solvent to obtain a polysilazane mixed solution;
[0007] S2: adding ammonia borane to the polysilazane mixed solution at a temperature of -10°C to 0°C, stirring and reacting to obtain a high boron content polymer.
[0008] Optionally, step S2 specifically includes: adding ammonia borane to the polysilazane mixed solution, stirring the mixture at a temperature of -10°C to 0°C, and performing reduced pressure distillation on the solution after the reaction to remove organic solvents and impurities to obtain a high boron content polymer.
[0009] Optionally, the solution after the reaction is distilled under reduced pressure in a rotating state.
[0010] Optionally, the organic solvent comprises toluene and / or acetone.
[0011] Optionally, the concentration of polysilazane in the polysilazane mixed solution is 10-30 wt %.
[0012] Optionally, the mass ratio of the added polysilazane to ammonia borane is (5-1):1.
[0013] Optionally, in step S2, the reaction is stirred at a temperature of -10°C to 0°C for 1-3h.
[0014] In a second aspect, the present invention provides a high-boron content polymer, which is prepared by the preparation method of the high-boron content polymer as described in any one of the above items.
[0015] Optionally, the boron content in the high-boron-content polymer is higher than 20 wt %.
[0016] In a third aspect, the present invention provides an application of the high-boron content polymer as described above in the field of preparing organic precursor polymer-derived ceramics.
[0017] The high-boron-content polymer and the preparation method and application thereof of the present invention have the following beneficial effects: polysilazane is dissolved in an organic solvent, and ammonia borane and polysilazane react with boron hydrogen at a temperature of -10°C to 0°C with the assistance of a low-temperature liquid phase to prepare a high-boron-content polymer; using ammonia borane as a boron source avoids the influence of inorganic elements such as chlorine and sulfur in traditional boron sources (such as boryl chlorosilane, borane dimethyl sulfide and boron trichloride), reduces the difficulty of synthesis and increases the synthesis efficiency; and compared with the boron source of traditional synthetic polymers, ammonia borane has a higher boron content and is non-toxic and safe; at the same time, its synthesis can be completed under low temperature conditions, avoiding the high-temperature, long-time and complex synthesis process of traditional polymer preparation, making the reaction easier and safer, improving the synthesis efficiency of synthetic polymers, and facilitating the mass production of high-boron-content polymers. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a flow chart of a method for preparing a high-boron content polymer according to an embodiment of the present invention;
[0019] Figure 2 The X-ray photoelectron spectrum of the high boron content polymer of Example 1 of the present invention;
[0020] Figure 3 This is an infrared spectrum of the high boron content polymer of Example 1 of the present invention;
[0021] Figure 4 This is a thermogravimetric curve of the high boron content polymer of Example 1 of the present invention. DETAILED DESCRIPTION
[0022] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.
[0023] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;
[0024] The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.
[0025] In the related art, a very effective way to produce high-performance ceramics (SiC / Si3N4 / SiBCN) is to prepare them through the organic precursor polymer-derived ceramic (PDC) method, which can provide a uniform and controllable chemical composition for high-purity ceramic materials at the molecular scale. Therefore, the regulation of the structure and function of PDC ceramics can be achieved based on the design of the element types and contents in the polymer. Among them, the molecular structure with a high boron content helps to improve the high-temperature thermal stability and high-temperature oxidation resistance of PDC ceramics, enabling further application and expansion in high-temperature ablation-resistant fields such as aerospace, and high boron content can increase the high-temperature residual carbon rate and ceramic yield of the polymer. Therefore, high-boron content polymers have received widespread attention from the scientific research community and the industrial community.
[0026] In the prior art, a boron source is provided by boryl chlorosilane, borane dimethyl sulfide and boron trichloride, and a boron-containing polymer is finally prepared by multi-step reaction with other silicon-containing elements, carbon elements and nitrogen-containing small molecules. However, the boron content in the traditional boron source (boryl chlorosilane, borane dimethyl sulfide and boron trichloride) is relatively low, resulting in a relatively low boron content in the final synthetic polymer, generally less than 10wt%. In addition, a large amount of inorganic elements such as chlorine and sulfur are contained in the side chain in the traditional boron source, which not only reduces its reactivity, but also requires the reaction temperature to be increased to ensure the synthesis of the polymer; and it is necessary to carry out multiple different temperature reaction synthesis and multiple purification to avoid introducing inorganic elements into the final synthetic polymer.
[0027] In view of the problems existing in the above-mentioned related technologies, this embodiment provides a high-boron content polymer and a preparation method and application thereof.
[0028] like Figure 1 As shown, a method for preparing a high-boron content polymer provided by an embodiment of the present invention comprises the following steps:
[0029] S1: Under the protection of nitrogen or argon, dissolving polysilazane in an organic solvent to obtain a polysilazane mixed solution;
[0030] S2: adding ammonia borane to the polysilazane mixed solution at a temperature of -10°C to 0°C, stirring and reacting to obtain a high boron content polymer.
[0031] In this embodiment, polysilazane is dissolved in an organic solvent, and ammonia borane with a high boron content is used as a boron source. At a temperature of -10°C to 0°C, a borohydride reaction occurs between ammonia borane and polysilazane with the assistance of a low-temperature liquid phase to prepare a polymer with a high boron content. Using ammonia borane as a boron source avoids the influence of inorganic elements such as chlorine and sulfur in traditional boron sources (such as boryl chlorosilane, borane dimethyl sulfide and boron trichloride), reduces the difficulty of synthesis and increases the synthesis efficiency; and compared with the boron source of traditional synthetic polymers, ammonia borane has a higher boron content and is non-toxic and safe; at the same time, its synthesis can be completed under low temperature conditions, avoiding the high-temperature, long-term and complex synthesis process of traditional polymer preparation, making the reaction easier and safer, and improving the synthesis efficiency of synthetic polymers.
[0032] Specifically, ammonia borane is added dropwise to the polysilazane mixed solution to uniformly disperse the ammonia borane in the mixed solution, thereby improving the reaction efficiency.
[0033] In this embodiment, polysilazane and ammonia borane react at low temperature at a temperature of -10°C to 0°C. Ammonia borane undergoes a polymerization reaction when heated. After heating, the molecular structure of ammonia borane changes and reorganizes, and the molecules interact with each other, and first polymerize into (NH2BH2)n. If heating is continued, it will continue to polymerize into (NHBH)n, which will lead to waste of ammonia borane, and heating will also lead to waste of energy. If the reaction temperature is too low, below -10°C, it is easy to make the reaction difficult and slow.
[0034] Optionally, step S2 specifically includes: adding ammonia borane to the polysilazane mixed solution, stirring the mixture at a temperature of -10°C to 0°C, and performing reduced pressure distillation on the solution after the reaction to remove organic solvents and impurities to obtain a high boron content polymer.
[0035] In this optional embodiment, impurities, organic solvents, by-products, etc. in the high-boron content polymer can be removed.
[0036] Optionally, the solution after the reaction is distilled under reduced pressure in a rotating state.
[0037] In this optional embodiment, the reduced pressure distillation is performed using a rotary method, which is easy to operate.
[0038] Optionally, the organic solvent comprises toluene and / or acetone.
[0039] Specifically, in the process of adding polysilazane to the organic solvent, it is necessary to slowly add polysilazane to the organic solvent and perform ultrasonic dispersion to prepare a mixed solution in which polysilazane is uniformly dissolved in the organic solvent.
[0040] Optionally, the concentration of polysilazane in the polysilazane mixed solution is 10-30 wt %.
[0041] In this optional embodiment, when the concentration of polysilazane is low, for example, less than 10wt%, the synthesis efficiency and synthesis amount of the boron-containing polymer are easily reduced due to the low concentration of the reactants. When the concentration of polysilazane is high, for example, higher than 30wt%, it is easy to cause a higher viscosity in the solution, making it difficult for the polysilazane to be completely dissolved in the organic solvent and causing agglomeration.
[0042] Optionally, the mass ratio of the added polysilazane to ammonia borane is (5-1):1.
[0043] In this optional embodiment, by changing the ratio of polysilazane to ammonia borane, the type and content of the boron-containing polymer can be controlled. When the mass ratio of polysilazane to ammonia borane is selected to be (5-1):1, the ratio is appropriate, which can improve the synthesis efficiency of the high-boron-content polymer and can increase the boron content of the high-boron-content polymer.
[0044] Optionally, in step S2, the reaction is stirred at a temperature of -10°C to 0°C for 1-3h.
[0045] In this optional embodiment, the synthesis reaction can be completed in a relatively short time, thus avoiding the long and complicated synthesis process of the traditional preparation of polymers and improving the synthesis efficiency of the synthetic polymers.
[0046] A high-boron content polymer provided in an embodiment of the present invention is prepared by the preparation method of a high-boron content polymer as described in any one of the above items.
[0047] In this embodiment, the high-boron content polymer has a high boron content and good stability.
[0048] Optionally, the boron content in the high-boron-content polymer is higher than 20 wt %.
[0049] In this optional embodiment, the high-boron content polymer has a high boron content and good stability.
[0050] An embodiment of the present invention provides an application of the high-boron content polymer as described above in the field of preparing organic precursor polymer-derived ceramics.
[0051] In this embodiment, the high-boron content polymer has a high boron content. The molecular structure of the high boron content helps to improve the high-temperature thermal stability and high-temperature oxidation resistance of the organic precursor polymer-derived ceramics, and can increase the high-temperature residual carbon rate and ceramic yield of the polymer, thereby being able to prepare organic precursor polymer-derived ceramics (PCD ceramics) with excellent high-temperature performance.
[0052] The present invention is further described below in conjunction with specific embodiments.
[0053] Example 1, Preparation of high boron content polymer
[0054] In the first step, 20 g of polysilazane was allowed to stand in a glove box filled with nitrogen for 1 hour, and then slowly added into 80 g of toluene organic solvent, and the polysilazane was completely dissolved in the toluene organic solvent by ultrasonic vibration to prepare a mixed solution with a polysilazane concentration of 20 wt%.
[0055] In the second step, ammonia borane is slowly added to the mixed solution prepared in the first step, the mass ratio of polysilazane to ammonia borane is 2:1, and the mixture is stirred evenly in a stirrer to obtain a mixed reaction solution with a suitable viscosity.
[0056] In the third step, the mixed reaction solution in the second step is subjected to a low-temperature reaction: the reaction time is 1 h and the reaction temperature is 0°C.
[0057] The fourth step, subjecting the mixed solution after the reaction in the third step to reduced pressure distillation, comprises: subjecting the mixed solution to reduced pressure distillation in a rotating state to obtain a polymer with a high boron content.
[0058] like Figure 2 As shown, the composition of the obtained high boron content polymer was analyzed by X-ray, as shown in FIG. Figure 3 As shown, infrared spectroscopy is used to analyze and identify the material molecules of the obtained high boron content polymer, such as Figure 2 and Figure 3 As shown, the high-boron content polymer prepared in this embodiment contains five elements: silicon, boron, carbon, nitrogen and hydrogen, and is an organic polymer with BN-Si-C as the main chain and -CH3 as the side chain.
[0059] like Figure 4 As shown, the thermal gravimetric analysis of the obtained high boron content polymer was performed using the DSC thermal analysis method (Differential Scanning Calorimeter) to obtain a thermal gravimetric curve of the high boron content polymer of Example 1. Figure 4 It can be seen that high-boron content polymers have higher stability and yield, which is conducive to the preparation of PCD ceramics with excellent high-temperature performance.
[0060] Example 2, Preparation of high boron content polymer
[0061] In the first step, 20 g of polysilazane was allowed to stand in a glove box filled with argon for 1 hour, and then slowly added into 80 g of acetone organic solvent, and the polysilazane was completely dissolved in the toluene organic solvent by ultrasonic vibration to prepare a mixed solution with a polysilazane concentration of 20 wt%.
[0062] In the second step, ammonia borane is slowly added to the mixed solution prepared in the first step, the mass ratio of polysilazane to ammonia borane is 2:1, and the mixture is stirred evenly in a stirrer to obtain a mixed reaction solution with a suitable viscosity.
[0063] In the third step, the mixed reaction solution in the second step is subjected to a low-temperature reaction: the reaction time is 2 h and the reaction temperature is 0°C.
[0064] The fourth step, subjecting the mixed solution after the reaction in the third step to reduced pressure distillation, comprises: subjecting the mixed solution to reduced pressure distillation in a rotating state to obtain a polymer with a high boron content.
[0065] Example 3, Preparation of high boron content polymer
[0066] In the first step, 10 g of polysilazane was allowed to stand in a glove box filled with argon for 1 hour, and then slowly added into 90 g of toluene organic solvent, and the polysilazane was completely dissolved in the toluene organic solvent by ultrasonic vibration to prepare a mixed solution with a polysilazane concentration of 10 wt%.
[0067] In the second step, ammonia borane is slowly added to the mixed solution prepared in the first step, the mass ratio of polysilazane to ammonia borane is 2:1, and the mixture is stirred evenly in a stirrer to obtain a mixed reaction solution with a suitable viscosity.
[0068] In the third step, the mixed reaction solution in the second step is subjected to a low-temperature reaction: the reaction time is 3 h and the reaction temperature is 0°C.
[0069] The fourth step, subjecting the mixed solution after the reaction in the third step to reduced pressure distillation, comprises: subjecting the mixed solution to reduced pressure distillation in a rotating state to obtain a polymer with a high boron content.
[0070] Example 4, Preparation of high boron content polymer
[0071] In the first step, 30 g of polysilazane was allowed to stand in a glove box filled with argon for 1 hour, and then slowly added into 70 g of toluene organic solvent, and the polysilazane was completely dissolved in the toluene organic solvent by ultrasonic vibration to prepare a mixed solution with a polysilazane concentration of 30 wt%.
[0072] In the second step, ammonia borane is slowly added to the mixed solution prepared in the first step, the mass ratio of polysilazane to ammonia borane is 5:1, and the mixture is stirred evenly in a stirrer to obtain a mixed reaction solution with a suitable viscosity.
[0073] In the third step, the mixed reaction solution in the second step is subjected to a low-temperature reaction: the reaction time is 1 h and the reaction temperature is -5°C.
[0074] The fourth step, subjecting the mixed solution after the reaction in the third step to reduced pressure distillation, comprises: subjecting the mixed solution to reduced pressure distillation in a rotating state to obtain a polymer with a high boron content.
[0075] Example 5, Preparation of high boron content polymer
[0076] In the first step, 20 g of polysilazane was allowed to stand in a glove box filled with argon for 1 hour, and then slowly added into 80 g of toluene organic solvent, and the polysilazane was completely dissolved in the toluene organic solvent by ultrasonic vibration to prepare a mixed solution with a polysilazane concentration of 20 wt%.
[0077] In the second step, ammonia borane is slowly added to the mixed solution prepared in the first step, with the mass ratio of polysilazane to ammonia borane being 1:1, and the mixture is stirred evenly in a stirrer to obtain a mixed reaction solution with a suitable viscosity.
[0078] In the third step, the mixed reaction solution in the second step is subjected to a low-temperature reaction: the reaction time is 1 h and the reaction temperature is -10°C.
[0079] The fourth step, subjecting the mixed solution after the reaction in the third step to reduced pressure distillation, comprises: subjecting the mixed solution to reduced pressure distillation in a rotating state to obtain a polymer with a high boron content.
[0080] The results of Examples 2-5 are the same as those of Example 1. The elements in the prepared high-boron content polymers are silicon, boron, carbon, nitrogen and hydrogen, and the polymers are organic polymers with BN-Si-C as the main chain and -CH3 as the side chain. The high-boron content polymers obtained in Examples 2-5 also have high stability and yield, which is conducive to the preparation of PCD ceramics with excellent high-temperature performance.
[0081] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A method for preparing a high-boron content polymer, characterized in that: The following steps are involved: S1: Under the protection of nitrogen or argon, dissolving polysilazane in an organic solvent to obtain a polysilazane mixed solution; S2: adding ammonia borane to the polysilazane mixed solution at a temperature of -10°C to 0°C, stirring and reacting to obtain a high boron content polymer.
2. The method for preparing a high boron content polymer according to claim 1, characterized in that: The step S2 specifically includes: adding ammonia borane to the polysilazane mixed solution, stirring and reacting at a temperature of -10°C to 0°C, and performing reduced pressure distillation on the solution after the reaction to remove the organic solvent and impurities to obtain the high boron content polymer.
3. The method for preparing a high boron content polymer according to claim 2, characterized in that: The solution after the reaction is subjected to reduced pressure distillation under a rotating state.
4. The method for preparing a high boron content polymer according to claim 1, characterized in that: The organic solvent includes toluene and / or acetone.
5. The method for preparing a high boron content polymer according to claim 1, characterized in that: The concentration of the polysilazane in the polysilazane mixed solution is 10-30 wt %.
6. The method for preparing a high boron content polymer according to claim 1, characterized in that: The mass ratio of the added polysilazane to the added ammonia borane is (5-1):
1.
7. The method for preparing a high boron content polymer according to claim 1, characterized in that: In the step S2, the reaction is stirred at a temperature of -10°C to 0°C for 1-3 hours.
8. A high boron content polymer, characterized in that The polymer is prepared by the method for preparing a high-boron content polymer as described in any one of claims 1 to 7.
9. The high boron content polymer according to claim 8, characterized in that The boron content in the high-boron-content polymer is higher than 20 wt %.
10. Use of the high boron content polymer according to claim 8 or 9 in the field of preparing organic precursor polymer-derived ceramics.
Citation Information
Patent Citations
Preparation method for liquid polyborosilazane
CN102115539A
Carborane polymer with high boron content and synthesis method thereof
CN114015059A
Polyborosilazane and process for producing same
US5030744A