Pseudoplastic fluid polishing liquid and polishing method
By using pseudoplastic fluid polishing fluid and specific polishing methods, and utilizing shear thinning characteristics and rotation speed adjustment, the problem of polishing complex curved surfaces is solved, and high-efficiency, low-cost precision polishing effects are achieved.
Patent Information
- Application Number
- CN202310012240.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-05
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-01-05
AI Technical Summary
Existing polishing technologies are difficult to achieve efficient, low-cost precision polishing when processing complex curved surfaces, and most rely on manual operations with poor stability and repeatability, and some methods have environmental pollution or high costs.
A polishing fluid containing 75%-97% pseudoplastic fluid and 3%-25% abrasive is used, and the shear thinning characteristics of the pseudoplastic fluid are used to adjust the viscosity at different rotational speeds, combined with a stirring blade and a rotating mechanism for vertical and horizontal movements for polishing.
Ultra-high precision polishing with simple operation and low cost is achieved, the surface roughness of the workpiece is significantly reduced, and the method is highly stable and efficient.
Smart Images

Figure CN116082962B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of precision polishing, and in particular to a pseudoplastic fluid polishing liquid and a polishing method. Background Art
[0002] With the increasing requirements of precision instruments and high-precision parts for the smoothness of the workpiece surface, how to achieve simple, efficient and low-cost workpiece surface polishing is an urgent problem to be solved. Usually, surface polishing is the process of contacting the polishing tool with the workpiece surface and grinding and removing the protrusions on the workpiece surface under certain relative pressure and movement. The more precise the polishing, the better the contact and fit between the curved surface of the polishing tool and the curved surface of the workpiece. However, as the designed curved surface becomes more and more complex, it is difficult for the polishing tool to adapt to the requirements of the workpiece surface curvature.
[0003] In my country, a large number of manual operations are still used in actual polishing production. Not only is the processing process long, but the stability and repeatability are poor, and the processing cost is high. Therefore, it is very necessary to research and develop a polishing method that is simple to operate, low-cost, and suitable for complex surfaces. The existing new polishing technologies mainly include abrasive fluid polishing, electrochemical polishing, plasma polishing, electrorheological polishing, magnetorheological polishing, etc. Abrasive fluid polishing is to treat the surface of the workpiece by a fluid containing abrasives under the action of impact pressure. This method requires the use of an abrasive fluid transport device, which has a complex structure and is difficult to maintain; electrochemical polishing has good surface quality and high processing efficiency, but the electrolyte is easy to pollute the environment and is greatly restricted by environmental protection policies. Plasma polishing is to polish the surface of the workpiece using the plasma formed by the high-voltage electric field at the interface between the workpiece and the working medium. The surface quality is good, but the size is large and the processing efficiency is low. Electrorheological polishing and magnetorheological polishing mainly use electric fields or magnetic fields to control the rheological polishing fluid of conductive abrasives or magnetic abrasives to polish the workpiece surface. It is a kind of efficient and flexible polishing method that can achieve good processing effects. However, the relatively complex electric field and magnetic field auxiliary equipment and the high cost of using processing media restrict the application of this type of polishing method. Summary of the invention
[0004] The purpose of the present invention is to provide a pseudoplastic fluid polishing liquid and a polishing method, which can overcome the shortcomings and defects of existing contact polishing and other polishing technologies, and utilize the unique shear thinning characteristics of pseudoplastic fluid to give full play to its advantages in ultra-high precision polishing.
[0005] The present invention achieves the above-mentioned purpose through the following technical solutions:
[0006] A pseudoplastic fluid polishing liquid comprises 75%-97% pseudoplastic fluid and 3%-25% abrasive particles by volume.
[0007] A further improvement is that at 20° C., the viscosity of the pseudoplastic fluid at a rotation speed of 1 rpm is 8000-80000 mcP, and the viscosity at a rotation speed of 100 rpm is 200-8000 mcP.
[0008] A further improvement is that the pseudoplastic fluid comprises silicone oil, water, an active agent and a thickener.
[0009] A further improvement is that the weight ratio of the components in the pseudoplastic fluid is silicone oil: water: active agent: thickener = 15-25%: 50-70%: 5-15%: 10-20%.
[0010] A further improvement is that the abrasive has a regular or irregular appearance shape and a particle size range of 0.02-100 μm.
[0011] A further improvement is that the abrasive is selected from one or a mixture of silicon dioxide, silicon carbide, aluminum oxide, zirconium oxide, diamond, carbon nitride, boron nitride, and boron carbide.
[0012] A further improvement is that the working temperature range of the polishing liquid is 0-40°C and the polishing rotation speed is 0-300rpm.
[0013] The present invention also provides a pseudoplastic fluid polishing method, the steps comprising:
[0014] Prepare a polishing working chamber, set a stirring plate with a rotating mechanism at the bottom of the chamber, fill the chamber with the above-mentioned pseudoplastic fluid polishing liquid, and then hang the workpiece to be polished in the chamber through a fixed frame;
[0015] The rotating mechanism is started to drive the pseudoplastic fluid polishing liquid to rotate at high speed through the stirring blade, and the workpiece to be polished is completely immersed in the pseudoplastic fluid polishing liquid through the fixed frame, and the workpiece to be polished is moved in the vertical and horizontal directions to perform polishing in different states.
[0016] The beneficial effect of the present invention is that: the present invention proposes a pseudoplastic fluid polishing liquid and polishing method with simple principle and low cost, that is, during the polishing process, when the workpiece and the polishing liquid perform relative shear motion, the shear thinning characteristics unique to the pseudoplastic fluid are utilized, and as the motion rate increases, the viscosity of the polishing liquid decreases and the resistance decreases, thereby weakening the grinding effect of the abrasive on the workpiece, thereby facilitating ultra-high precision polishing. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a schematic diagram of the implementation structure of the pseudoplastic fluid polishing method;
[0018] In the figure: 1. fixed frame; 2. workpiece to be polished; 3. pseudoplastic fluid polishing liquid; 4. cavity; 5. stirring blade; 6. rotating mechanism. DETAILED DESCRIPTION
[0019] The present application is further described in detail below in conjunction with the accompanying drawings. It is necessary to point out here that the following specific implementation methods are only used to further illustrate the present application and cannot be understood as limiting the scope of protection of the present application. Technical personnel in this field can make some non-essential improvements and adjustments to the present application based on the above application content.
[0020] A pseudoplastic fluid polishing liquid comprises 75%-97% pseudoplastic fluid and 3%-25% abrasive particles by volume.
[0021] The pseudoplastic fluid comprises silicone oil, water, an active agent and a thickener, and the weight ratio is silicone oil: water: active agent: thickener = 15-25%: 50-70%: 5-15%: 10-20%. At 20°C, the viscosity of the pseudoplastic fluid is 8000-80000 mcP at a rotation speed of 1 rpm, and the viscosity is 200-8000 mcP at a rotation speed of 100 rpm.
[0022] The abrasive has a regular or irregular appearance and a particle size range of 0.02-100 μm. The abrasive is selected from one or more mixtures of silicon dioxide, silicon carbide, aluminum oxide, zirconium oxide, diamond, carbon nitride, boron nitride, and boron carbide.
[0023] The optimal working temperature range of the polishing liquid is 0-40°C, and the polishing speed is 0-300rpm.
[0024] Combine the following Figure 1 As shown, two polishing method embodiments using the above-mentioned pseudoplastic fluid polishing liquid are introduced:
[0025] Embodiment 1:
[0026] In this embodiment, the polishing liquid preparation and the abrasive are configured according to the proportions shown in Table 1.
[0027] Table 1: Polishing liquid ratio table
[0028] Polishing liquid pseudoplastic fluid ratio Silicone oil: water: surfactant: thickener = 15%: 70%: 5%: 20% Polishing fluid abrasive 2000 mesh silicon carbide and aluminum oxide abrasive, 1:1 volume ratio Pseudoplastic fluid volume ratio 85% Viscosity at room temperature (20°C) 20000mcP
[0029] Fix the workpiece 2 to be polished (stainless steel pipe, diameter Φ150mm, height 100mm, thickness 2mm, with three groups of round holes on it) on the workpiece fixing frame 1, pour 200L of polishing liquid according to the proportion in Table 1 into the polishing working chamber 4, start the rotating mechanism 6, and the stirring blade 5 drives the pseudoplastic fluid polishing liquid 3 to rotate at high speed. The workpiece fixing frame 1 immerses the workpiece 2 to be polished in the polishing liquid, and moves in the vertical and horizontal directions to adjust the polishing working state. The specific polishing sequence is shown in Table 2:
[0030] Table 2: Polishing schedule
[0031] Speed time 50rpm 6 minutes 80rpm 2 minutes 150rpm 8 minutes
[0032] After polishing, the surface roughness of the workpiece dropped from 50.4nm to 14nm, and the polishing effect was good.
[0033] Embodiment 2:
[0034] In this embodiment, the polishing liquid preparation and the abrasive are configured according to the proportions shown in Table 3.
[0035] Table 3: Polishing liquid ratio table
[0036] Polishing liquid pseudoplastic fluid ratio Silicone oil: water: surfactant: thickener = 25%: 50%: 15%: 10% Polishing fluid abrasive 2500 mesh zirconia abrasive Pseudoplastic fluid volume ratio 80% Viscosity at room temperature (20°C) 42000mcP
[0037] Fix the workpiece 2 to be polished (stainless steel pipe, 550mm long, 400mm high, 50mm thick, with multiple flow channels on it) on the workpiece fixing frame 1, pour 400L of polishing liquid according to the proportion in Table 3 into the polishing working chamber 4, start the rotating mechanism 6, and the stirring blade 5 drives the pseudoplastic fluid polishing liquid 3 to rotate at high speed. The workpiece fixing frame 1 immerses the workpiece 2 to be polished in the polishing liquid, and moves in the vertical and horizontal directions to adjust the polishing working state. The specific polishing sequence is shown in Table 4:
[0038] Table 4: Polishing schedule
[0039]
[0040]
[0041] After polishing, the surface roughness of the workpiece dropped from 18.4nm to 2.5nm, and the polishing effect was good.
[0042] It can be seen that the present invention utilizes the physical properties of the polishing liquid fluid and uses the differences in viscosity, resistance, and force of the fluid at different flow rates to refine the polishing effect of the polishing liquid. It not only has a simple structure and low cost, but also is easy to operate and has good stability. It is an efficient and flexible polishing method.
[0043] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A pseudoplastic fluid polishing method, characterized in that the steps include: Prepare a polishing working chamber, set a stirring piece with a rotating mechanism at the bottom of the chamber, fill the chamber with pseudoplastic fluid polishing liquid, and then suspend the workpiece to be polished in the chamber through a fixed frame; start the rotating mechanism, drive the pseudoplastic fluid polishing liquid to rotate at high speed through the stirring piece, immerse the workpiece to be polished in the pseudoplastic fluid polishing liquid through the fixed frame, and move the workpiece to be polished in the vertical and horizontal directions to perform polishing in different states; The polishing liquid includes 75%-97% pseudoplastic fluid and 3%-25% abrasive particles by volume; At 20° C., the viscosity of the pseudoplastic fluid at a rotation speed of 1 rpm is 8000-80000 mcP, and the viscosity at a rotation speed of 100 rpm is 200-8000 mcP; The components of the pseudoplastic fluid include silicone oil, water, an active agent and a thickener; The weight ratio of each component in the pseudoplastic fluid is silicone oil: water: active agent: thickener = 15-25%: 50-70%: 5-15%: 10-20%; The working temperature range of the polishing liquid is 0-40° C., and the polishing rotation speed is 0-300 rpm.
2. A pseudoplastic fluid polishing method according to claim 1, characterized in that: The abrasive particles have a regular or irregular appearance shape, and a particle size range of 0.02-100 μm.
3. A pseudoplastic fluid polishing method according to claim 1, characterized in that: The abrasive particles are selected from one or more mixtures of silicon dioxide, silicon carbide, aluminum oxide, zirconium oxide, diamond, carbon nitride, boron nitride and boron carbide.