A phosphorus solid-based road base material and its preparation process

By using raw materials such as phosphogypsum, phosphotail slag, fly ash and nano-silica sol in the road base materials, combined with hard curing agents and water reducing agents, the crack problems in low effective utilization rate and tidal environments are solved, and the cracks in the environment of phosphogypsum are improved. The durability and compressive strength of the road base layer are achieved, and the density and stability of the material are improved.

CN116120022BActive Publication Date: 2024-11-05HUBEI JIUXIA ENTERPRISE MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211628264.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-17
Publication Date
2024-11-05
Estimated Expiration
2042-12-17

AI Technical Summary

Technical Problem

The effective utilization rate of phosphogypsum is low, resulting in waste and pollution of land resources. At the same time, the high content of phosphogypsum will lead to the expansion and strength of the road base material, and it is easy to produce cracks in a tidal environment, affecting the quality and safety of the project.

Method used

The phosphate solid-based road base materials are used, including phosphogypsum, phosphorus tailings slag, fly ash, nanosilica sol and nanoaluminum sol, and the slurry flow and pore structure are improved through the combination of hard curing agent and water reducing agent. Reduce curing shrinkage, improve durability and compressive strength.

Benefits of technology

It effectively improves the durability and compressive strength of the road base layer, reduces the curing shrinkage and porosity, enhances the density and stability of the material, and solves the problems of insufficient road performance and cracks caused by excessive phosphogypsum content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004004532900000081
    Figure BDA0004004532900000081
Patent Text Reader

Abstract

The invention discloses a phosphorus solid-based road base material, which comprises the following raw materials by weight: 80-90 parts of phosphorus solid raw materials, 5-15 parts of powder curing agent, 3-8 parts of powder, 3-8 parts of hard curing agent, 1-4 parts of water reducing agent, and 0.5-1.5 parts of sodium alginate. In addition, a preparation process of the road base material is also disclosed. The road base has a dense structure, high compressive strength and rigidity, strong durability, good adaptability, and improves the working performance and stability of the road base material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of C04B28, and in particular to a phosphorus solid-based road base material and a preparation process thereof. Background Art

[0002] Phosphogypsum is a major solid waste produced in the wet phosphoric acid process. It has a complex composition, including phosphoric acid, calcium sulfate, fluoride and other substances. The effective utilization rate of phosphogypsum in my country is less than 10%, and the general treatment method is simple landfill, which not only causes a huge waste of land resources, but also the organic matter such as fluorine and phosphorus contained in it will pollute groundwater and destroy soil resources. In addition, phosphogypsum may also produce sulfur dioxide and other substances that are harmful to people's health and life under certain conditions. Therefore, achieving effective utilization of phosphogypsum is an urgent problem to be solved.

[0003] CN104961421A discloses a red mud phosphogypsum hydraulic road base material and a preparation process thereof. The raw materials include phosphogypsum, red mud, ordinary silica cement, and a hydraulic curing agent. The red mud and phosphogypsum are used to produce the road base material, turning waste into treasure. However, the overall dosage of phosphogypsum is small, and the dosage of phosphogypsum is limited. If the content of phosphogypsum is too high, the mixture will expand, the strength will be reduced or even lost, resulting in insufficient road performance. At the same time, in a humid air environment, the existing road base will infiltrate internally and exchange moisture with the air under the action of the humidity gradient, resulting in an increase in the porosity of the road base, which is prone to cracks, affecting the stability of the surface layer, reducing the strength of the components, and affecting the quality and safety of the project. Summary of the invention

[0004] To solve the above problems, the present invention provides a phosphorus solid-based road base material, which includes the following preparation raw materials, by weight: 80-90 parts of phosphorus solid raw materials, 5-15 parts of powder curing agent, 3-8 parts of powder, 3-8 parts of hard curing agent, 1-4 parts of water reducing agent, and 0.5-1.5 parts of sodium alginate.

[0005] A preferred solution is 82 parts of phosphorus solid raw material, 10 parts of powder curing agent, 6 parts of powder, 5 parts of hard curing agent, 2 parts of water reducing agent, and 1 part of sodium alginate.

[0006] Furthermore, the solid phosphorus raw materials include phosphogypsum and phosphorus tailings.

[0007] Furthermore, the mass ratio of the phosphogypsum to the phosphorus tailings is (60-80):(10-20).

[0008] In a preferred embodiment, the mass ratio of the phosphogypsum to the phosphorus tailings is 70:12.

[0009] Furthermore, the powder curing agent is silicate cement or aluminate cement.

[0010] Furthermore, the powder curing agent is silicate cement.

[0011] Furthermore, the silicate cement is one or more of PO 42.5, PO 42.5R, PO 52.5, and PO 52.5R.

[0012] In a preferred embodiment, the silicate cement is PO 42.5.

[0013] Furthermore, the powder is selected from fly ash or mineral powder.

[0014] Preferably, the powder is fly ash.

[0015] Furthermore, the fly ash includes fly ash hollow microspheres, thermal power plant fly ash

[0016] Furthermore, the mass ratio of the fly ash hollow microspheres to the fly ash from a thermal power plant is (1-3):(3-5).

[0017] In a preferred embodiment, the mass ratio of the fly ash hollow microspheres to the fly ash from a thermal power plant is 1.5:4.

[0018] Based on the system of the present invention, a large amount of phosphogypsum and phosphate ore tailings are used in the preparation of road base. The use of a hard curing agent can effectively shorten the gel time of the slurry. Due to the large amount of solid phosphorus raw materials, the fluidity of the slurry is reduced, and gaps are inevitably present between the raw materials. The inventors found in the process of exploration that by introducing a powder curing agent and fly ash in a mass ratio of (8-15): (5-8), especially when the fly ash includes hollow fly ash microbeads and fly ash from a thermal power plant in a mass ratio of (1-3): (3-5), the fluidity of the slurry can be effectively improved, filled in the gaps in the road base material, and the curing shrinkage rate can be reduced. The durability of the subsequent road base is effectively improved, and the density of the road base structure is increased. The inventor speculates that the reason may be that the introduction of a certain amount of fly ash hollow microspheres and fly ash from thermal power plants, on the one hand, improves the fluidity of the road base slurry, and to a certain extent offsets the adverse effect of the introduction of hard curing agent on the fluidity of the road base slurry; on the other hand, the active ingredients in the fly ash hollow microspheres and fly ash from thermal power plants react chemically with the calcium hydroxide in the road base material, filling the voids in the materials, compensating for the volume shrinkage of the road base due to temperature stress during subsequent processing of the road base material, reducing the curing shrinkage rate, optimizing the pore structure of the road base, increasing the density of the road base structure, and effectively improving the durability of the subsequent road base.

[0019] Calculated by mass percentage, the raw materials for preparing the hard curing agent include: 20-30% of sol A, 0.01-2% of sol B, and the balance of water.

[0020] Furthermore, the raw materials for preparing the hard curing agent are: 24.2% of sol A, 0.82% of sol B, and the balance of water.

[0021] The sol A is selected from one or more of nano-silica sol, nano-aluminum sol, nano-zirconium oxide sol, nano-titanium sol, nano-zinc oxide sol, and nano-carbon sol.

[0022] Furthermore, the sol A is nano silica sol.

[0023] The sol B is selected from one or more of nano-silica sol, nano-aluminum sol, nano-zirconia sol, nano-titanium sol, nano-zinc oxide sol, and nano-carbon sol.

[0024] Furthermore, the sol B is nano aluminum sol.

[0025] Furthermore, the particle size of the nano silica sol is 8-20 nm, and the particle size of the nano alumina sol is 10-15 nm.

[0026] Furthermore, the nano-silica sol is organically modified nano-silica sol.

[0027] Furthermore, the organically modified nano-silica sol is an alkyl-modified nano-silica sol.

[0028] Based on the system of the present invention, a nanoparticle aqueous solution containing nano-silica sol and nano-aluminum sol is used as a hard curing agent for phosphogypsum in the system, and a colloidal chemical reaction occurs with the phosphorus solid raw material in the system under the action of compaction work to form a stably consolidated road base, effectively solving the problem of insufficient road performance caused by expansion of road base materials, reduced strength or even loss of strength due to excessively high phosphogypsum content. The inventors found during the research process that by controlling the particle size of nano-silica sol to 8-20nm and the particle size of nano-alumina sol to 10-15nm, the induction period of cement hydration can be accelerated, more binding sites are provided for the gel, and the hydration of cement in the system is effectively promoted; in addition, due to the influence of the surface groups of the nano-silica sol, it has a strong surface activity in the system and is easy to agglomerate, which reduces the activity of the nano-silica sol. The inventors found during the research process that by introducing organically modified nano-silica sol, especially when the organically modified nano-silica sol is an alkyl-modified nano-silica sol, it is compatible with the alkaline environment of the system and is not easy to agglomerate, so that the nano-silica sol and nano-alumina sol in the system penetrate into the pore structure of the road base material, react with the calcium hydroxide in the road base material, reduce the total porosity and capillary porosity of the road base material slurry, and improve the compressive strength, chloride ion permeability and durability of the road base.

[0029] Furthermore, the water reducer is selected from at least one of aminosulfonate water reducers, polycarboxylic acid water reducers, melamine water reducers, aliphatic high-efficiency water reducers, and naphthalene water reducers.

[0030] Furthermore, the water reducer is a combination of a polycarboxylic acid-based high-efficiency water reducer and a naphthalene-based water reducer.

[0031] Furthermore, the mass ratio of the polycarboxylic acid-based high-efficiency water reducer to the naphthalene-based water reducer is (0.5-1):(1.8-3).

[0032] In a preferred embodiment, the mass ratio of the polycarboxylic acid-based high-efficiency water reducer to the naphthalene-based water reducer is 0.8:2.5.

[0033] The inventors found in the process of exploration that based on the system of the present invention, by introducing a polycarboxylic acid-based high-efficiency water reducer and a naphthalene-based water reducer in a mass ratio of (0.5-1): (1.8-3), the mechanical properties of the road base are minimally affected, and good matching adaptability is achieved with the phosphorus solid raw material and silicate cement in the system, and the synergistic effect can be maximized. On the one hand, the nano-silica sol and nano-aluminum sol in the system are encapsulated to achieve good dispersion of the nano-active particles in the system. On the other hand, they are adsorbed on the surface of the phosphorus solid raw material and the powder curing agent silicate cement particles, which helps to disperse the silicate cement, increase the fluidity of the road base slurry, and improve the working performance and stability.

[0034] As a preferred technical solution, the mass ratio of the fly ash, hardening agent and water reducing agent is (3-8): (3-8): (1-4).

[0035] Road base materials are widely used in the preparation of road bases in various regions. In the low-temperature and humid southwest region, the humid air environment increases the internal percolation of the road base, and the water exchange with the air under the action of the humidity gradient causes the porosity of the road base to increase, which is easy to produce cracks, affecting the stability of the surface layer, reducing the strength of the components, and affecting the quality and safety of the project. Based on the system of the present invention, under the joint action of fly ash, hard curing agent, and water reducing agent, the microstructure of the road base formed in the later stage is more compact, and the interface transition zone between phosphogypsum, phosphorus tailings and cement is effectively improved, and the rigidity of the road base is effectively improved. By introducing specific fly ash, hardening agent and water reducing agent, and controlling the mass ratio of the fly ash, hardening agent and water reducing agent to be (3-8): (3-8): (1-4), the water reducing agent wraps the nano-silica sol and nano-alumina sol, thereby avoiding the problem of incomplete hydration of cement due to the agglomeration of nano-silica sol and nano-alumina sol in the hardening agent. The nano-silica sol and nano-alumina sol consume the alkaline substances of efflorescence from the source to form a gel to play a filling and bonding effect, thereby reducing the internal pore diameter and the total number of pores of the road base, and reducing the transmission channels of alkali and salt substances in the road base material from the inside of the road base to the surface accumulation, thereby ensuring the stability and construction strength of the road base and solving the problem of slow early strength development of the road base due to the introduction of fly ash.

[0036] A preparation process of a phosphorus solid-based road base material comprises the following steps:

[0037] (1) 80-90 parts by mass of solid phosphorus raw material, 5-15 parts of powder curing agent, 3-8 parts of powder, and 0.5-1.5 parts of sodium alginate are mixed and stirred to obtain a mixture A;

[0038] (2) By mass percentage, 20-30% of sol A, 0.01-2% of sol B, and water are mixed and stirred to obtain a hard curing agent;

[0039] (3) According to weight, mix the mixture A, 3-8 parts of hardening curing agent and 1-4 parts of water reducing agent and stir until uniformly mixed.

[0040] A preferred solution is a process for preparing a phosphorus solid-based road base material, comprising the following steps:

[0041] (1) 82 parts by mass of solid phosphorus raw material, 10 parts by mass of powder curing agent, 6 parts by mass of powder material, and 1 part by mass of sodium alginate were mixed and stirred to obtain a mixture A;

[0042] (2) According to mass percentage, 24.2% of sol A, 0.82% of sol B and water are mixed and stirred to obtain a hard curing agent;

[0043] (3) Mix the mixture A, 5 parts of hardening agent and 2 parts of water reducing agent by weight and stir until uniformly mixed.

[0044] Beneficial effects:

[0045] 1. The present invention adopts nanoparticle aqueous solution of nano-silica sol and nano-aluminum sol as a hardening agent for phosphogypsum in the system, which forms a stably consolidated road base with the phosphorus solid raw material in the system, and at the same time promotes the hydration of cement in the system, penetrates into the pore structure of the road base material, and improves the compressive strength of the road base.

[0046] 2. The present invention introduces fly ash hollow microspheres and fly ash from thermal power plants in a mass ratio of (1-3): (3-5) and fills them into the voids of the road base material to improve the fluidity of the slurry, reduce the curing shrinkage, effectively improve the durability of the subsequent road base, and increase the density of the road base structure.

[0047] 3. The present invention introduces a polycarboxylic acid-based high-efficiency water reducer and a naphthalene-based water reducer in a mass ratio of (0.5-1): (1.8-3), which have good adaptability with the phosphorus solid raw materials and silicate cement in the system, thereby improving the working performance and stability of the road base slurry.

[0048] 4. Under the joint action of fly ash, hardening curing agent and water reducing agent, the road base material of the present invention forms a denser microstructure of the road base in the later stage, effectively improves the interface transition zone between phosphogypsum, phosphorus tailings and cement, and effectively improves the stiffness of the road base. DETAILED DESCRIPTION

[0049] Example 1

[0050] Embodiment 1 of the present invention provides a phosphorus solid-based road base material, which includes the following raw materials by mass: 90 parts of phosphorus solid raw materials, 12 parts of PO 42.5 silicate cement, 5 parts of fly ash, 0.5 parts of sodium alginate, 1 part of water reducer, and 6 parts of hard curing agent.

[0051] The phosphorus solid raw material includes phosphogypsum and phosphorus tailings in a mass ratio of 80:10.

[0052] The fly ash includes fly ash hollow microbeads and fly ash from thermal power plants, with a mass ratio of 1:3.

[0053] The water reducer comprises a polycarboxylic acid-based high-efficiency water reducer and a naphthalene-based water reducer, with a mass ratio of 0.5:3.

[0054] The organic modified nano silica sol was purchased from Jinan Yinfeng Silicon Products Co., Ltd., model SC-201.

[0055] The nano aluminum sol was purchased from Beijing Dekedaojin Technology Co., Ltd., model number is DK-Al-SL.

[0056] The polycarboxylic acid-based high-efficiency water reducer was purchased from Yupande International Trading Co., Ltd., model HR-01.

[0057] The naphthalene-based water reducer was purchased from Jinan Sunny Chemical Technology Co., Ltd., model FDN-A.

[0058] Embodiment 1 of the present invention provides, on the other hand, a process for preparing a phosphorus solid-based road base material, comprising the following steps:

[0059] (1) According to parts by mass, 90 parts of solid phosphorus raw material, 12 parts of PO 42.5 silicate cement, 5 parts of fly ash, and 0.5 parts of sodium alginate were mixed and stirred to obtain a mixture A;

[0060] (2) According to the mass percentage, 20% of alkyl-modified nano-silica sol, 0.01% of nano-aluminum sol and water are mixed and stirred to obtain a hard curing agent;

[0061] (3) According to weight, the mixture A, 6 parts of hardening curing agent and 1 part of water reducing agent are stirred and mixed uniformly.

[0062] Example 2

[0063] On the one hand, Example 2 of the present invention provides a phosphorus solid-based road base material, which includes the following raw materials by mass: 80 parts of phosphorus solid raw materials, 5 parts of PO 42.5 silicate cement, 8 parts of fly ash, 1.5 parts of sodium alginate, 4 parts of water reducer, and 3 parts of hard curing agent.

[0064] The phosphorus solid raw material includes phosphogypsum and phosphorus tailings in a mass ratio of 60:20.

[0065] The fly ash includes fly ash hollow microbeads and fly ash from thermal power plants, with a mass ratio of 3:5.

[0066] The water reducer comprises a polycarboxylic acid-based high-efficiency water reducer and a naphthalene-based water reducer, with a mass ratio of 1:1.8.

[0067] The organic modified nano silica sol was purchased from Jinan Yinfeng Silicon Products Co., Ltd., model SC-201.

[0068] The nano aluminum sol was purchased from Beijing Dekedaojin Technology Co., Ltd., model number is DK-Al-SL.

[0069] The polycarboxylic acid-based high-efficiency water reducer was purchased from Yupande International Trading Co., Ltd., model HR-01.

[0070] The naphthalene-based water reducer was purchased from Jinan Sunny Chemical Technology Co., Ltd., model FDN-A.

[0071] Embodiment 2 of the present invention provides, on the other hand, a process for preparing a phosphorus solid-based road base material, comprising the following steps:

[0072] (1) 80 parts by mass of solid phosphorus raw material, 5 parts of PO 42.5 silicate cement, 8 parts of fly ash, and 1.5 parts of sodium alginate were mixed and stirred to obtain a mixture A;

[0073] (2) According to the mass percentage, 30% of alkyl-modified nano-silica sol, 2% of nano-aluminum sol and water are mixed and stirred to obtain a hard curing agent;

[0074] (3) According to weight, the mixture A, 3 parts of hardening curing agent and 4 parts of water reducing agent are stirred and mixed uniformly.

[0075] Example 3

[0076] On the one hand, Example 3 of the present invention provides a phosphorus solid-based road base material, which includes the following raw materials by mass: 82 parts of phosphorus solid raw materials, 10 parts of PO 42.5 silicate cement, 6 parts of fly ash, 1 part of sodium alginate, 2 parts of water reducer, and 5 parts of hard curing agent.

[0077] The phosphorus solid raw material includes phosphogypsum and phosphorus tailings in a mass ratio of 70:12.

[0078] The fly ash includes fly ash hollow microspheres and fly ash from thermal power plants, with a mass ratio of 1.5:4.

[0079] The water reducer comprises a polycarboxylic acid-based high-efficiency water reducer and a naphthalene-based water reducer, with a mass ratio of 0.8:2.5.

[0080] The organic modified nano silica sol was purchased from Jinan Yinfeng Silicon Products Co., Ltd., model SC-201.

[0081] The nano aluminum sol was purchased from Beijing Dekedaojin Technology Co., Ltd., model number is DK-Al-SL.

[0082] The polycarboxylic acid-based high-efficiency water reducer was purchased from Yupande International Trading Co., Ltd., model HR-01.

[0083] The naphthalene-based water reducer was purchased from Jinan Sunny Chemical Technology Co., Ltd., model FDN-A.

[0084] Embodiment 3 of the present invention provides, on the other hand, a process for preparing a phosphorus solid-based road base material, comprising the following steps:

[0085] (1) 82 parts by mass of solid phosphorus raw material, 10 parts by mass of PO 42.5 silicate cement, 6 parts by mass of fly ash, and 1 part by mass of sodium alginate were mixed and stirred to obtain a mixture A;

[0086] (2) According to the mass percentage, 24.2% of alkyl-modified nano-silica sol, 0.82% of nano-aluminum sol and water are mixed and stirred to obtain a hard curing agent;

[0087] (3) According to weight, the mixture A, 5 parts of hardening curing agent and 2 parts of water reducing agent are stirred and mixed uniformly.

[0088] Comparative Example 1

[0089] Take 24.2% of ammonium nano-silica sol, 0.82% of nano-aluminum sol and water, mix and stir evenly to obtain a hard curing agent, and the rest is the same as in Example 3.

[0090] The ammonium nano-silica sol was purchased from Zhejiang Delixin Micro-Nano Technology Co., Ltd., model JA10-25 / 1.

[0091] Comparative Example 2

[0092] The fly ash includes fly ash hollow microbeads and fly ash from thermal power plants, with a mass ratio of 3:1, and the rest is the same as in Example 3.

[0093] Comparative Example 3

[0094] The mass ratio of the polycarboxylic acid-based high-efficiency water reducer to the naphthalene-based water reducer is 2:1, and the rest is the same as in Example 3.

[0095] Comparative Example 4

[0096] The mass ratio of fly ash, hardening agent and water reducing agent is 9:9:4, and the rest is the same as in Example 3.

[0097] Performance Testing

[0098] 1. According to the test method of "Test Code for Inorganic Binder Stabilized Materials for Highway Engineering" (JTGE51-2009), the above-mentioned base materials are subjected to unconfined compression, splitting and flexural tensile strength tests.

[0099] The quick-curing road base material was mixed with water to obtain a slurry with a moisture content of 15%, which was spread and rolled on the road surface and kept moisturized for 3 days to form a solidified and stable road base. After that, unconfined compression test, splitting strength test and flexural tensile strength test were carried out, and the test results were filled in the following table:

[0100]

[0101] 2. According to the test method of "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering" (JTGE51-2009), the water permeability performance of the above-mentioned base materials was tested. The test used 200mm*200mm cylindrical specimens. Among them, the initial water volume of the water seepage test was 2000mL, and the water seepage time was 24h. The sample evaluation indicators are: A: water seepage is less than 10mL; B: water seepage is greater than 10mL and less than 50mL; C: water seepage is greater than 50mL.

[0102] Water seepage performance evaluation Example 1 A Example 2 A Example 3 A Comparative Example 1 B Comparative Example 2 C Comparative Example 3 C Comparative Example 4 C

[0103] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A phosphorus solid-based road base material, characterized in that: The preparation raw materials include the following by weight: 80-90 parts of phosphorus solid raw materials, 5-15 parts of powder curing agent, 3-8 parts of powder, 3-8 parts of hard curing agent, 1-4 parts of water reducing agent, and 0.5-1.5 parts of sodium alginate; The solid phosphorus raw material includes phosphogypsum and phosphorus tailings; the powder curing agent is silicate cement or aluminate cement; the powder is fly ash; the fly ash includes fly ash hollow microspheres and fly ash from thermal power plants, with a mass ratio of 1.5:4; The mass ratio of the phosphogypsum and phosphorus tailings is (60-80): (10-30); The raw materials for preparing the hard curing agent include, by weight percentage, 20-30% of sol A, 0.01-2% of sol B, and the balance of water; The sol A is an alkyl-modified nano-silica sol, and the solvent B is a nano-aluminum sol; The water reducer is a combination of a polycarboxylic acid-based high-efficiency water reducer and a naphthalene-based water reducer, and the mass ratio of the polycarboxylic acid-based high-efficiency water reducer to the naphthalene-based water reducer is (0.5-1):(1.8-3).

2. The road base material according to claim 1, characterized in that: The powder curing agent is silicate cement.

3. The road base material according to claim 2, characterized in that: The silicate cement is one or more of PO 42.5, PO42.5R, PO 52.5, and PO 52.5R.

4. A process for preparing a phosphorus solid-based road base material according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) By weight, 80-90 parts of solid phosphorus raw material, 5-15 parts of powder curing agent, 3-8 parts of powder material, and 0.5-1.5 parts of sodium alginate are mixed and stirred to obtain a mixture A; (2) By mass percentage, 20-30% of sol A, 0.01-2% of sol B and water are mixed and stirred to obtain a hard curing agent; (3) According to weight, mix the mixture A, 3-8 parts of hardening curing agent and 1-4 parts of water reducing agent evenly.