A super-macroporous hydrogel and its preparation method and application
By adding polyvinyl alcohol to the sodium alginate solution, the super-porous hydrogel is formed by cross-linking reaction, the problem of complex preparation and poor mechanical properties in the prior art is solved, and super-porous water with high porosity and large pore size is achieved The preparation of gel is suitable for a variety of applications in the field of biomedical medicine.
Patent Information
- Application Number
- CN202310030838.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-01-06
AI Technical Summary
The existing ultra-large pore hydrogel preparation methods are complex and have poor mechanical properties, which are difficult to meet the wide application needs in the field of biomedicine.
By adding polyvinyl alcohol to the pre-solution of sodium alginate, an ultra-large pore structure was formed in one step by cross-linking reaction, and the gel was given strong mechanical properties, an ultra-large pore hydrogel with high pore ratio and large pore size was prepared.
It realizes simple and fast ultra-large pore hydrogel preparation, obtains superior mechanical properties and high porosity (about 85%), and is suitable for cell culture, drug delivery and organoid construction.
Smart Images

Figure CN116120619B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of biotechnology, and in particular relates to a super-macroporous hydrogel and a preparation method and application thereof. Background Art
[0002] Ultraporous hydrogels are defined as hydrogels with an internal pore size of more than 1 micron. As a new type of biomedical material, they have been favored by more and more researchers due to their high similarity in structure and composition with many human tissues and organs, especially in the fields of tissue regeneration, drug delivery, and organoid construction. In the field of tissue regeneration, by loading cells, drugs or cytokines, etc., the characteristics of macroporous hydrogels that are highly similar to human tissues and organs in structure and physical properties can provide mechanical support and biochemical signals to cells, inducing cells to better repair damaged tissues and rebuild the structure and function of tissues. In the field of drug delivery, macroporous hydrogels can be applied to the affected area in the form of patches, and the ultra-large pore size is conducive to the rapid release of cells or drug molecules in the affected area, achieving an efficient therapeutic effect. In addition, in the field of organoids, the ultra-large pore structure and biomimetic physical properties provide a suitable environment for cell proliferation and differentiation, making them ideal scaffold materials for organoid construction.
[0003] Currently, the methods commonly used to prepare super-macroporous hydrogels include freeze-drying, template method, and pore-forming agent method. However, the super-macroporous hydrogels prepared by these methods have two main disadvantages. One is that they require complex preparation processes. Too many preparation processes are not conducive to large-scale commercial production. In addition, the mechanical properties are poor. The super-macroporous structure is a structural defect in material mechanics. Under the action of external forces, these super-macroporous structures are more likely to cause material damage. Therefore, improving the preparation method of super-macroporous hydrogels and improving their mechanical properties will help super-macroporous hydrogels to be widely used in the biomedical field in the future.
[0004] The invention with publication number CN112725327A discloses a method for preparing a cell immobilization carrier, the preparation method comprising the following steps: mixing sodium alginate solution and polyvinyl alcohol evenly to obtain a carrier solution; wherein the mass ratio of the sodium alginate to the polyvinyl alcohol is 1:2-10; adding diatomaceous earth to the carrier solution, mixing evenly, squeezing the gel mixture dropwise into a cross-linking solution in a continuously stirred state to solidify to form beads, washing the beads and freezing and cross-linking at a temperature of -25 to -15°C, and obtaining a cell immobilization carrier after thawing. The sodium alginate solution and polyvinyl alcohol can be cross-linked into a gel under the action of a cross-linking agent.
[0005] The invention with publication number CN103040727A provides a method for preparing a drug and protein sustained-release alginate hybrid gel. The preparation method is: firstly prepare calcium alginate hydrogel, then immerse the calcium alginate hydrogel in a certain concentration of trisodium phosphate, diammonium hydrogen phosphate, sodium silicate, sodium carbonate, sodium oxalate and other inorganic salt solutions to swell for a certain time, then immerse the swollen calcium alginate hydrogel in a drug and protein aqueous solution containing a certain concentration of calcium ions for a certain time to crosslink, and obtain a drug and protein sustained-release alginate hybrid gel.
[0006] However, there is no report in the prior art on the preparation of ultra-macroporous hydrogel using sodium alginate and polyvinyl alcohol. Summary of the invention
[0007] In order to solve the problems in the background technology, the present invention proposes a simple method for preparing super-macroporous hydrogel using polyvinyl alcohol. The present invention adds polyvinyl alcohol to a sodium alginate pre-solution, and forms a super-macroporous structure in one step during the gelation process of the sodium alginate induced by the polyvinyl alcohol, and at the same time gives the gel stronger mechanical properties.
[0008] A method for preparing a super-macroporous hydrogel comprises the following steps:
[0009] (1) respectively preparing a sodium alginate solution, a polyvinyl alcohol solution and a calcium chloride solution;
[0010] (2) mixing the sodium alginate solution and the polyvinyl alcohol solution to obtain a polyvinyl alcohol / sodium alginate mixed solution;
[0011] (3) adding a crosslinking agent calcium chloride solution to the polyvinyl alcohol / sodium alginate mixed solution to obtain a super-macroporous hydrogel composed of polyvinyl alcohol and sodium alginate by crosslinking.
[0012] The concentration of the sodium alginate solution is 4wt%, the concentration of the polyvinyl alcohol solution is 10wt%, and the sodium alginate solution and the polyvinyl alcohol solution are mixed in a volume ratio of 1:1.
[0013] Preferably, in step (1), the concentration of the calcium chloride solution is 0.5 M, and the volume ratio of the calcium chloride solution to the polyvinyl alcohol / sodium alginate mixed solution is 3:2.
[0014] Preferably, in step (3), before adding the calcium chloride solution, the bubbles in the polyvinyl alcohol / sodium alginate mixed solution are first removed.
[0015] Preferably, in step (3), the cross-linking process is left to stand for at least 12 hours.
[0016] Preferably, in step (3), after the cross-linking is completed, the obtained supermacroporous hydrogel is soaked in ultrapure water to remove free calcium ions.
[0017] Preferably, the supermacroporous hydrogel has a pore size distribution of 100 to 900 μm.
[0018] The invention also provides a super macroporous hydrogel prepared by the preparation method.
[0019] The present invention also provides the use of the superporous hydrogel in cell culture. During the use, the superporous hydrogel is immersed in a culture medium, and then cells are injected into the pores inside the superporous hydrogel for cell culture.
[0020] The present invention also provides a cell culture method, which uses the superporous hydrogel, immerses the superporous hydrogel in a culture medium, and then injects cells into the pores inside the superporous hydrogel for cell culture.
[0021] The present invention selects sodium alginate as the skeleton material of the gel to provide the material with necessary mechanical properties, and polyvinyl alcohol is added thereto to induce phase separation, forming a high-density phase formed by the aggregation of sodium alginate and a low-density phase formed by polyvinyl alcohol. The high-density phase formed by the close aggregation of cross-linked sodium alginate is the skeleton structure, and the low-density phase containing a large amount of water formed by the free polyvinyl alcohol is the pore structure.
[0022] The present invention obtains a super-macroporous sodium alginate hydrogel with high internal porosity (~85%) and large pore size (100 microns to 900 microns) through a simple and rapid preparation method, and simultaneously obtains excellent mechanical properties. The super-macroporous hydrogel of the present invention can be used for cell culture and is expected to be applied in the fields of tissue engineering, drug delivery, organoid construction, etc.
[0023] When preparing the ultra-macroporous hydrogel in the present invention, it is necessary to use sodium alginate and polyvinyl alcohol at a specific concentration and ratio, otherwise the macroporous pore structure inside the hydrogel cannot be effectively obtained during cross-linking. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The following is the preparation process of the super-macroporous hydrogel in Example 1 and Example 2.
[0025] Figure 2 The cross-sectional view of the supermacroporous hydrogel in Example 1 and the supermacroporous structure observed under a microscope.
[0026] Figure 3 The hydrogels prepared with different ratios of polyvinyl alcohol and sodium alginate in Example 1 and their structures observed under a microscope.
[0027] Figure 4 It is the pore size distribution obtained after statistical analysis of the microscope imaging results in Example 1.
[0028] Figure 5These are the test results of the compression performance test on the super-macroporous hydrogel in Example 2.
[0029] Figure 6 The growth status of cells in the supermacroporous hydrogel under a microscope in Example 3, scale bar 200 μm. DETAILED DESCRIPTION
[0030] Example 1
[0031] (1) Preparation of sodium alginate solution: 8 g of sodium alginate powder was dissolved in 192 g of ultrapure water at room temperature to obtain a 4 wt % sodium alginate solution.
[0032] (2) Preparation of polyvinyl alcohol (PVA) solution: 20 g of PVA powder was dissolved in 90° C. hot water (180 g) with continuous stirring to obtain a 10 wt % PVA solution.
[0033] (3) Preparing a polyvinyl alcohol / sodium alginate mixed solution: The sodium alginate solution and the PVA solution in steps (1) and (2) are blended in a volume ratio of 1:1, and stirred continuously at room temperature until the mixture is uniform and free of steam pockets.
[0034] (4) Preparation of control group solution: The sodium alginate and PVA solutions in steps (1) and (2) were mixed at a volume ratio of 5:1 and 1:5 respectively as the control group ratio.
[0035] (5) Preparation of calcium chloride solution: Weigh 11.1 g of calcium chloride granules, dissolve in 200 ml of ultrapure water, and obtain a 0.5 M calcium chloride solution by ultrasonic treatment.
[0036] (6) Preparing a porous hydrogel in a centrifuge tube: First, take 2 ml of the mixed solution in step (3) and add it to a 5 ml centrifuge tube, then use a centrifuge to remove the bubbles generated during the addition of the solution, and then slowly add the calcium chloride solution in step (5) into the centrifuge tube, so that the calcium chloride solution fills the remaining space in the centrifuge tube.
[0037] (7) Prepare a control group gel in a centrifuge tube: Take 2 ml of the sodium alginate solution in step (1) and the control group solution in step (4), add them to a 5 ml centrifuge tube, and then use a centrifuge to remove the bubbles generated during the addition of the solution. Then slowly add the calcium chloride solution in step (5) into the centrifuge tube, and fill the remaining space in the centrifuge tube with the calcium chloride solution.
[0038] (8) Standing crosslinking: The centrifuge tube samples obtained in step (6) and step (7) are stood at room temperature for 12 hours to allow the calcium chloride solution and sodium alginate to fully crosslink, thereby obtaining a super-macroporous hydrogel composite of polyvinyl alcohol and sodium alginate and a control group gel.
[0039] (9) Removal of free calcium ions: The porous hydrogel and the control group gel in step (8) were taken out and immersed in ultrapure water for 24 hours, with the water changed every 12 hours to obtain the final hydrogel sample. The gels obtained in the end included a super-macroporous hydrogel (abbreviated as 1-1) with a polyvinyl alcohol / sodium alginate mixing ratio of 1:1, a control group gel, a composite gel with a mixing ratio of 5:1 (abbreviated as 5-1) and 1:5 (abbreviated as 1-5), and a hydrogel of pure sodium alginate (abbreviated as Alg).
[0040] (10) Pore size distribution: First, the ultra-large pore gel and the control group gel in step (9) are cut into thin slices of about 1 mm using a cutting machine, and the central area of the sample cross section is observed under an optical microscope. After taking pictures, the pore structure in the microscope photos is statistically analyzed using software.
[0041] (11) Porosity (P) test: The super-macroporous hydrogel (1-1) in step (9) was cut into pieces with a thickness of 3 mm, and then the mass (m1) was weighed. The cut sample was then placed on a paper towel and the gel was squeezed by hand to remove the water inside. After repeated squeezing three times, the mass of the sample was weighed (m2). The porosity can be calculated based on the mass change between the two weighings:
[0042] P=(m1-m2) / m1×100%
[0043] (12) Moisture content test (Q): The super-macroporous hydrogel in step (9) was sliced and weighed to obtain a mass m1, and then placed in an oven at 80°C for 24 hours. After the sample was completely dried, it was weighed to obtain m2. The moisture content of the super-macroporous hydrogel can be calculated by the mass change before and after the sample was dried:
[0044] Q = (m1-m2) / m1×100%.
[0045] Result analysis:
[0046] like Figure 1 As shown in the figure, after polyvinyl alcohol and sodium alginate solution were mixed in a volume ratio of 1:1, the super-macroporous hydrogel prepared in a centrifuge tube was in the shape of a white bullet, and the middle part was cut by a cutting machine to obtain Figure 2 From the cross-sectional view of the disc sample shown, we can see that the outer layer of the gel presents a white and dense structure, while the inner layer presents a loose and hollow structure. Figure 3As shown in the figure, when the volume ratio of polyvinyl alcohol to sodium alginate is 5:1 and 1:5, or when the hydrogel is prepared with pure sodium alginate solution, the super-large pore structure cannot be obtained. When the central area of the super-large pore hydrogel disc sample is observed under an optical microscope, it can be found that the pore size in the central area is distributed in a gradient within the range of 100 to 900 microns. The super-large pore hydrogel prepared by mixing polyvinyl alcohol and sodium alginate solution in a volume ratio of 1:1 was tested, and the pore size was statistically analyzed using the analysis software of the optical microscope. It was further found that, as shown in FIG. Figure 4 As shown in the figure, sample 1 and sample 2 are repeated twice. It can be seen that the pore sizes of most large pores are distributed in the range of 100 to 500 microns, and the pore sizes above 500 microns are concentrated in the middle area. This phenomenon of the pore size being distributed in a gradient manner from large to small inside is related to the way calcium ions penetrate from the outside to the inside to perform cross-linking.
[0047] In addition, in order to determine the porosity of the superporous hydrogel, a cutting machine was used to cut the superporous hydrogel into pieces with a thickness of about 5 mm. The free water in the pores was drained out by repeated squeezing. Based on the mass change before and after the water was drained, it was calculated that the porosity of the superporous hydrogel was about 85%, which is a relatively high level among the reported superporous hydrogels.
[0048] Example 2
[0049] (1) Preparation of sodium alginate solution: 8 g of sodium alginate powder was dissolved in 192 g of ultrapure water at room temperature to obtain a 4 wt % sodium alginate solution.
[0050] (2) Preparation of polyvinyl alcohol (PVA) solution: 20 g of PVA powder was dissolved in 90° C. hot water (180 g) with continuous stirring to obtain a 10 wt % PVA solution.
[0051] (3) Preparing a polyvinyl alcohol / sodium alginate mixed solution: The sodium alginate solution and the PVA solution in steps (1) and (2) are blended in a volume ratio of 1:1, and stirred continuously at room temperature until the mixture is uniform and free of steam pockets.
[0052] (4) Preparation of calcium chloride solution: Weigh 11.1 g of calcium chloride granules, dissolve in 200 ml of ultrapure water, and obtain a 0.5 M calcium chloride solution by ultrasonic treatment.
[0053] (5) Preparing a porous hydrogel in a centrifuge tube: First, take 2 ml of the mixed solution in step (3) and add it to a 5 ml centrifuge tube, then use a centrifuge to remove the bubbles generated during the addition of the solution, and then slowly add the calcium chloride solution in step (4) into the centrifuge tube, and fill the remaining space in the centrifuge tube with the calcium chloride solution.
[0054] (6) Standing crosslinking: The centrifuge tube sample obtained in step (5) is stood at room temperature for 12 hours to allow the calcium chloride solution and sodium alginate to fully crosslink, thereby obtaining a super-macroporous hydrogel composite of polyvinyl alcohol and sodium alginate.
[0055] (7) Removal of free calcium ions: The ultraporous hydrogel prepared in step (6) was taken out and immersed in ultrapure water for 24 hours, with the water being changed every 12 hours to obtain the final macroporous hydrogel sample.
[0056] Result analysis:
[0057] The super-macroporous hydrogel prepared from the centrifuge tube was cut into cylindrical samples with a height of 9 mm and 16 mm by a cutting machine. The compression performance test was carried out at room temperature with a compression rate set at 5 mm / min. The test results are shown in Figure 5 (Two replicates were tested at each height, respectively as sample 1 and sample 2) As shown in the figure, the fracture stress of the 16mm sample can reach more than 6MPa, and the fracture stress of the 9mm sample can reach nearly 1MPa. In addition, the compression modulus of the sample can be calculated by the ratio of stress to strain at 1% compression strain, as shown in Figure 5 As shown in the right figure, the compression modulus of the supermacroporous hydrogels is around 0.3 MPa, which is comparable to the supermacroporous hydrogels reported so far.
[0058] Example 3
[0059] (1) Preparation of sodium alginate solution: 8 g of sodium alginate powder was dissolved in 192 g of ultrapure water at room temperature to obtain a 4 wt % sodium alginate solution.
[0060] (2) Preparation of polyvinyl alcohol (PVA) solution: 20 g of PVA powder was dissolved in 90° C. hot water (180 g) with continuous stirring to obtain a 10 wt % PVA solution.
[0061] (3) Preparing a polyvinyl alcohol / sodium alginate mixed solution: The sodium alginate solution and the PVA solution in steps (1) and (2) are blended in a volume ratio of 1:1, and stirred continuously at room temperature until the mixture is uniform and free of steam pockets.
[0062] (4) Preparation of calcium chloride solution: Weigh 11.1 g of calcium chloride granules, dissolve in 200 ml of ultrapure water, and obtain a 0.5 M calcium chloride solution by ultrasonic treatment.
[0063] (5) Preparing a porous hydrogel in a centrifuge tube: First, take 2 ml of the mixed solution in step (3) and add it to a 5 ml centrifuge tube, then use a centrifuge to remove the bubbles generated during the addition of the solution, and then slowly add the calcium chloride solution in step (4) into the centrifuge tube, and fill the remaining space in the centrifuge tube with the calcium chloride solution.
[0064] (6) Standing crosslinking: The centrifuge tube sample obtained in step (5) is stood at room temperature for 12 hours to allow the calcium chloride solution and sodium alginate to fully crosslink, thereby obtaining a super-macroporous hydrogel composite of polyvinyl alcohol and sodium alginate.
[0065] (7) Removing free calcium ions: The superporous hydrogel in step (6) was taken out and immersed in ultrapure water for 24 hours, with the water being changed every 12 hours to obtain the final superporous hydrogel sample.
[0066] (8) Prepare complete cell culture medium: add 10% fetal bovine serum and 1% penicillin-streptomycin solution to high-glucose DMEM culture medium.
[0067] (9) Culture of KPC mouse pancreatic cancer cells: KPC mouse pancreatic cancer cells were cultured using the complete culture medium prepared in step (8) in a cell culture incubator at 37° C. and 5% CO 2 . The culture medium was changed every day and the cells were passaged every 3 days using trypsin digestion.
[0068] (10) Soaking the gel in culture medium: The ultra-macroporous hydrogel sample obtained in step (7) is first cut into 9 mm high cylinders, sterilized by high pressure, placed in a sterile 48-well plate, and then soaked in the cell culture medium prepared in step (8). After soaking for 12 hours, the gel reaches an equilibrium state.
[0069] (11) Culturing cells in superporous gel: The KPC cells cultured in step (9) were digested with trypsin, fresh culture medium was added, and the cells were resuspended to 2×10 4 / mL, and then use a pipette to inject 1mL of cell suspension into each superporous hydrogel for culture. Since the pore structure of the superporous hydrogel is interconnected with the outside, the cells injected into the pore structure can continue to obtain nutrients from the culture medium. The replacement of the culture medium is also consistent with the traditional cell culture method, and no special treatment is required.
[0070] (12) Observing cell growth: After culturing the cells in the ultraporous hydrogel for a certain period of time, the growth status of the cells is observed under an optical microscope.
[0071] Result analysis:
[0072] like Figure 6As shown in the figure, after culturing KPC cells in macroporous gel for 24 hours, it was observed under an optical microscope that, unlike the cells that generally adhere to the bottom of the well plate, the cells grown in the super-macroporous hydrogel were spherical and translucent particles, about 20 to 30 microns in size, much smaller than the cells that adhere to the bottom of the well plate. After 48 hours of culture, the cells proliferated inside the macroporous gel and formed obvious cell spheres. These results show that the environment of macroporous gel can effectively support the growth of KPC cells and induce the formation of cell spheres. Compared with cells cultured in commonly used well plates, cells cultured in macroporous gels are more similar to the cell state in real tissues and organs, and are expected to be applied to the establishment of animal cancer models and tissue engineering fields such as organoid construction.
Claims
1. Application of super-macroporous hydrogel in cell culture, characterized in that: When used, the superporous hydrogel is immersed in a culture medium, and then cells are injected into the pores inside the superporous hydrogel for cell culture. The method for preparing the super-macroporous hydrogel comprises the following steps: (1) respectively preparing a sodium alginate solution, a polyvinyl alcohol solution and a calcium chloride solution; (2) mixing the sodium alginate solution and the polyvinyl alcohol solution to obtain a polyvinyl alcohol / sodium alginate mixed solution; (3) adding a crosslinking agent calcium chloride solution to the polyvinyl alcohol / sodium alginate mixed solution to obtain a super-macroporous hydrogel composed of polyvinyl alcohol and sodium alginate by crosslinking. The concentration of the sodium alginate solution is 4wt%, the concentration of the polyvinyl alcohol solution is 10wt%, and the sodium alginate solution and the polyvinyl alcohol solution are mixed in a volume ratio of 1:
1. The super-macroporous hydrogel has a pore size distribution of 100 to 900 μm; In step (1), the concentration of the calcium chloride solution is 0.5 M, and the volume ratio of the calcium chloride solution to the polyvinyl alcohol / sodium alginate mixed solution is 3:2; In step (3), before adding the calcium chloride solution, remove the bubbles in the polyvinyl alcohol / sodium alginate mixed solution; In step (3), the cross-linking process is allowed to stand for at least 12 hours; In step (3), after the cross-linking is completed, the obtained supermacroporous hydrogel is soaked in ultrapure water to remove free calcium ions.
2. A cell culture method, characterized in that: Using a superporous hydrogel, the superporous hydrogel is immersed in a culture medium, and then cells are injected into the pores inside the superporous hydrogel for cell culture. The method for preparing the super-macroporous hydrogel comprises the following steps: (1) respectively preparing a sodium alginate solution, a polyvinyl alcohol solution and a calcium chloride solution; (2) mixing the sodium alginate solution and the polyvinyl alcohol solution to obtain a polyvinyl alcohol / sodium alginate mixed solution; (3) adding a crosslinking agent calcium chloride solution to the polyvinyl alcohol / sodium alginate mixed solution to obtain a super-macroporous hydrogel composed of polyvinyl alcohol and sodium alginate by crosslinking. The concentration of the sodium alginate solution is 4wt%, the concentration of the polyvinyl alcohol solution is 10wt%, and the sodium alginate solution and the polyvinyl alcohol solution are mixed in a volume ratio of 1:
1. The super-macroporous hydrogel has a pore size distribution of 100 to 900 μm; In step (1), the concentration of the calcium chloride solution is 0.5 M, and the volume ratio of the calcium chloride solution to the polyvinyl alcohol / sodium alginate mixed solution is 3:2; In step (3), before adding the calcium chloride solution, remove the bubbles in the polyvinyl alcohol / sodium alginate mixed solution; In step (3), the cross-linking process is allowed to stand for at least 12 hours; In step (3), after the cross-linking is completed, the obtained supermacroporous hydrogel is soaked in ultrapure water to remove free calcium ions.
Citation Information
Patent Citations
Preparation method of drug and protein sustained-release alginate hybrid gel
CN103040727A
Preparation method and application of cell immobilization carrier
CN112725327A
Double-crosslinked sodium alginate hydrogel and preparation method and application thereof
CN105713106A
Alginate-polyvinyl alcohol nano composite dual-network gel and preparation method thereof
CN107189090A
Self-healing polyvinyl alcohol-alginate double-network gel and preparation method thereof
CN107254056A