Method for collaboratively removing nitrogen oxides, mercury and dioxins, catalyst and method for preparing catalyst

By using a catalyst system with support such as titanium oxide and active ingredients such as vanadium oxide, synergistically removes nitrogen oxides, mercury and dioxins, the emission control problem in the existing technology is solved, and high efficiency and stability are achieved The removal of multiple pollutants is suitable for industrial applications.

CN116116210BActive Publication Date: 2024-11-12TSINGHUA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310198801.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-03
Publication Date
2024-11-12
Estimated Expiration
2043-03-03

AI Technical Summary

Technical Problem

The prior art is difficult to effectively control the emission of nitrogen oxides (NOx), mercury (Hg0) and dioxins under the absence of hydrogen chloride, and the tungsten-titanium catalyst may increase the dioxin content during the process.

Method used

Using a synergistic catalyst composed of support such as titanium oxide, aluminum oxide and active ingredients such as vanadium oxide, the NOx and dioxin are treated separately through a two-step catalyst system, and the catalytic performance is enhanced by using sulfate ions and phosphate ions to achieve the Coordinated removal within the SCR reactor.

Benefits of technology

It achieves excellent NH3 selective reduction NO activity, Hg0 oxidation efficiency and dioxin conversion in the range of 250-350℃, and has stable sulfur and water resistance, reducing industrial costs and space limitations, and is suitable for industrial mass production. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005060240680000171
    Figure GDA0005060240680000171
  • Figure GDA0005060240680000191
    Figure GDA0005060240680000191
  • Figure HDA0004108246700000011
    Figure HDA0004108246700000011
Patent Text Reader

Abstract

The present invention provides a method for collaboratively removing nitrogen oxides, mercury and dioxins, a catalyst and a method for preparing the catalyst. The method for collaboratively removing nitrogen oxides, mercury and dioxins comprises the following steps: a step of removing nitrogen oxides using a first catalyst; and a step of removing dioxins and mercury using a second catalyst. The method for removing nitrogen oxides, mercury and dioxins of the present invention is simple and easy to operate, has broad application prospects, and is suitable for industrial mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for removing nitrogen oxides, mercury and dioxins, a catalyst and a method for preparing the catalyst, and belongs to the field of environmental protection and waste gas purification. Background Art

[0002] With the rapid development of modern industry, a large amount of industrial waste gas has caused increasingly serious air pollution, which has become one of the most concerned issues. x ) is an important primary pollutant that causes haze and ground-level ozone. Dioxin is a persistent and highly toxic substance that can directly and seriously harm the human body and other organisms. Mercury (Hg 0 ) is highly toxic and bioaccumulative, causing a variety of adverse effects on human health and biological systems. x , dioxin and Hg 0 It coexists in the flue gas of industrial processes such as cement production, metal smelting, waste incineration, and steel sintering. In order to solve the above pollution problems, countries around the world are gradually tightening the emission standards of related industrial flue gas.

[0003] Ammonia selective catalytic reduction (NH3-SCR) denitrification technology is currently the most widely used technology in industry. The core technology of SCR is commercial vanadium-based catalyst, which can effectively control NO x At the same time, a large number of studies have shown that vanadium-based SCR catalysts can indeed promote Hg 0 The oxidation of volatile organic compounds (VOCs) can also be achieved, which makes it possible to use SCR catalysts to simultaneously achieve the oxidation of NO x , Hg 0 It is possible to control multiple pollutants such as VOCs, but this process requires the injection of hydrogen chloride (HCl), which will cause corrosion to the equipment. At the same time, in actual applications, it is found that after the flue gas passes through the vanadium tungsten titanium catalyst, the dioxin content will increase instead of decrease, which makes the tungsten titanium catalyst also a dioxin producer.

[0004] Therefore, a catalyst was used to effectively control NO in the absence of HCl. x , Hg 0 The emission of multiple pollutants such as CO2 and VOCs will have great theoretical, economic and practical significance for the development of promising multi-pollution control technologies. Summary of the invention

[0005] Problem that the invention aims to solve

[0006] In view of the technical problems existing in the current technology, the present invention first provides a method for removing nitrogen oxides, mercury and dioxins. The method of the present invention is simple and easy to operate, and has broad application prospects.

[0007] Furthermore, the present invention also provides a catalyst for removing nitrogen oxides, mercury and dioxins, which has excellent catalytic effect, excellent NH3 selective reduction of NO activity, Hg 0 Oxidation efficiency, dioxin (chlorobenzene) conversion rate, and stable anti-sulfur and water resistance.

[0008] Furthermore, the present invention also provides a method for preparing the catalyst, which is simple and easy to implement, and the raw materials are easy to obtain, and is suitable for industrial mass production.

[0009] Solutions for solving problems

[0010] The present invention provides a method for collaboratively removing nitrogen oxides, mercury and dioxins, which comprises the following steps:

[0011] A step of removing nitrogen oxides using a first catalyst;

[0012] A step of removing dioxins and mercury using a second catalyst.

[0013] According to the method of the present invention, the first catalyst comprises a first carrier and a first active ingredient. Based on the total mass of the first catalyst being 100%, the content of the first carrier is 80-99%; the content of the first active ingredient is 1-15%.

[0014] According to the method of the present invention, the first carrier comprises one or a combination of two or more of titanium oxide, aluminum oxide, cerium oxide, zirconium oxide, tin oxide and silicon oxide; and / or

[0015] The first active component includes one or a combination of two or more of vanadium oxide, iron oxide, copper oxide, tungsten oxide, molybdenum oxide and manganese oxide.

[0016] According to the method of the present invention, based on the total mass of the first catalyst as 100%, in the first carrier, the content of the titanium oxide is 75%-90%, the content of the aluminum oxide is 0%-5%, the content of the cerium oxide is 1%-10%, the content of the zirconium oxide is 0%-5%, the content of the tin oxide is 1%-10%, and the content of the silicon oxide is 0%-5%; and / or

[0017] Taking the total mass of the first catalyst as 100%, in the first active ingredient, the content of the vanadium oxide is 1%-3%, the content of the iron oxide is 0%-5%, the content of the copper oxide is 0%-1%, the content of the tungsten oxide is 0%-5%, the content of the molybdenum oxide is 1%-5%, and the content of the manganese oxide is 1%-5%.

[0018] According to the method of the present invention, the first catalyst further contains sulfate ions; based on the total mass of the first catalyst being 100%, the content of the sulfate ions is 1.5 to 3% in terms of SO3; and / or

[0019] The first catalyst further contains phosphate ions. Based on the total mass of the first catalyst being 100%, the content of the phosphate ions is less than 5% in terms of P2O5.

[0020] According to the method of the present invention, the second catalyst comprises a second carrier and a second active ingredient. Based on the total mass of the second catalyst being 100%, the content of the second carrier is 80-99%; the content of the second active ingredient is 1-15%.

[0021] According to the method of the present invention, the second carrier comprises one or a combination of two or more of titanium oxide, aluminum oxide, cerium oxide, zirconium oxide, tin oxide and silicon oxide; and / or

[0022] The second active component includes one or a combination of two or more of ruthenium oxide, platinum oxide, cobalt oxide, gold oxide, vanadium oxide, iron oxide, copper oxide, molybdenum oxide and manganese oxide.

[0023] According to the method of the present invention, based on the total mass of the second catalyst as 100%, in the second carrier, the content of the titanium oxide is 70%-90%, the content of the aluminum oxide is 0%-5%, the content of the cerium oxide is 1%-10%, the content of the zirconium oxide is 0%-5%, the content of the tin oxide is 1%-10%, and the content of the silicon oxide is 0%-5%; and / or

[0024] Taking the total mass of the second catalyst as 100%, in the second active ingredient, the content of ruthenium oxide is 0.1%-1%, the content of platinum oxide is 0%-1%, the content of cobalt oxide is 1%-20%, the content of gold oxide is 0%-1%, the content of vanadium oxide is 0%-5%, the content of iron oxide is 0%-1%, the content of copper oxide is 0%-5%, the content of molybdenum oxide is 0%-5%, and the content of manganese oxide is 0%-10%.

[0025] According to the method of the present invention, the second catalyst further contains phosphate ions, and based on the total mass of the second catalyst being 100%, the content of the phosphate ions is less than 5% in terms of P2O5.

[0026] The present invention also provides a catalyst, which comprises the first catalyst according to the present invention.

[0027] The present invention also provides a method for preparing the first catalyst according to the present invention, which comprises the following steps:

[0028] dissolving a precursor of a first carrier in a solvent to obtain a first carrier precursor solution;

[0029] The first carrier precursor solution is mixed with an alkaline precipitant and then dried to obtain a first carrier dry product;

[0030] calcining the first carrier dried product to obtain a first carrier;

[0031] dissolving a precursor of a first active ingredient and a co-solvent in a solvent to obtain a first active ingredient precursor solution;

[0032] Mixing a first carrier, an optional structural aid and a first active ingredient precursor solution and drying the mixture to obtain a first mixed product;

[0033] calcining the first mixed product to obtain a first catalyst powder;

[0034] The first catalyst powder is made into a slurry, and the slurry is extruded or coated onto a substrate to obtain a first catalyst precursor;

[0035] The first catalyst precursor is dried and then calcined to obtain a first catalyst.

[0036] The present invention further provides a catalyst, which comprises the second catalyst according to the present invention.

[0037] The present invention further provides a method for preparing the first catalyst according to the present invention, which comprises the following steps:

[0038] dissolving a precursor of a second carrier in a solvent to obtain a second carrier precursor solution;

[0039] The second carrier precursor solution is mixed with an alkaline precipitant and then dried to obtain a second carrier dry product;

[0040] calcining the second carrier dried product to obtain a second carrier;

[0041] dissolving a precursor of a second active ingredient and a co-solvent in a solvent to obtain a second active ingredient precursor solution;

[0042] Mixing a second carrier, an optional structural aid and a second active ingredient precursor solution and drying the mixture to obtain a second mixed product;

[0043] calcining the second mixed product to obtain a second catalyst powder;

[0044] The second catalyst powder is made into slurry, and the slurry is extruded or coated onto a substrate to obtain a second catalyst precursor;

[0045] The second catalyst precursor is dried and then calcined to obtain a second catalyst.

[0046] Effects of the Invention

[0047] Compared with the prior art, the present invention has at least one of the following beneficial effects:

[0048] (1) The method for removing nitrogen oxides, mercury and dioxins of the present invention is simple and easy to implement, convenient to operate, has broad application prospects, and is suitable for industrial mass production.

[0049] (2) The catalyst prepared by the present invention for removing nitrogen oxides, mercury and dioxins exhibits good activity for selective reduction of NO by NH3 in the range of 250-350°C. 0 Oxidation efficiency, dioxin (chlorobenzene) conversion rate, and stable anti-sulfur and water resistance.

[0050] (3) The catalyst for removing nitrogen oxides, mercury and dioxins prepared by the present invention can be used in one SCR reactor, which reduces industrial costs, solves space limitations, and does not require separation of SCR and Hg 0 , dioxin (chlorobenzene) oxidation unit, which is environmentally friendly and green. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 The invention shows a method for removing nitrogen oxides, mercury and dioxins in an integrated series process and a corresponding performance curve in an application process;

[0052] Figure 2 Another method for removing nitrogen oxides, mercury and dioxins of the present invention is shown in the application process of the split series process and the corresponding performance curve. DETAILED DESCRIPTION

[0053] Various exemplary embodiments, features and aspects of the present invention will be described in detail below. The word "exemplary" used here means "used as an example, embodiment or illustrative". Any embodiment described here as "exemplary" is not necessarily interpreted as being superior or better than other embodiments.

[0054] In addition, in order to better illustrate the present invention, numerous specific details are provided in the following specific embodiments. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In other examples, methods, means, equipment and steps well known to those skilled in the art are not described in detail in order to highlight the subject matter of the present invention.

[0055] Unless otherwise stated, the units used in this specification are all international standard units, and the numerical values ​​and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.

[0056] In this specification, the word "may" means both performing a certain process and not performing a certain process.

[0057] In this specification, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.

[0058] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values ​​A and B.

[0059] In this specification, when "normal temperature" or "room temperature" is used, the temperature may be 10-40°C.

[0060] <First aspect>

[0061] First Catalyst

[0062] The first aspect of the present invention first provides a first catalyst. The first catalyst of the present invention comprises a first carrier and a first active ingredient. Taking the total mass of the first catalyst as 100%, the content of the first carrier is 80-99%, for example: 82%, 84%, 86%, 88%, 92%, 94%, 96%, 98%, etc.; the content of the first active ingredient is 1-15%, for example: 2%, 4%, 6%, 8%, 10%, 12%, 14%, etc. When the content of the first carrier is 80-99% and the content of the first active ingredient is 1-15%, the catalytic performance of the first catalyst is excellent.

[0063] In the present invention, the main function of the first carrier is to provide a large specific surface area, stability and mechanical strength, a certain catalyst shape and size, disperse the first active component, reduce the amount of the first active component used, and improve the anti-poisoning performance of the catalyst. The main function of the first active component of the present invention is to provide NO x The first catalyst of the present invention has an ammonia oxidation rate of less than 10% at 300°C.

[0064] In some specific embodiments, the first carrier comprises one or a combination of two or more of titanium oxide, aluminum oxide, cerium oxide, zirconium oxide, tin oxide and silicon oxide; and / or the first active ingredient comprises one or a combination of two or more of vanadium oxide, iron oxide, copper oxide, tungsten oxide, molybdenum oxide and manganese oxide.

[0065] Specifically, based on the total mass of the first catalyst as 100%, in the first carrier, the content of titanium oxide is 75%-90%, for example: 78%, 80%, 82%, 84%, 86%, 88% and the like; the content of aluminum oxide is 0%-5%, for example: 1%, 2%, 3%, 4% and the like; the content of cerium oxide is 1%-10%, for example: 2%, 4%, 6%, 8% and the like; the content of zirconium oxide is 0%-5%, for example: 1%, 2%, 3%, 4% and the like; the content of tin oxide is 1%-10%, for example: 2%, 4%, 6%, 8% and the like; the content of silicon oxide is 0%-5%, for example: 1%, 2%, 3%, 4% and the like.

[0066] Taking the total mass of the first catalyst as 100%, in the first active ingredient, the content of the vanadium oxide is 1%-3%, for example: 1.5%, 2%, 2.5%, etc.; the content of the iron oxide is 0%-5%, for example: 1%, 2%, 3%, 4%, etc.; the content of the copper oxide is 0%-1%, for example: 0.2%, 0.4%, 0.6%, 0.8%, etc.; the content of the tungsten oxide is 0%-5%, for example: 1%, 2%, 3%, 4%, etc.; the content of the molybdenum oxide is 1%-5%, for example: 2%, 3%, 4%, etc.; the content of the manganese oxide is 1%-5%, for example: 2%, 3%, 4%, etc.

[0067] When the contents of the first carrier and the first active material of the present invention are within the above ranges, the function of the first catalyst can be most effectively exerted.

[0068] It should be noted that the total content of other impurity oxides in the first catalyst of the present invention should be less than 1%.

[0069] In some specific embodiments, the first catalyst also contains sulfate ions; taking the total mass of the first catalyst as 100%, the content of sulfate ions in terms of SO3 is 1.5-3%, for example: 1.8%, 2%, 2.2%, 2.5%, 2.8%, etc.

[0070] In the present invention, sulfate ions can be used to enhance the adsorption of reducing agent ammonia to promote denitrification activity, while inhibiting the over-oxidation of ammonia molecules and inhibiting the generation of byproducts such as nitrous oxide. Generally speaking, sulfate ions in the catalyst come from sulfur-containing impurities in titanium dioxide itself. If the sulfate content is insufficient, additional sulfate substances need to be added to increase the sulfur content in the finished catalyst.

[0071] In some specific embodiments, the first catalyst composition further contains phosphate ions, and the content of the phosphate ions is 5% or less, preferably greater than 0% and less than 5%, such as 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, etc., based on the total mass of the first catalyst composition as 100%, and calculated as P2O5. In the present invention, the phosphate ions can stabilize the active sites on the surface of the first catalyst, so that it maintains the configuration at high temperature (>300°C); at the same time, they also have a certain effect of enhancing ammonia adsorption and inhibiting the generation of nitrous oxide.

[0072] Preparation method of the first catalyst

[0073] The first aspect of the present invention also provides a method for preparing a first catalyst according to the present invention, which comprises the following steps:

[0074] dissolving a precursor of a first carrier in a solvent to obtain a first carrier precursor solution;

[0075] The first carrier precursor solution is mixed with an alkaline precipitant and then dried to obtain a first carrier dry product;

[0076] calcining the first carrier dried product to obtain a first carrier;

[0077] dissolving a precursor of a first active ingredient and a co-solvent in a solvent to obtain a first active ingredient precursor solution;

[0078] Mixing a first carrier, an optional structural aid and a first active ingredient precursor solution and drying the mixture to obtain a first mixed product;

[0079] calcining the first mixed product to obtain a first catalyst powder;

[0080] The first catalyst powder is made into a slurry, and the slurry is extruded or coated onto a substrate to obtain a first catalyst precursor;

[0081] The first catalyst precursor is dried and then calcined to obtain a first catalyst.

[0082] The precursor of the first carrier may include a soluble salt of the first carrier or an oxide of the first carrier, or a combination of one or more thereof. Specifically, the soluble salt may be a mixture of one or more of their respective inorganic acid salts such as nitrates, sulfates, hydrochlorides, or their hydrates, or may be a mixture of one or more of their respective organic acid salts such as acetates, oxalates, or their hydrates.

[0083] Similarly, the first active ingredient precursor includes one or a combination of two or more soluble salts of the first active ingredient. Specifically, the soluble salt may be a mixture of one or more inorganic acid salts such as nitrates, sulfates, hydrochlorides, or hydrates thereof, or may be a mixture of one or more organic acid salts such as acetates, oxalates, or hydrates thereof.

[0084] Specifically, the precursor of the first carrier includes one or more combinations of titanium source, aluminum source, cerium source, zirconium source, tin source and silicon source; the titanium source includes one or more combinations of titanium tetrachloride, titanium sulfate, TiO2, tetrabutyl titanate, titanium sol; the aluminum source includes one or more combinations of aluminum sulfate, aluminum chloride, aluminum nitrate, aluminum sol, etc.; the cerium source includes one or more combinations of cerium chloride, cerium nitrate, cerium sulfate, etc.; the zirconium source includes one or more combinations of zirconium chloride, zirconium nitrate, zirconium sulfate, etc.; the tin source includes one or more combinations of tin chloride (tin tetrachloride), stannous chloride, stannous sulfate, stannous nitrate, stannous oxalate, etc.; the silicon source includes one or more combinations of silicon dioxide, silicic acid, aluminum silicate, silica sol, etc.

[0085] The first active component precursor includes one or more of a vanadium source, an iron source, a copper source, a tungsten source, a molybdenum source and a manganese source. The vanadium source includes one or more of ammonium metavanadate, vanadium oxysulfate and vanadium tetrachloride; the iron source includes one or more of ferrous sulfate, ferric chloride and ferric nitrate; the copper source includes one or more of copper sulfate, copper chloride and copper nitrate; the tungsten source includes one or more of ammonium tungstate, ammonium metatungstate and ammonium paratungstate; the molybdenum source includes one or more of ammonium metamolybdate, ammonium molybdate and ammonium paramolybdate; the manganese source includes one or more of manganese nitrate, manganese chloride and manganese sulfate.

[0086] The present invention does not specifically limit the solvent used to dissolve the first active ingredient precursor, and it can be some commonly used solvents in the art, such as water, etc. In addition, when dissolving the precursor, some auxiliary solvents can be used in consideration of the dissolution conditions.

[0087] The present invention does not specifically limit the alkaline precipitant, and it can be some alkaline substances commonly used in the art, such as NaOH, KOH, ammonia water and other commonly used alkaline substances. The present invention does not specifically limit the amount of the alkaline precipitant, and generally the pH value is adjusted to 8-11.

[0088] Furthermore, a structural additive may be added to the first mixed product, and the mass content of the structural additive may be 1%-8%. Specifically, in the present invention, the structural additive may be glass fiber, ceramic fiber, etc.

[0089] For drying, in the present invention, the drying temperature can be 50-90°C and the drying time can be 2-20 hours. Calcination can be carried out in a staged activation manner, specifically, calcination can be carried out at 150-200°C for 1-3 hours, and then calcination can be carried out at 400-600°C for 1-3 hours.

[0090] <Second Aspect>

[0091] Second catalyst

[0092] The second aspect of the present invention first provides a second catalyst. The second catalyst of the present invention comprises a second carrier and a second active ingredient, and based on the total mass of the second catalyst as 100%, the content of the second carrier is 80-99%, for example: 82%, 84%, 86%, 88%, 92%, 94%, 96%, 98%, etc.; the content of the second active ingredient is 1-15%, for example: 2%, 4%, 6%, 8%, 10%, 12%, 14%, etc.

[0093] The second catalyst of the present invention has a mercury removal rate of more than 95% in the range of 200-350°C, a dioxin removal rate of more than 90% at 275°C, and has stable sulfur and water resistance.

[0094] In some specific embodiments, the second carrier comprises one or a combination of two or more of titanium oxide, aluminum oxide, cerium oxide, zirconium oxide, tin oxide and silicon oxide; and / or, the second active ingredient comprises one or a combination of two or more of ruthenium oxide, platinum oxide, cobalt oxide, gold oxide, vanadium oxide, iron oxide, copper oxide, molybdenum oxide and manganese oxide.

[0095] Specifically, based on the total mass of the second catalyst as 100%, in the second carrier, the content of titanium oxide is 70%-90%, for example: 72%, 74%, 76%, 78%, 80%, 82%, 84%, 86%, 88% and the like; the content of aluminum oxide is 0%-5%, for example: 1%, 2%, 3%, 4% and the like; the content of cerium oxide is 1%-10%, for example: 2%, 4%, 6%, 8% and the like; the content of zirconium oxide is 0%-5%, for example: 1%, 2%, 3%, 4% and the like; the content of tin oxide is 1%-10%, for example: 2%, 4%, 6%, 8% and the like; the content of silicon oxide is 0%-5%, for example: 1%, 2%, 3%, 4% and the like.

[0096] Taking the total mass of the second catalyst as 100%, in the second active component, the content of the ruthenium oxide is 0.1%-1%, for example: 0.3%, 0.5%, 0.7%, 0.9%, etc.; the content of the platinum oxide is 0%-1%, for example: 0.1%, 0.3%, 0.5%, 0.7%, 0.9%, etc.; the content of the cobalt oxide is 1%-20%, for example: 2%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, etc.; the content of the gold oxide is 0%-1%, for example: 0.1%, 0 .3%, 0.5%, 0.7%, 0.9% and the like; the content of the vanadium oxide is 0%-5%, for example: 1%, 2%, 3%, 4% and the like; the content of the iron oxide is 0%-1%, for example: 0.1%, 0.3%, 0.5%, 0.7%, 0.9% and the like; the content of the copper oxide is 0%-5%, for example: 1%, 2%, 3%, 4% and the like; the content of the molybdenum oxide is 0%-5%, for example: 1%, 2%, 3%, 4% and the like; the content of the manganese oxide is 0%-10%, for example: 2%, 4%, 6%, 8% and the like.

[0097] When the contents of the components of the second carrier and the second active material of the present invention are within the above ranges, the function of the second catalyst can be most effectively exerted.

[0098] It should be noted that the total content of other impurity oxides in the second catalyst of the present invention should be less than 1%.

[0099] In some specific embodiments, the second catalyst further contains phosphate ions. Taking the total mass of the second catalyst as 100%, the content of the phosphate ions is 5% or less, preferably greater than 0% and less than 5%, such as 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, etc. In the second catalyst of the present invention, the phosphate ions enhance the catalyst's and Lewis acid sites, and through steric effects, the addition of phosphate groups enhances the interaction between molecules on the catalyst surface.

[0100] Preparation method of the second catalyst

[0101] The second aspect of the present invention also provides a method for preparing a second catalyst according to the present invention, which comprises the following steps:

[0102] dissolving a second carrier precursor in a solvent to obtain a second carrier precursor solution;

[0103] The second carrier precursor solution is mixed with an alkaline precipitant and then dried to obtain a second carrier dry product;

[0104] calcining the second carrier dried product to obtain a second carrier;

[0105] dissolving a precursor of a second active ingredient and a co-solvent in a solvent to obtain a second active ingredient precursor solution;

[0106] Mixing a second carrier, an optional structural aid and a second active ingredient precursor solution and drying the mixture to obtain a second mixed product;

[0107] calcining the second mixed product to obtain a second catalyst powder;

[0108] The second catalyst powder is made into slurry, and the slurry is extruded or coated onto a substrate to obtain a second catalyst precursor;

[0109] The second catalyst precursor is dried and then calcined to obtain a second catalyst.

[0110] The precursor of the second carrier may include a soluble salt of the second carrier or an oxide of the second carrier, or a combination of one or more thereof. Specifically, the soluble salt may be a mixture of one or more thereof of an inorganic acid salt such as nitrate, sulfate, hydrochloride, or a hydrate thereof, or may be a mixture of one or more thereof of an organic acid salt such as acetate, oxalate, or a hydrate thereof.

[0111] The second active ingredient precursor includes one or a combination of two or more soluble salts of the second active ingredient. Specifically, the soluble salt may be a mixture of one or more inorganic acid salts such as nitrates, sulfates, hydrochlorides, or hydrates thereof, or may be a mixture of one or more organic acid salts such as acetates, oxalates, or hydrates thereof.

[0112] Specifically, the precursor of the second carrier includes one or more combinations of titanium source, aluminum source, cerium source, zirconium source, tin source and silicon source; the titanium source includes one or more combinations of titanium tetrachloride, titanium sulfate, TiO2, tetrabutyl titanate, titanium sol; the aluminum source includes one or more combinations of aluminum sulfate, aluminum chloride, aluminum nitrate, aluminum sol, etc.; the cerium source includes one or more combinations of cerium chloride, cerium nitrate, cerium sulfate, etc.; the zirconium source includes one or more combinations of zirconium chloride, zirconium nitrate, zirconium sulfate, etc.; the tin source includes one or more combinations of tin chloride (tin tetrachloride), stannous chloride, stannous sulfate, stannous nitrate, stannous oxalate, etc.; the silicon source includes one or more combinations of silicon dioxide, silicic acid, aluminum silicate, silica sol, etc.

[0113] The second active component precursor includes one or more combinations of ruthenium source, platinum source, cobalt source, gold source, vanadium source, iron source, copper source, molybdenum source and manganese source. The ruthenium source includes one or more combinations of ruthenium chloride, ruthenium nitrate and ruthenium sulfate; the platinum source includes one or more combinations of chloroplatinic acid, ammonium chloroplatinate and potassium chloroplatinate; the cobalt source includes one or more combinations of cobalt nitrate, cobalt chloride and cobalt sulfate; the gold source includes chloroauric acid; the vanadium source includes one or more combinations of ammonium metavanadate, vanadium oxysulfate and vanadium tetrachloride; the iron source includes one or more combinations of ferrous sulfate, ferric chloride and ferric nitrate; the copper source includes one or more combinations of copper sulfate, copper chloride and copper nitrate; the molybdenum source includes one or more combinations of ammonium metamolybdate, ammonium molybdate and ammonium paramolybdate; the manganese source includes one or more combinations of manganese nitrate, manganese chloride and manganese sulfate.

[0114] The present invention does not specifically limit the solvent used to dissolve the second active ingredient precursor, and it can be some commonly used solvents in the art, such as water, etc. In addition, when dissolving the precursor, some auxiliary solvents can be used in consideration of the dissolution conditions.

[0115] The present invention does not specifically limit the alkaline precipitant, and it can be some alkaline substances commonly used in the art, such as NaOH, KOH, ammonia water and other commonly used alkaline substances. The present invention does not specifically limit the amount of the alkaline precipitant, and generally the pH value is adjusted to 8-11.

[0116] Furthermore, a structural additive may be added to the second mixed product. The mass content of the structural additive is 1%-8%. Specifically, in the present invention, the structural additive may be glass fiber, ceramic fiber, etc.

[0117] For drying, in the present invention, the drying temperature can be 50-90°C and the drying time can be 2-20 hours. Calcination can be carried out in a staged activation manner, specifically, calcination can be carried out at 150-200°C for 1-3 hours, and then calcination can be carried out at 400-600°C for 1-3 hours.

[0118] <Third Aspect>

[0119] The third aspect of the present invention provides a method for synergistically removing nitrogen oxides, mercury and dioxins, which comprises the following steps:

[0120] A step of removing nitrogen oxides using a second catalyst;

[0121] A step of removing dioxins and mercury using a second catalyst.

[0122] In the present invention, the first catalyst and the second catalyst in the series method are located in the same reactor, i.e., a dual-function reactor; in the integrated series method, the first catalyst accounts for 50%-80% of the total length of the substrate, and the second catalyst accounts for 20%-50% of the total length of the substrate. In the split series method, the first catalyst layer is close to the air inlet end, and the second catalyst layer is close to the air outlet end. In the integrated method, the first catalyst accounts for 50%-80% of the total length of the substrate, and the second catalyst accounts for 20%-50% of the total length of the substrate.

[0123] The integrated series connection method and application process have the characteristics of small footprint, simple operation, low energy consumption, etc., which can greatly reduce the cost of flue gas treatment. The split series connection method and application process have the characteristics of flexible installation and wide application range, and can be modified on the basis of the original flue gas treatment facilities.

[0124] The method for removing nitrogen oxides, mercury and dioxins of the present invention shows good denitrification rate (70-99%) and mercury removal efficiency (80%-95%) in the range of 200-350°C, and the dioxin (chlorobenzene) removal rate is higher than 90% at 275°C, and has stable sulfur and water resistance.

[0125] Example

[0126] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0127] Example 1

[0128] (1) Preparation of the first catalyst

[0129] Dissolve titanium tetrachloride, silica sol, cerium nitrate and tin tetrachloride in appropriate amount of water, add alkaline precipitant ammonia water, control the pH to 9, filter and wash until the pH is about 7, dry at 60℃ for 10h, calcine at 180℃ for 2h, calcine at 500℃ for 2h to obtain a catalyst carrier; then dissolve the co-solvent monoethanolamine in appropriate amount of water, then add ammonium metavanadate, ammonium metamolybdate, ammonium metatungstate and ammonium sulfate and ammonium phosphate to dissolve; immediately add the prepared catalyst carrier, add glass fiber (mass content 3%), mix, and extrude into a honeycomb catalyst. Dry at 80℃ for 6h, calcine at 180℃ for 1h, calcine at 500℃ for 3h, and the heating rate is 1℃ / min to obtain the first catalyst.

[0130] The raw material ratio is calculated according to titanium dioxide (80%, the same mass fraction below), aluminum oxide (3%), cerium dioxide (3.5%), tin dioxide (5%), vanadium pentoxide (1.5%), molybdenum trioxide (1.5%), tungsten trioxide (1.5%) and sulfate (2.5%), phosphate (1.5%).

[0131] The ammonia oxidation efficiency of the catalyst was tested by simulating actual working conditions. The simulated gas components included: 500ppm NH3, 6% O2, N2 as the balance gas, the reaction was stabilized at 300℃, and the space velocity was 80000h -1 The ammonia oxidation efficiency was tested using a Gasmet portable Fourier transform infrared gas analyzer, and the ammonia oxidation rate of the obtained catalyst was about 1% at 300°C.

[0132] The specific surface area of ​​the catalyst was measured on an American Micromeritics ASAP 2460 physical adsorption instrument. After the N2 adsorption-desorption curve of the test sample was tested at a low temperature of 77K, the specific surface area of ​​the catalyst was calculated using the Brunauer-EmmettTeller (BET) formula. Before measuring the specific surface area, the catalyst must be vacuum degassed at 300°C for about 3 hours to remove impurities and water adsorbed on the catalyst surface to ensure the accuracy of the results. The specific surface area of ​​the catalyst obtained is about 115m 2 / g.

[0133] (2) Preparation of the Second Catalyst

[0134] Dissolve titanium sulfate, silica sol, cerium nitrate and stannous sulfate in a proper amount of water, add ammonia alkaline precipitant, control the pH to 10, filter and wash to a pH of about 7, dry at 80°C for 8 hours, calcine at 180°C for 3 hours, and calcine at 500°C for 3 hours to obtain a catalyst carrier; then add ruthenium nitrate, cobalt nitrate, ammonium metamolybdate and ammonium phosphate to dissolve; immediately add the prepared catalyst carrier, add glass fiber (mass content 2%) and ceramic fiber (mass content 1%), prepare a slurry, apply it to the catalyst carrier, dry at 80°C for 6 hours, calcine at 180°C for 2 hours, and calcine at 400°C for 3 hours to obtain a second catalyst.

[0135] The raw material ratio is calculated according to titanium dioxide (77%, the same as below in mass fraction), silicon dioxide (3%), cerium dioxide (6.5%), tin dioxide (5%), ruthenium dioxide (0.5%), cobalt tetroxide (3%), molybdenum trioxide (3%) and phosphate (2%).

[0136] The mercury and dioxin efficiency of the catalyst was tested by simulating actual working conditions (using the model compound chlorobenzene for the experiment). The simulated gas components included: 100ppm chlorobenzene, 80ug / m 3 Hg 0 , 6% O2, N2 as balance gas, stable reaction temperature 250-300℃, space velocity 80000h -1 The chlorobenzene removal rate was tested using a Gasmet portable Fourier transform infrared gas analyzer, and the mercury removal efficiency was tested using a Lumex RA-915+ mercury analyzer. The mercury removal efficiency of the obtained catalyst was 99% at 250°C, and the chlorobenzene removal rate was higher than 90% at 275°C.

[0137] The specific surface area of ​​the catalyst was measured on an American Micromeritics ASAP 2460 physical adsorption instrument. After the N2 adsorption-desorption curve of the test sample was tested at a low temperature of 77K, the specific surface area of ​​the catalyst was calculated using the Brunauer-EmmettTeller (BET) formula. Before measuring the specific surface area, the catalyst must be vacuum degassed at 300°C for about 3 hours to remove impurities and water adsorbed on the catalyst surface to ensure the accuracy of the results. The specific surface area of ​​the catalyst obtained is about 135m 2 / g.

[0138] (3) Methods for removing nitrogen oxides, dioxins and mercury

[0139] This embodiment adopts a split-type series connection method and application process, such as Figure 1 As shown, the first catalyst layer is close to the air inlet end, and the second catalyst layer is close to the air outlet end. The two catalysts can be in close contact or have a certain distance between them. The first catalyst is placed in three layers, and then the second catalyst is placed in three layers.

[0140] (4) Performance testing

[0141] The ammonia oxidation efficiency of the catalyst was tested by simulating actual working conditions. The simulated gas components included: 500ppm NH3, 500ppm NO, 100ppm chlorobenzene (when necessary), 80ug / m 3 Hg 0 , 6% O2, N2 as balance gas, air velocity 80000h -1 , using Gasmet portable Fourier transform infrared gas analyzer to test NO x The removal rate and chlorobenzene removal rate were tested using LumexRA-915+ mercury analyzer. Figure 1 As shown), the reaction temperature is 275-350°C, NO x The removal rate is over 90%, the mercury removal rate is 85%, and the chlorobenzene removal rate is over 90%. However, when there is no chlorobenzene, the mercury removal rate is greatly reduced. It can be seen that under this condition, the chlorine species in dioxins can be used to effectively promote mercury oxidation, thereby achieving a synergistic removal effect.

[0142] Pilot test

[0143] In a pilot test at a waste incineration power plant, three layers of the first catalyst were placed on the upper layer, and three layers of the second catalyst were placed on the lower layer. The flue gas was 4000m 3 / h, the inlet flue gas temperature was about 300℃, and the NO x The removal rate and dioxin removal rate were measured, and the mercury removal efficiency was tested using a Lumex RA-915+ mercury analyzer. The results are shown in Table 1.

[0144] Table 1 Experimental results of split process in Example 1

[0145]

[0146] It can be seen from Table 1 that the preparation method and application process of a tandem catalyst for the coordinated removal of nitrogen oxides, mercury and dioxins of the present invention have excellent denitrification and removal of mercury and dioxins performance.

[0147] Example 2

[0148] (1) Preparation of the first catalyst

[0149] Dissolve titanium sulfate, aluminum sol, ammonium cerium nitrate, and tin tetrachloride in an appropriate amount of water, add alkaline precipitant ammonia water and ammonium bicarbonate, control the pH to 10, filter and wash until the pH is about 7, dry at 70°C for 9 hours, calcine at 200°C for 1 hour, and calcine at 500°C for 3 hours to obtain a catalyst carrier; then dissolve the co-solvent monoethanolamine in an appropriate amount of water, and then add ammonium metavanadate, ammonium metamolybdate, ammonium metatungstate, ammonium sulfate, and ammonium phosphate to dissolve; immediately add the prepared catalyst carrier, add glass fiber (mass content 1.5%) and ceramic fiber (mass content 2%), dry at 90°C for 5 hours, calcine at 180°C for 1 hour, calcine at 500°C for 4 hours, and heat up at a rate of 1°C / min to obtain the powder of the first catalyst. Prepare a slurry, apply it to the substrate in a forward direction, the first catalyst accounts for 70% of the total length of the substrate, dry at 80°C for 6 hours, calcine at 180°C for 2 hours, and calcine at 500°C for 3 hours to obtain the first catalyst.

[0150] The raw material ratio is calculated according to titanium dioxide (82%, the same mass fraction below), aluminum oxide (2%), cerium dioxide (3.5%), tin dioxide (4%), vanadium pentoxide (1.5%), molybdenum trioxide (1%), tungsten trioxide (2%) and sulfate (2.5%), phosphate (1.5%).

[0151] The ammonia oxidation efficiency of the catalyst was tested by simulating actual working conditions. The simulated gas components included: 500ppm NH3, 6% O2, N2 as the balance gas, the reaction was stabilized at 300℃, and the space velocity was 80000h -1 The ammonia oxidation efficiency was tested using a Gasmet portable Fourier transform infrared gas analyzer, and the ammonia oxidation rate of the obtained catalyst was about 2% at 300°C.

[0152] The specific surface area of ​​the catalyst was measured on an American Micromeritics ASAP 2460 physical adsorption instrument. After the N2 adsorption-desorption curve of the test sample was tested at a low temperature of 77K, the specific surface area of ​​the catalyst was calculated using the Brunauer-EmmettTeller (BET) formula. Before measuring the specific surface area, the catalyst must be vacuum degassed at 300°C for about 3 hours to remove impurities and water adsorbed on the catalyst surface to ensure the accuracy of the results. The specific surface area of ​​the catalyst obtained is about 110m 2 / g.

[0153] (2) Preparation of the Second Catalyst

[0154] Dissolve tetrabutyl titanate, silica sol, cerium nitrate and stannous sulfate in appropriate amount of water, add alkaline precipitant ammonia water, control pH to 9, filter and wash until pH is about 7, dry at 80℃ for 10h, calcine at 180℃ for 3h, calcine at 450℃ for 2h to obtain catalyst carrier; then add ruthenium nitrate, cobalt nitrate, ammonium metamolybdate and ammonium phosphate to dissolve; immediately add the prepared catalyst carrier, add glass fiber (mass content 2%) and ceramic fiber (mass content 2%), dry at 90℃ for 5h, calcine at 180℃ for 1h, calcine at 400℃ for 4h, and obtain the powder of the second catalyst. Prepare slurry, reversely coat on the substrate, the second catalyst accounts for 30% of the total length of the substrate, dry at 60℃ for 10h, calcine at 180℃ for 3h, calcine at 450℃ for 3h, and obtain the series catalyst with the first catalyst and the second catalyst.

[0155] The raw material ratio is calculated according to titanium dioxide (79%, the same mass fraction below), silicon dioxide (3%), cerium dioxide (7.5%), tin dioxide (3%), ruthenium dioxide (0.5%), cobalt tetroxide (4%), molybdenum trioxide (2%) and phosphate (1%).

[0156] The mercury and dioxin efficiency of the catalyst was tested by simulating actual working conditions (using the model compound chlorobenzene for the experiment). The simulated gas components included: 100ppm chlorobenzene, 80ug / m 3 Hg 0 , 6% O2, N2 as balance gas, stable reaction at 250-300℃, space velocity 80000h -1 The chlorobenzene removal rate was tested using a Gasmet portable Fourier transform infrared gas analyzer, and the mercury removal efficiency was tested using a Lumex RA-915+ mercury analyzer. The mercury removal efficiency of the obtained catalyst was 99% at 250°C, and the chlorobenzene removal rate was higher than 90% at 275°C.

[0157] The specific surface area of ​​the catalyst was measured on an American Micromeritics ASAP 2460 physical adsorption instrument. After the N2 adsorption-desorption curve of the test sample was tested at a low temperature of 77K, the specific surface area of ​​the catalyst was calculated using the Brunauer-EmmettTeller (BET) formula. Before measuring the specific surface area, the catalyst must be vacuum degassed at 300°C for about 3 hours to remove impurities and water adsorbed on the catalyst surface to ensure the accuracy of the results. The specific surface area of ​​the catalyst obtained is about 175m 2 / g.

[0158] (3) Methods for removing nitrogen oxides, dioxins and mercury

[0159] This embodiment adopts an integrated series connection method and application process, such as Figure 2As shown, in the integrated type, the first catalyst occupies 70% of the total length of the substrate, and the second catalyst occupies 30% of the total length of the substrate. When placed, the end coated with the first catalyst is placed at the air inlet end.

[0160] (4) Performance testing

[0161] The ammonia oxidation efficiency of the catalyst was tested by simulating actual working conditions. The simulated gas components included: 500ppm NH3, 500ppm NO, 100ppm chlorobenzene (when necessary), 80ug / m 3 Hg 0 , 6% O2, N2 as balance gas, air velocity 80000h -1 , using Gasmet portable Fourier transform infrared gas analyzer to test NO x The removal rate and chlorobenzene removal rate were tested using LumexRA-915+ mercury analyzer. Figure 2 As shown), the reaction temperature is 275-350°C, NO x The removal rate is over 90%, the mercury removal rate is 80%, and the chlorobenzene removal rate is over 90%. However, when there is no chlorobenzene, the mercury removal rate is greatly reduced. It can be seen that under this condition, the chlorine species in dioxins can be used to effectively promote mercury oxidation, thereby achieving a synergistic removal effect.

[0162] Pilot test

[0163] In a pilot test at a waste incineration power plant, the first catalyst in the integrated type accounts for 70% of the total length of the substrate, and the second catalyst accounts for 30% of the total length of the substrate. When placed, the end coated with the first catalyst is placed at the air inlet end, and the flue gas is 4000m 3 / h, the inlet flue gas temperature was about 300℃, and the NO x The removal efficiency and dioxin removal rate were tested using a Lumex RA-915+ mercury analyzer. The results are shown in Table 2.

[0164] Table 2: Experimental results of integrated process in Example 2

[0165]

[0166] It can be seen from Table 2 that the preparation method and application process of a tandem catalyst for the coordinated removal of nitrogen oxides, mercury and dioxins of the present invention have excellent denitrification and removal of mercury and dioxins performance.

[0167] It should be noted that, although the technical solution of the present invention is introduced with specific examples, those skilled in the art will appreciate that the present invention should not be limited thereto.

[0168] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A method for synergistically removing nitrogen oxides, mercury and dioxins, characterized in that: The following steps are involved: A step of removing nitrogen oxides using a first catalyst; The step of removing dioxins and mercury using a second catalyst; wherein, The second catalyst comprises a second carrier and a second active component. Based on the total mass of the second catalyst being 100%, the content of the second carrier is 80-99%; the content of the second active component is 1-15%; The second carrier includes titanium oxide, cerium oxide and tin oxide; the second active component includes ruthenium oxide and cobalt oxide; wherein, Based on the total mass of the second catalyst as 100%, in the second carrier, the content of the titanium oxide is 70%-90%, the content of the cerium oxide is 1%-10%, and the content of the tin oxide is 1%-10%; Based on 100% of the total mass of the second catalyst, in the second active component, the content of the ruthenium oxide is 0.1%-1%, and the content of the cobalt oxide is 1%-14%.

2. The method according to claim 1, characterized in that The first catalyst includes a first carrier and a first active component. Based on the total mass of the first catalyst being 100%, the content of the first carrier is 80-99%; and the content of the first active component is 1-15%.

3. The method according to claim 2, characterized in that The first carrier comprises one or a combination of two or more of titanium oxide, aluminum oxide, cerium oxide, zirconium oxide, tin oxide and silicon oxide; and / or The first active component includes one or a combination of two or more of vanadium oxide, iron oxide, copper oxide, tungsten oxide, molybdenum oxide and manganese oxide.

4. The method according to claim 3, characterized in that Based on the total mass of the first catalyst as 100%, in the first carrier, the content of the titanium oxide is 75%-90%, the content of the aluminum oxide is 0%-5%, the content of the cerium oxide is 1%-10%, the content of the zirconium oxide is 0%-5%, the content of the tin oxide is 1%-10%, and the content of the silicon oxide is 0%-5%; and / or Based on the total mass of the first catalyst as 100%, in the first active ingredient, the content of the vanadium oxide is 1%-3%, the content of the iron oxide is 0%-5%, the content of the copper oxide is 0%-1%, the content of the tungsten oxide is 0%-5%, the content of the molybdenum oxide is 1%-5%, and the content of the manganese oxide is 1%-5%.

5. The method according to any one of claims 1 to 4, characterized in that: The first catalyst further contains sulfate ions; based on the total mass of the first catalyst being 100%, the content of the sulfate ions is 1.5-3% in terms of SO3; and / or The first catalyst further contains phosphate ions. Based on the total mass of the first catalyst being 100%, the content of the phosphate ions is less than 5% in terms of P2O5.

6. The method according to any one of claims 1 to 4, characterized in that: The second carrier further comprises one or a combination of two or more of aluminum oxide, zirconium oxide and silicon oxide; and / or The second active component further comprises one or a combination of two or more of platinum oxide, gold oxide, vanadium oxide, iron oxide, copper oxide, molybdenum oxide and manganese oxide.

7. The method according to claim 6, characterized in that Based on the total mass of the second catalyst as 100%, in the second carrier, the content of the aluminum oxide is 0%-5%, the content of the zirconium oxide is 0%-5%, and the content of the silicon oxide is 0%-5%; and / or Based on the total mass of the second catalyst as 100%, in the second active component, the content of the platinum oxide is 0%-1%, the content of the gold oxide is 0%-1%, the content of the vanadium oxide is 0%-5%, the content of the iron oxide is 0%-1%, the content of the copper oxide is 0%-5%, the content of the molybdenum oxide is 0%-5%, and the content of the manganese oxide is 0%-10%.

8. The method according to any one of claims 1 to 4, characterized in that: The second catalyst further contains phosphate ions. Based on the total mass of the second catalyst being 100%, the content of the phosphate ions is less than 5% in terms of P2O5.

9. The method according to any one of claims 1 to 4, characterized in that: The preparation method of the first catalyst comprises the following steps: dissolving a precursor of a first carrier in a solvent to obtain a first carrier precursor solution; The first carrier precursor solution is mixed with an alkaline precipitant and then dried to obtain a first carrier dry product; calcining the first carrier dried product to obtain a first carrier; dissolving a precursor of a first active ingredient and a co-solvent in a solvent to obtain a first active ingredient precursor solution; Mixing a first carrier, an optional structural aid and a first active ingredient precursor solution and drying the mixture to obtain a first mixed product; calcining the first mixed product to obtain a first catalyst powder; The first catalyst powder is made into a slurry, and the slurry is extruded or coated onto a substrate to obtain a first catalyst precursor; The first catalyst precursor is dried and then calcined to obtain a first catalyst.

10. The method according to any one of claims 1 to 4, characterized in that: The preparation method of the second catalyst comprises the following steps: dissolving a precursor of a second carrier in a solvent to obtain a second carrier precursor solution; The second carrier precursor solution is mixed with an alkaline precipitant and then dried to obtain a second carrier dry product; calcining the second carrier dried product to obtain a second carrier; dissolving a precursor of a second active ingredient and a co-solvent in a solvent to obtain a second active ingredient precursor solution; Mixing a second carrier, an optional structural aid and a second active ingredient precursor solution and drying the mixture to obtain a second mixed product; calcining the second mixed product to obtain a second catalyst powder; The second catalyst powder is made into slurry, and the slurry is extruded or coated onto a substrate to obtain a second catalyst precursor; The second catalyst precursor is dried and then calcined to obtain a second catalyst.