A polyurethane-cement composite grouting material for water and mud bursting in a karst tunnel with a cavity rich in loess and a water blocking and consolidation construction method thereof

By using polyurethane-cement composite grouting materials and water-blocking and consolidation construction methods in karst tunnels, the problem of water and mud bursting in the loess area is solved, rapid repair and long-term stable operation of karst tunnels are achieved, and the service life of the tunnel is extended. High durability, lightweight, waterproof and other characteristics.

CN116102302BActive Publication Date: 2024-12-06山西省交通科技研发有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211271332.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-17
Publication Date
2024-12-06
Estimated Expiration
2042-10-17

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively solve the water and mud in the karst tunnel with loess-rich dissolution cavity, resulting in serious problems of water and water inrush, affecting the safety and service life of the tunnel.

Method used

Polyurethane-cement composite grouting materials and their water-blocking consolidation construction methods are adopted to quickly consolidate loess to prevent water and mud bursts and form stable Tunnel curtains to ensure the safety of the tunnel.

Benefits of technology

It realizes rapid repair and long-term stable operation of karst tunnels with loess-rich dissolving cavity, extends the service life of the tunnel, prevents water and mud bursts during the summer rainy period, and has high durability, light weight, waterproof, early strength, etc. characteristic.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116102302B_ABST
    Figure CN116102302B_ABST
Patent Text Reader

Abstract

The present invention discloses a polyurethane-cement composite grouting material for water and mud bursts in a karst tunnel with a cavity rich in loess and a water blocking and consolidation construction method thereof. The raw material composition of the polyurethane-cement composite grouting material includes oily polyurethane, cement, sodium silicate, bauxite, and metakaolin, and each raw material is used after being mixed with water. The material has the advantages of low permeability, high durability, excellent aging resistance and mechanical properties, and green environmental protection. The water blocking and consolidation construction method adopted by the present invention can quickly repair water and mud bursts in a karst tunnel with a cavity rich in loess, prevent water and mud bursts caused by loess in a karst tunnel with a cavity rich in loess during the abundant rainy period in summer, consolidate loess, fill the cavities, and enable the karst tunnel with a cavity rich in loess to operate safely and stably for a long time, thereby extending the service life of the tunnel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of grouting materials for water and mud bursting in karst tunnels with rich loess in the dissolution cavity, and specifically relates to a polyurethane-cement composite grouting material for water and mud bursting in karst tunnels with rich loess in the dissolution cavity and a water blocking and consolidation construction method thereof. Background Art

[0002] With the continuous development of social economy, the level of infrastructure construction in my country has been continuously improved, and tunnel construction has gradually moved towards the characteristics of deep burial, high water pressure, long distance, and large diameter. Problems such as water gushing, water and mud gushing caused by loess collapsibility and unknown water bodies in tunnels are becoming more and more serious. How to effectively avoid and treat water and mud gushing disasters in karst tunnels with rich loess in the cavity is an important scientific issue facing tunnel construction in Shanxi Province.

[0003] Combined with the hydrogeology of the karst geology in the loess region, a detailed analysis of water inrush is conducted, and with the help of engineering practice cases, a grouting design method for preventing and controlling water inrush in deep buried high-pressure water-rich tunnels is proposed, which provides a reference and reference for the implementation of similar projects in the future and is of great significance to the improvement of tunnel water inrush control technology. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the present invention provides a polyurethane-cement composite grouting material for karst tunnels with loess-rich cavities that has the advantages of low permeability, high durability, excellent aging resistance and mechanical properties, and green environmental protection, and a water blocking and consolidation construction method thereof.

[0005] The raw material composition of the polyurethane-cement composite grouting material for water and mud bursts in karst tunnels with loess-rich cavities includes 5 parts by mass of oily polyurethane, 30-40 parts by mass of cement, 10-15 parts by mass of sodium silicate, 15-25 parts by mass of bauxite, and 15-25 parts by mass of kaolin. The raw materials are mixed with water and used, and the amount of water added is 0.8-1.2 times the sum of the mass of cement and sodium silicate.

[0006] The oily polyurethane is composed, by mass, of 20 parts of castor oil-based polyoxyethylene ether, 10 parts of polyether 204, 10 parts of polyether 303, 40 parts of toluene diisocyanate (TDI), 0.1 parts of dibutyltin dilaurate (catalyst), 0.3 parts of stannous octoate (catalyst), 2 parts of 1,6-hexanediol (chain extender), 1 part of glycerol (chain extender), 2 parts of xylene (diluent), 0.3 parts of benzoyl chloride (retarder), 0.3 parts of benzenesulfonyl chloride (retarder), 2 parts of n-heptane (foaming agent), and 2 parts of dibutyl phthalate (plasticizer).

[0007] The preparation method of the polyurethane-cement composite grouting material for karst tunnels with loess-rich cavities is as follows: first, cement, sodium silicate, bauxite, kaolin and water are mixed in proportion and stirred for 30 minutes to 60 minutes to make them evenly mixed, then oily polyurethane is added and stirred for 15 seconds, and grouting is started when the viscosity is between 10Pa.s and 100Pa.s, and the prepared slurry is required to be filled within 60 minutes.

[0008] The water blocking and consolidation construction method is:

[0009] (1) The thickness of the grouting wall is determined according to the amount of water and mud inrush, and it is laid out within 100m-150m in front of the tunnel breach where water and mud inrush occur. Solid sodium hydroxide is added to promote the consolidation of the water-containing loess.

[0010] (2) The water and mud inrush levels are classified according to the amount of water and mud inrush in the tunnel. The geological survey method, geological radar method, transient electromagnetic method, and elastic wave emission method are used to comprehensively conduct advanced geological prediction, detect the water content and geological conditions in front of the tunnel face, and use advanced large-pipe shed grouting combined with radial grouting, adding polyurethane-cement composite grouting materials to consolidate the loess and broken surrounding rock in the karst in front of the tunnel face or lining;

[0011] (3) Add a 40cm-50cm drainage ditch or temporarily use a welded pipe to divert water to the cross tunnel through a multi-stage water pump and then discharge it out of the tunnel to form a drainage channel for sudden water and mud.

[0012] (4) Use large pipe shed or radial grouting method to arrange holes with plum blossom piles, with a hole diameter of 89mm-108mm. After grouting, a water and mud inrush curtain is formed in the grouting area. The depth of each grouting is not less than 20m, and no less than 5m is reserved as a grouting rock plate to prevent secondary water and mud inrush disasters;

[0013] (5) The core sampling method and water pressure test are used to evaluate the grouting effect, and the ground penetrating radar and transient electromagnetic are used to detect the grouting effect.

[0014] The specific operations of step (5) are as follows: on-site determination of the permeability coefficient and the actual number of hammer blows to test the grouting effects of the single-hole grouting test and the multi-hole grouting test; after grouting the tunnel working face, 3-5 inspection holes are drilled in the excavation face, and cores are taken to measure the water leakage and test the grouting water blocking effect; the grouting quality is comprehensively determined by the inspection hole water pressure test combined with the analysis method, the inspection hole method and the geophysical method; the core water leakage in the hard rock formation borehole should be less than 0.4L / min / m, and the core water leakage in the broken zone rock formation should be less than 0.2L / min / m.

[0015] The polyurethane-cement composite grouting material for water and mud bursts in karst tunnels with loess-rich cavities prepared by the present invention has the characteristics of light weight, high expansion, early strength, waterproofness, and rapidity. The water blocking and consolidation construction method for water and mud bursts in karst tunnels proposed by the present invention includes the steps of laying out grouting walls, determining the amount of water and mud bursts in tunnels and advanced geological prediction, preventing rapid grouting of water and mud burst consolidation bodies, building drainage channels, designing and treating curtain grouting for water and mud bursts in tunnels, and evaluating and testing grouting effects. The water blocking and consolidation construction method for water and mud bursts in karst tunnels with loess-rich cavities can quickly repair water and mud bursts in karst tunnels with loess-rich cavities, prevent water and mud bursts caused by loess in karst tunnels with loess-rich cavities during the abundant rainy season in summer, consolidate loess, fill the cavities, and enable long-term safe and stable operation of karst tunnels with loess-rich cavities, thereby extending the service life of the tunnels. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 Photo of water and mud bursting in a karst tunnel with loess-rich cavity.

[0017] Figure 2 Photo of the drainage channel used to prevent water and mud bursts in a karst tunnel with a cavity rich in loess.

[0018] Figure 3 Process roadmap for the water blocking and consolidation construction method of polyurethane-cement composite grouting materials for water and mud inrush in karst tunnels with loess-rich cavities.

[0019] Figure 4 Photo of the layout of grouting holes on the tunnel face. DETAILED DESCRIPTION

[0020] Embodiment 1:

[0021] (1) Preparation of oily polyurethane: weigh 20 parts by mass of castor oil-based polyoxyethylene ether, 10 parts of polyether 204, 10 parts of polyether 303, 40 parts of toluene diisocyanate, 0.1 parts of dibutyltin dilaurate, 0.3 parts of stannous octoate, 2 parts of 1,6-hexanediol, 1 part of glycerol, 2 parts of xylene, 0.3 parts of benzoyl chloride, 0.3 parts of benzenesulfonyl chloride, 2 parts of n-heptane, and 2 parts of dibutyl phthalate and mix them.

[0022] (2) Prepare polyurethane-cement composite grouting materials for sudden water and mud in karst tunnels with loess-rich cavities: the composition by mass percentage is 5% oily polyurethane, 40% cement, 10% sodium silicate, 25% bauxite, and 20% kaolin. First, mix cement, sodium silicate, bauxite, and kaolin with water and stir for 30 minutes to make them evenly mixed. The amount of water added is 100% of the sum of the mass of cement and sodium silicate. Then add oily polyurethane and stir for 15 seconds. When the viscosity is 10Pa.s, start grouting. The prepared slurry is required to be filled within 60 minutes. The compressive strength of the core sample of the grouting material is 45MPa, and the permeability coefficient is 10-8 cm / s, the core sample is intact without obvious damage.

[0023] (3) Construction method for water blocking and consolidation of karst tunnel water and mud inrush: The thickness of the grouting wall is determined to be 5m according to the amount of water and mud inrush, and it is laid 100m in front of the tunnel water and mud inrush breach to consolidate the water-containing loess. Sodium hydroxide solid is appropriately added to promote the consolidation of the water-containing loess. The water and mud inrush levels are divided according to the amount of water and mud inrush in the tunnel. The geological survey method, geological radar method, transient electromagnetic method, and elastic wave emission method are used to comprehensively conduct advanced geological prediction, detect the water content and geological conditions in front of the tunnel face, and use ultraviolet radiation to detect the water content and geological conditions in front of the tunnel face. The front large pipe shed grouting is combined with radial grouting to prevent sudden water and mud, and to consolidate the loess in the karst in front of the tunnel face or lining as soon as possible to avoid sudden water and mud disasters. Polyurethane-cement composite grouting materials are added to quickly consolidate the loess and broken surrounding rock in the karst; a 40cm drainage ditch is added or welded pipes are temporarily used to lead water to the cross tunnel position through multi-stage water pumps and then discharge it out of the tunnel to form a drainage channel for sudden water and mud; a large pipe shed or radial grouting method is used to arrange holes with plum blossom piles with a hole diameter of 89mm, such as Figure 4 As shown, after grouting, a water and mud curtain is formed in the grouting area. The depth of each grouting is 30m, and 5m is reserved as a grouting rock plate to prevent secondary water and mud disasters. Inspection and evaluation of grouting effect: The permeability coefficient and the measured hammer blow number measured on site are used to test the grouting effect of single-hole grouting test and multi-hole grouting test. After grouting of the tunnel working face, 5 inspection holes should be drilled in the excavation face, and the core should be taken to measure the leakage and test the grouting water blocking effect. The grouting quality inspection should be based on the inspection hole water pressure test, combined with comprehensive judgment such as analysis method, inspection hole method and geophysical prospecting method. The core water leakage in the hard rock formation borehole is 0.1L / min / m, and the core water leakage in the broken zone rock formation is 0L / min / m.

[0024] Embodiment 2:

[0025] (1) Preparation of oily polyurethane: weigh 20 parts by mass of castor oil-based polyoxyethylene ether, 10 parts of polyether 204, 10 parts of polyether 303, 40 parts of toluene diisocyanate, 0.1 parts of dibutyltin dilaurate, 0.3 parts of stannous octoate, 2 parts of 1,6-hexanediol, 1 part of glycerol, 2 parts of xylene, 0.3 parts of benzoyl chloride, 0.3 parts of benzenesulfonyl chloride, 2 parts of n-heptane, and 2 parts of dibutyl phthalate and mix them.

[0026] (2) Prepare polyurethane-cement composite grouting materials for sudden water and mud in karst tunnels with loess-rich cavities: the composition by mass percentage is 5% oily polyurethane, 30% cement, 15% sodium silicate, 25% bauxite, and 25% kaolin. First, mix cement, sodium silicate, bauxite, and kaolin with water and stir for 50 minutes to make them evenly mixed. The amount of water added is 100% of the sum of the mass of cement and sodium silicate. Then add oily polyurethane and stir for 15 seconds. When the viscosity is 35 Pa.s, start grouting. The prepared slurry is required to be filled within 60 minutes. The compressive strength of the core sample of the grouting material is 49MPa, and the permeability coefficient is 1.2*10 -8 cm / s, the core sample is intact without obvious damage.

[0027] (3) Construction method for blocking and consolidating water and mud in karst tunnels: The thickness of the grouting wall is determined to be 8m according to the amount of water and mud inrush, and it is laid 120m in front of the tunnel breach to consolidate the water-containing loess. Sodium hydroxide solid is appropriately added to promote the consolidation of the water-containing loess. The water and mud inrush levels are divided according to the amount of water and mud inrush in the tunnel. The geological survey method, geological radar method, transient electromagnetic method, and elastic wave emission method are used to comprehensively conduct advanced geological prediction, detect the water content and geological conditions in front of the tunnel face, and use advanced large-pipe grouting combined with radial grouting to prevent water and mud inrush, and consolidate the loess in the karst in front of the tunnel face or lining as soon as possible to avoid water and mud inrush. Mud disasters, polyurethane-cement composite grouting materials are added to quickly consolidate the loess and broken surrounding rocks in the karst, thus forming a rapid grouting method; add a 50cm drainage ditch or temporarily use a welded pipe, and use a multi-stage water pump to lead water to the cross tunnel position and then discharge it outside the tunnel to form a drainage channel for sudden water and mud; use a large pipe shed or radial grouting method to use plum blossom piles to arrange holes with a hole diameter of 89mm. After grouting, the grouting area forms a tunnel sudden water and mud curtain. The grouting depth is 30m each time, and 8m is retained as a grouting rock plate to prevent secondary sudden water and mud disasters; the grouting effect is evaluated by core sampling method and water pressure test, and the grouting effect is detected by ground penetrating radar and transient electromagnetic. Inspection and evaluation of grouting effect: The permeability coefficient and the measured hammer number measured on site should be used to inspect the grouting effect of single-hole grouting test and multi-hole grouting test. After grouting the tunnel working face, it is advisable to drill 5 inspection holes in the excavation face, take cores to measure the leakage, and inspect the grouting water blocking effect. The grouting quality inspection should be mainly based on the inspection hole water pressure test, combined with the analysis method, inspection hole method and geophysical method. The core water leakage in the hard rock formation is 0.0L / min / m, and the core water leakage in the broken zone rock formation is 0.1L / min / m.

[0028] Embodiment 3:

[0029] (1) Preparation of oily polyurethane: weigh 20 parts by mass of castor oil-based polyoxyethylene ether, 10 parts of polyether 204, 10 parts of polyether 303, 40 parts of toluene diisocyanate, 0.1 parts of dibutyltin dilaurate, 0.3 parts of stannous octoate, 2 parts of 1,6-hexanediol, 1 part of glycerol, 2 parts of xylene, 0.3 parts of benzoyl chloride, 0.3 parts of benzenesulfonyl chloride, 2 parts of n-heptane, and 2 parts of dibutyl phthalate and mix them.

[0030] (2) Prepare polyurethane-cement composite grouting materials for karst tunnels with loess-rich cavities to treat water and mud inrush: the composition by mass percentage is 5% oily polyurethane, 40% cement, 15% sodium silicate, 15% bauxite, and 25% kaolin. First, mix cement, sodium silicate, bauxite, and kaolin with water and stir for 40 minutes to make them evenly mixed. The amount of water added is 100% of the sum of the mass of cement and sodium silicate. Then add oily polyurethane and stir for 15 seconds. When the viscosity is 100 Pa.s, start grouting. The prepared slurry is required to be filled within 60 minutes. The compressive strength of the core sample of the grouting material is 56MPa, and the permeability coefficient is 2.6*10 -8 cm / s, the core sample is intact without obvious damage.

[0031] (3) Construction method for blocking and consolidating water and mud in karst tunnels: The thickness of the grouting wall is determined to be 5 m according to the amount of water and mud inrush, and it is laid 150 m in front of the tunnel breach to consolidate the water-containing loess. Sodium hydroxide solid is appropriately added to promote the consolidation of the water-containing loess. The water and mud inrush levels are classified according to the amount of water and mud inrush in the tunnel. The geological survey method, geological radar method, transient electromagnetic method, and elastic wave emission method are used to comprehensively conduct advanced geological prediction, detect the water content and geological conditions in front of the tunnel face, and use advanced large-pipe grouting combined with radial grouting to prevent water and mud inrush, and consolidate the loess in the karst in front of the tunnel face or lining as soon as possible to avoid water and mud inrush. Disasters, polyurethane-cement composite grouting materials are added to quickly consolidate the loess and broken surrounding rocks in the karst, thus forming a rapid grouting method; add a 50cm drainage ditch or temporarily use a welded pipe, and use a multi-stage water pump to lead water to the cross tunnel position and then discharge it outside the tunnel to form a drainage channel for sudden water and mud; use a large pipe shed or radial grouting method to use plum blossom piles to arrange holes with a hole diameter of 108mm. After grouting, the grouting area forms a tunnel sudden water and mud curtain. The grouting depth is 25m each time, and 5m is retained as a grouting rock plate to prevent secondary sudden water and mud disasters; the core sampling method and water pressure test are used to evaluate the grouting effect, and the ground penetrating radar and transient electromagnetic are used to detect the grouting effect. Inspection and evaluation of grouting effect: The permeability coefficient and the measured hammer number measured on site should be used to inspect the grouting effect of the single-hole grouting test and the multi-hole grouting test. After grouting the tunnel working face, it is advisable to drill 3 inspection holes on the excavation face, take cores to measure the leakage, and inspect the grouting water blocking effect. The grouting quality inspection should be mainly based on the inspection hole water pressure test, combined with the analysis method, inspection hole method and geophysical prospecting method. The core water leakage in the hard rock formation borehole is 0.0L / min / m, and the core water leakage in the broken zone rock formation is 0.0L / min / m.

Claims

1. A water plugging and consolidation construction method, characterized in that: The specific steps of the construction method are: (1) The thickness of the grouting wall is determined according to the amount of water and mud inrush, and it is laid out within 100m-150m in front of the breach of the tunnel where water and mud inrush occur. Solid sodium hydroxide is added to promote the consolidation of the water-containing loess. (2) The water and mud inrush levels are classified according to the amount of water and mud inrush in the tunnel. The geological survey method, geological radar method, transient electromagnetic method, and elastic wave emission method are used to comprehensively conduct advanced geological prediction, detect the water content and geological conditions in front of the tunnel face, and use advanced large-pipe shed grouting combined with radial grouting, adding polyurethane-cement composite grouting materials to consolidate the loess and broken surrounding rock in the karst in front of the tunnel face or lining; (3) Add a 40cm-50cm drainage ditch or temporarily use a welded pipe to divert water to the cross tunnel through a multi-stage water pump and then discharge it out of the tunnel to form a drainage channel for sudden water and mud. (4) Use plum blossom piles to arrange holes with a diameter of 89 mm to 108 mm using a large pipe shed or radial grouting method. After grouting, a water and mud inrush curtain is formed in the grouting area. The depth of each grouting is not less than 20 m, and no less than 5 m is retained as a grouting rock plate to prevent secondary water and mud inrush disasters; (5) Use core sampling method and water pressure test to evaluate the grouting effect, and use ground penetrating radar and transient electromagnetic to detect the grouting effect; The raw material composition of the polyurethane-cement composite grouting material includes 5 parts by mass of oily polyurethane, 30-40 parts by mass of cement, 10-15 parts by mass of sodium silicate, 15-25 parts by mass of bauxite, and 15-25 parts by mass of metakaolin, and each raw material is mixed with water before use; The oily polyurethane is composed, by mass, of 20 parts of castor oil-based polyoxyethylene ether, 10 parts of polyether 204, 10 parts of polyether 303, 40 parts of toluene diisocyanate, 0.1 parts of dibutyltin dilaurate, 0.3 parts of stannous octoate, 2 parts of 1,6-hexanediol, 1 part of glycerol, 2 parts of xylene, 0.3 parts of benzoyl chloride, 0.3 parts of benzenesulfonyl chloride, 2 parts of n-heptane, and 2 parts of dibutyl phthalate; The specific operations of step (5) are as follows: on-site determination of the permeability coefficient and the actual number of hammer blows to test the grouting effects of the single-hole grouting test and the multi-hole grouting test; after grouting the tunnel working face, 3-5 inspection holes are drilled in the excavation face to take cores to measure the water leakage and test the grouting water blocking effect; the grouting quality is comprehensively determined by the inspection hole water pressure test combined with the analysis method, the inspection hole method and the geophysical method; the core water leakage in the hard rock formation should be less than 0.4 L / min / m, and the core water leakage in the broken zone rock formation should be less than 0.2 L / min / m.

2. The water blocking and consolidation construction method according to claim 1, characterized in that: The amount of water added is 0.8-1.2 times the sum of the mass of cement and sodium silicate.

3. The water blocking and consolidation construction method according to claim 1, characterized in that: The specific operation of the preparation method of the polyurethane-cement composite grouting material is: first, cement, sodium silicate, bauxite, kaolin and water are mixed in proportion and stirred for 30 minutes to 60 minutes to make them evenly mixed, then oily polyurethane is added and stirred for 15 seconds, and grouting is started when the viscosity is between 10Pa.s and 100Pa.s, and the prepared slurry is required to be filled within 60 minutes.