Preparation method of hyperbranched flame-retardant waterborne polyurethane emulsion

By introducing silicone-hydroxyl-terminated modified melamine compounds into water-based polyurethane, the flame retardant properties and water resistance of hyperbranched water-based polyurethane are improved, solving the problems of insufficient fire resistance and thermal stability of traditional water-based polyurethane, and achieving high-performance Hyperbranched waterborne polyurethane products.

CN116102705BActive Publication Date: 2024-10-01JIANGSU HUAYUAN HI-TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111324628.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-10
Publication Date
2024-10-01
Estimated Expiration
2041-11-10

AI Technical Summary

Technical Problem

Due to its molecular chain structure, traditional water-based polyurethane has poor water resistance, insufficient thermal stability, and low fire resistance, which limits its application fields. In particular, the fire resistance of hyperbranched water-based polyurethane during combustion is still low, making it difficult to be widely used.

Method used

A new type of silicone-terminated modified melamine compound was prepared through organic synthesis and introduced into the water-based polyurethane molecular chain. A silicone-modified hyperbranched flame-retardant water-based polyurethane was designed and synthesized. The silicone-hydroxyl functionality was used to functionalize the functional groups and the melamine. Flame retardant properties, improve its flame retardant properties and water resistance.

Benefits of technology

A hyperbranched water-based polyurethane product with excellent flame retardant effect and good water resistance has been realized, which significantly improves its fire resistance and thermal stability. It is suitable for a wider range of application fields, while avoiding solvent residues. The product has high tensile strength and market prospects. broad.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of waterborne polyurethane, and discloses a method for preparing a hyperbranched flame-retardant waterborne polyurethane emulsion. Hydrogen-containing silane and olefinic acid resin are uniformly mixed and added with platinum dioxide, melamine and methanol are added after reflux filtration and distillation, methanol is removed after reaction, and acetic acid aqueous solution is added to obtain a silanol-terminated modified melamine compound; diisocyanate and oligomeric diol are reacted and then melamine compound is added, and then hydrophilic chain extender, organic bismuth, acetone, and water are added in sequence for self-emulsification and dispersion by high-speed stirring, and after the system becomes a uniform emulsion, acetone is removed to obtain a melamine-modified hyperbranched flame-retardant waterborne polyurethane emulsion. By synthesizing melamine compounds, crosslinking points are introduced into the molecular weight of polyurethane to form a body-shaped structure, which can not only improve the water resistance, heat resistance and wear resistance of the obtained waterborne polyurethane leather product, but also introduce melamine functional groups with excellent flame retardancy, and the obtained waterborne polyurethane product has good flame retardancy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterborne polyurethane synthesis, and in particular to a method for preparing a hyperbranched flame-retardant waterborne polyurethane emulsion. Background Art

[0002] Waterborne polyurethane (WPU) is a binary colloid system with water as a dispersant. It is non-toxic, pollution-free, safe and reliable, and fully complies with the concept of green environmental protection. It has developed rapidly and is widely used in synthetic leather, coatings, adhesives and other fields. However, the traditional WPU molecular chain is a linear structure with serious chain entanglement, resulting in high system viscosity and low solid content. Moreover, for the self-emulsifying WPU system, hydrophilic groups are introduced into its molecular chain, which makes the water resistance of the WPU film worse, making it difficult to compare with solvent-based PU.

[0003] Hyperbranched polymers have excellent performance, with advantages such as low viscosity, high rheology, and three-dimensional network structure. Introducing hyperbranched polymers into waterborne polyurethane molecular chains can give hyperbranched WPU good water resistance and strong thermal stability, significantly improving its performance. However, due to the high C and H values ​​in the molecular chain of hyperbranched waterborne polyurethane and the presence of O elements, its fire resistance is still very low, thus limiting its application field. In order to overcome this shortcoming and make hyperbranched WPU more widely used, it is necessary to perform flame retardant modification on it.

[0004] Among many flame retardants, the new silicone flame retardant produces silica particles that can migrate to the surface of the substrate when the material burns. It can not only play a flame retardant role, but also is environmentally friendly, and has received widespread attention from the industry. Unlike traditional flame retardants, the silicon-containing groups are introduced into the main chain or side chain of WPU through chemical methods such as polymerization and grafting. The resulting silicone-modified WPU has certain flame retardant and heat-resistant properties, as well as good water resistance. However, the flame retardant properties of the silicone flame retardant products currently developed are still insufficient, and other flame retardants still need to be added for use. Moreover, there are few reports on hyperbranched silicone flame retardants in the literature. Summary of the invention

[0005] Purpose of the invention: In view of the problems existing in the prior art, the present invention provides a method for preparing a hyperbranched flame-retardant waterborne polyurethane emulsion, preparing a new type of melamine compound modified by silicone hydroxyl end-capping by organic synthesis, and then introducing the compound into the molecular chain of waterborne polyurethane to obtain a silicone-modified hyperbranched flame-retardant waterborne polyurethane molecular chain, thereby obtaining a hyperbranched waterborne polyurethane product with excellent flame retardant effect and good water resistance.

[0006] Technical solution: The present invention provides a method for preparing a flame-retardant water-based polyurethane emulsion modified by organic silicon, comprising the following steps: S1: after uniformly mixing hydrogen-containing silane and olefinic acid resin, adding platinum dioxide as a catalyst, stirring evenly, refluxing at 80-90°C for 20-30h, filtering and distilling, adding melamine and methanol, reacting for 4-8h, distilling to remove methanol, adding a measured acetic acid aqueous solution to react for 6-24h, and obtaining a silanol-terminated modified melamine compound; S2: mixing diisocyanate and oligomer; The diol is stirred and reacted at 75-85°C for 0.5-2 hours, a certain amount of silanol-terminated modified melamine compound is added, and the reaction is stirred for 0.5-1.5 hours. A hydrophilic chain extender is added, and the reaction is stirred for 20-40 minutes. An organic bismuth catalyst is added, and the reaction is continued with stirring for 1-2 hours. A certain amount of acetone is added, and the reaction is continued with stirring for 0.5-1.5 hours. Water is added and stirred at a high speed for self-emulsification and dispersion. After the system becomes a uniform emulsion, acetone is removed to obtain a melamine-modified hyperbranched flame-retardant waterborne polyurethane emulsion.

[0007] Preferably, in S1, the molar ratio of hydrogen-containing silane, acrylic resin, platinum dioxide and melamine is 3:3-4:0.0002:1-1.3.

[0008] Preferably, in S1, the mass fraction of the acetic acid aqueous solution is 0.1-0.5 wt%.

[0009] Preferably, in S2, the molar ratio of diisocyanate, oligomeric diol, and silanol-terminated modified melamine compound is 1.2-2: 1-1.3: 0.12-0.8. Preferably, the hydrogen-containing silane is any one of the following: triethoxyhydrogensilane, methyldiethoxyhydrogensilane, trimethoxyhydrogensilane, and methyldimethoxyhydrogensilane.

[0010] Preferably, the acrylate resin is any one of the following: acrylic acid, 3-butenoic acid, 2-butenoic acid, 3-butenoic acid, 4-pentenoic acid, 5-hexenoic acid, 6-heptenoic acid, and 7-octenoic acid.

[0011] Preferably, the diisocyanate is any one of the following or a combination thereof: toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, methylcyclohexyl diisocyanate.

[0012] Preferably, the oligomeric diol is any one of the following or a combination thereof: poly(neopentyl adipate) glycol ester diol, poly(ethylene glycol-propylene glycol) adipate diol, polytetramethylene glycol (PTMG1000, PTMG2000), poly(neopentyl adipate) glycol-1,6-hexanediol adipate diol.

[0013] Beneficial effects: 1. The present invention utilizes the hydrosilylation reaction of hydrogen-containing silane and olefinic resin to introduce carboxyl groups into the organosilicon compound, and then reacts the carboxyl groups with melamine, and further utilizes the hydrolysis of silane alkoxy groups to synthesize novel polyhydroxyl-functionalized silanol-terminated modified melamine compounds, which have excellent flame retardant properties.

[0014] 2. Silicone-modified hyperbranched waterborne polyurethane is prepared by chain extension reaction of designed and synthesized polyhydroxyl-functionalized silanol-terminated modified melamine compounds with isocyanate. The flame retardant functional groups of silicone and melamine are introduced into the molecular chain at the same time, which can effectively improve the flame retardant properties of WPU. Moreover, through in-situ chemical reaction, the two functional groups are dispersed at the molecular level on the waterborne polyurethane molecular chain, which is beneficial to improve the stability of the emulsion and facilitate storage and transportation.

[0015] 3. The water-based polyurethane synthetic leather prepared by using the water-based polyurethane emulsion of the present invention has the characteristics of no solvent residue, high tensile strength, good water resistance, excellent flame retardancy, etc., and has broad market prospects.

[0016] 4. By utilizing the designed and synthesized silanol-terminated modified melamine compounds, cross-linking points are introduced into the polyurethane molecular weight to form a three-dimensional structure, which can not only effectively improve the water resistance, heat resistance and wear resistance of the obtained water-based polyurethane leather products, but also introduce melamine functional groups with excellent flame retardant properties. The obtained water-based polyurethane products have good flame retardancy. DETAILED DESCRIPTION

[0017] The present invention is described in detail below in conjunction with specific embodiments.

[0018] Implementation 1:

[0019] S1. 3 mol of triethoxysilane and 3 mol of acrylic acid were added to a three-necked flask, stirred and mixed for 10 min, and then 0.2 mmol of platinum dioxide was added as a catalyst. After stirring evenly, the mixture was refluxed at 85 °C for 24 h, filtered and distilled, and then 1 mol of melamine and 200 mL of methanol were added. After reacting for 6 h, the methanol was distilled off, and then a measured amount of acetic acid aqueous solution (0.1 wt%) was added and reacted for 24 h to obtain a silanol-terminated melamine compound;

[0020] S2. 2 mol of isophorone diisocyanate and 1.2 mol of poly(neopentyl adipate glycol) ester diol were stirred and reacted at 80°C for 2 hours, 0.12 mol of the silanol-terminated modified melamine compound prepared in S1 was added, and the reaction was stirred for 1 hour. A hydrophilic chain extender was added, and the reaction was stirred for 0.5 hour. An organic bismuth catalyst was added, and the reaction was continued with stirring for 1.5 hours. A certain amount of acetone was added, and the reaction was continued with stirring for 1 hour. Water was added and stirred at a high speed for self-emulsification and dispersion. After the system became a uniform emulsion, acetone was removed at 50°C and 0.1 MPa to obtain a melamine-modified organic silicone hyperbranched flame-retardant waterborne polyurethane emulsion.

[0021] Implementation 2:

[0022] S1. 3 mol of methyldiethoxyhydrosilane and 3.2 mol of 3-butenoic acid were added to a three-necked flask, stirred and mixed for 10 min, and then 0.2 mmol of platinum dioxide was added as a catalyst. After stirring evenly, the mixture was refluxed at 85 °C for 24 h, filtered and distilled, and then 1 mol of melamine and 200 mL of methanol were added. After reacting for 6 h, the methanol was distilled off, and then a measured amount of acetic acid aqueous solution (0.2 wt%) was added and reacted for 18 h to obtain a silanol-terminated melamine compound;

[0023] S2. 2 mol of hexamethylene diisocyanate and 1.2 mol of polytetrahydrofuran diol were stirred and reacted at 80°C for 1.5 hours, 0.15 mol of the silanol-terminated modified melamine compound prepared in S1 was added, and the reaction was stirred for 1 hour. A hydrophilic chain extender was added, and the reaction was stirred for 0.5 hours. An organic bismuth catalyst was added, and the reaction was continued with stirring for 1.5 hours. A certain amount of acetone was added, and the reaction was continued with stirring for 1 hour. Water was added and stirred at a high speed for self-emulsification and dispersion. After the system became a uniform emulsion, acetone was removed at 50°C and 0.1 MPa to obtain a melamine-modified hyperbranched flame-retardant waterborne polyurethane emulsion.

[0024] Implementation 3:

[0025] S1. Add 3 mol of trimethoxysilane and 3.5 mol of 4-pentenoic acid into a three-necked flask, stir and mix for 10 min, add 0.2 mmol of platinum dioxide as a catalyst, stir evenly, reflux at 85 °C for 24 h, filter and distill, add 1.3 mol of melamine and 200 mL of methanol, react for 6 h, distill to remove methanol, add a measured amount of acetic acid aqueous solution (0.3 wt%) and react for 10 h to obtain a silanol-terminated melamine compound;

[0026] S2. After 1.2 mol of isophorone diisocyanate and 1.3 mol of polyethylene glycol-propylene glycol adipate diol were stirred and reacted at 80°C for 0.5 hour, 0.8 mol of toluene diisocyanate was added and the stirring and reaction was continued for 1 hour. 0.08 mol of the silanol-terminated melamine compound prepared in S1 was added and the stirring and reaction was continued for 1 hour. A hydrophilic chain extender was added and the stirring and reaction was continued for 0.5 hour. An organic bismuth catalyst was added and the stirring and reaction was continued for 1.5 hours. A certain amount of acetone was added and the stirring and reaction was continued for 1 hour. Water was added and stirred at high speed for self-emulsification and dispersion. After the system became a uniform emulsion, acetone was removed at 50°C and 0.1 MPa to obtain a melamine-modified hyperbranched flame-retardant waterborne polyurethane emulsion.

[0027] Implementation 4:

[0028] S1. 3 mol of methyldimethoxysilane and 4 mol of 6-heptenoic acid were added to a three-necked flask, stirred and mixed for 10 min, and then 0.2 mmol of platinum dioxide was added as a catalyst. After stirring evenly, the mixture was refluxed at 85 °C for 24 h, filtered and distilled, and then 1.15 mol of melamine and 200 mL of methanol were added. After reacting for 6 h, the methanol was distilled off, and then a measured amount of acetic acid aqueous solution (0.5 wt%) was added and reacted for 6 h to obtain a silanol-terminated melamine compound;

[0029] S2. A mixture of 2 mol of isophorone diisocyanate, 0.6 mol of polytetrahydrofuran diol and 0.4 mol of polyneopentyl adipate diol was stirred and reacted at 80°C for 2 hours, 0.2 mol of the silanol-terminated melamine compound prepared by S1 was added, and the reaction was stirred for 1 hour. A hydrophilic chain extender was added, and the reaction was stirred for 0.5 hours. An organic bismuth catalyst was added, and the reaction was continued with stirring for 1.5 hours. A certain amount of acetone was added, and the reaction was continued with stirring for 1 hour. Water was added and stirred at high speed for self-emulsification and dispersion. After the system became a uniform emulsion, acetone was removed at 50°C and 0.1 MPa to obtain a melamine-modified hyperbranched flame-retardant waterborne polyurethane emulsion.

[0030] The melamine-modified hyperbranched flame-retardant aqueous polyurethane emulsion prepared in the above embodiments 1 to 4 has the following data on tensile strength, water resistance, heat resistance and flame retardancy of the film:

[0031] sample Tensile strength (MPa) Water immersion weight loss rate (wt.%) Initial decomposition temperature (°C) Flame retardant grade Example 1 14.6 0.12 232 Flame retardant Example 2 12.9 0.06 224 Flame retardant Example 3 11.5 0.14 229 Flame retardant Example 4 13.4 0.08 230 Flame retardant

[0032] Tensile strength: The polyurethane resin is made into a film with a thickness of about 1mm on a tetrafluoroethylene plate. After being completely dried, it is measured by a GMT-4204 microcomputer-controlled electronic universal testing machine produced by Meters Process Systems (China) Co., Ltd. in accordance with GB 8949-2008-T.

[0033] Water resistance: The polyurethane resin was made into a film with a thickness of about 1 mm on a tetrafluoroethylene plate. After being completely dried, it was immersed in deionized water at 25°C for 120 hours. After drying, it was weighed to examine the change in film weight before and after immersion.

[0034] Heat resistance: The polyurethane resin was made into a film with a thickness of about 1 mm on a tetrafluoroethylene plate. After complete drying, the sample was tested using a STA 409PC synchronous thermal analyzer in a nitrogen atmosphere at a heating rate of 10 ℃ / min from room temperature to 600 ℃.

[0035] Flame retardancy: measured by ZR-01 oxygen index tester produced by Qingdao Shanfang Instrument Co., Ltd., and divided into grades according to the value of oxygen index. Oxygen index less than 22% is flammable material, oxygen index greater than 27% is difficult to burn, and oxygen index between 22% and 27% is combustible material.

[0036] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent transformation or modification made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a hyperbranched flame-retardant aqueous polyurethane emulsion, characterized in that: The following steps are involved: S1: After mixing the hydrosilane and the acrylate resin evenly, add platinum dioxide as a catalyst, stir evenly, reflux at 80-90°C for 20-30h, add melamine and methanol after filtration and distillation, react for 4-8h, remove the methanol, add acetic acid aqueous solution and react for 6-24h to obtain a silanol-terminated modified melamine compound; Wherein, the hydrosilane is any one of the following: Triethoxysilane, methyldiethoxysilane, trimethoxysilane, methyldimethoxysilane; The molar ratio of hydrogen-containing silane, acrylic resin, platinum dioxide and melamine is 3:3-4:0.0002:1-1.3; S2: diisocyanate and oligomeric diol are stirred and reacted at 75-85°C for 0.5-2 hours, a certain amount of silanol-terminated modified melamine compound is added, and the reaction is stirred for 0.5-1.5 hours, a hydrophilic chain extender is added, and the reaction is stirred for 20-40 minutes, and an organic bismuth catalyst is added, and the reaction is continued with stirring for 1-2 hours, a certain amount of acetone is added, and the reaction is continued with stirring for 0.5-1.5 hours, and water is added for self-emulsification and dispersion by high-speed stirring. After the system becomes a uniform emulsion, the acetone is removed to obtain a melamine-modified hyperbranched flame-retardant waterborne polyurethane emulsion; The molar ratio of diisocyanate, oligomeric diol and silanol-terminated modified melamine compound is 1.2-2: 1-1.3: 0.12-0.

8.

2. The method for preparing a hyperbranched flame-retardant aqueous polyurethane emulsion according to claim 1, characterized in that: The molecular formula of the silanol-terminated modified melamine compound is as follows: 。 3. The method for preparing a hyperbranched flame-retardant aqueous polyurethane emulsion according to claim 1, characterized in that: In S1, the mass fraction of the acetic acid aqueous solution is 0.1-0.5wt%.

4. The method for preparing a hyperbranched flame-retardant aqueous polyurethane emulsion according to claim 1, characterized in that: In S2, acetone was removed at 50°C and 0.1 MPa.

5. The method for preparing a hyperbranched flame-retardant aqueous polyurethane emulsion according to any one of claims 1 to 4, characterized in that: The acrylic resin is any one of the following: Acrylic acid, 3-butenoic acid, 2-butenoic acid, 4-pentenoic acid, 5-hexenoic acid, 6-heptenoic acid, 7-octenoic acid.

6. The method for preparing a hyperbranched flame-retardant aqueous polyurethane emulsion according to any one of claims 1 to 4, characterized in that: The diisocyanate is any one or a combination of the following: Toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, methylcyclohexyl diisocyanate.

7. The method for preparing a hyperbranched flame-retardant aqueous polyurethane emulsion according to any one of claims 1 to 4, characterized in that: The oligomeric diol is any one or a combination of the following: Polyethylene glycol-propylene glycol adipate diol, polytetramethylene glycol adipate diol, polyneopentyl glycol-1,6-hexanediol adipate diol.