A long-acting anti-settling fracturing proppant and its preparation method and application
By using a combination of hard material particle core and polyether thiourea coating layer in fracturing proppants, a long-acting anti-settlement fracturing proppants are formed, which solves the problem of hydraulic crack narrowing caused by premature failure of the proppants. The high yield time of shale gas wells has been extended and the yield has been increased.
Patent Information
- Application Number
- CN202211662124.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-12-23
AI Technical Summary
The prior art is difficult to effectively prevent premature failure of fracturing proppants, resulting in narrowing of hydraulic fractures and reducing the yield of shale gas wells.
Long-acting anti-settlement fracturing proppant using a coated layer composed of a hard material and a compressed soluble material. The core is made of ceramic, quartz sand or resin sand material. The coated layer is made of polyether sulfur urea Preparation of materials is carried out by bonding to each other under a downhole temperature and pressure environment to form a pore network to maintain flow diversion capability.
It extends the high yield time of shale gas wells, maintains the diversion capacity of hydraulic fractures, prevents proppant subsidence, and improves the long-term output of shale gas wells.
Smart Images

Figure BDA0004014445510000021 
Figure BDA0004014445510000061 
Figure FDA0004830280160000011
Abstract
Description
Technical Field
[0001] The present invention relates to the field of petroleum exploitation, and in particular to a long-acting anti-settling fracturing proppant and a preparation method and application thereof. Background Art
[0002] Since the matrix permeability of unconventional oil and gas reservoirs such as shale gas, shale oil and tight sandstone is extremely low, in order to obtain industrial exploitation, it is necessary to carry out hydraulic fracturing and other measures on the unconventional oil and gas reservoirs to produce hydraulic fractures, and fill them with proppants to avoid the closure of hydraulic fractures due to formation closure stress, thereby increasing oil and gas flow channels and improving oil and gas production.
[0003] However, the large amount of slickwater fracturing fluid used in the hydraulic fracturing process will corrode the reservoir, causing the shale formation to soften. The quartz sand or ceramsite proppants will fall into the hydraulic fracture formation, causing the fractures to narrow and the conductivity to decrease. Shale gas development practice shows that shale gas wells often have high production in the early stages of production. Subsequently, the production will decrease rapidly, and eventually it will be maintained at a lower production level. The narrowing of hydraulic fractures caused by proppant failure is considered to be an important reason for the rapid decline in production.
[0004] How to prevent the premature failure of proppants, maintain the conductivity of hydraulic fractures, and extend the high production time of shale gas are issues of concern to shale gas developers. Xiang Degui et al. (2022) proposed a technical solution: by adding a certain proportion of shale enhancer to the fracturing fluid, the wettability of the fracturing fluid to the shale is changed, thereby inhibiting the erosion of the shale by the fracturing fluid. This technical solution can effectively maintain the hardness of shale and prevent the proppant from sinking into the shale in the early stage of shale gas development. However, with the exploitation of shale gas, the shale enhancer will be washed out of the shale formation by the fracturing fluid return fluid and the original formation water, gradually losing the enhancement effect, and unable to maintain the conductivity of the hydraulic fracture for a long time. Summary of the invention
[0005] One object of the present invention is to provide a long-lasting anti-settling fracturing proppant;
[0006] Another object of the present invention is to provide a method for preparing the long-acting anti-settling fracturing proppant.
[0007] Another object of the present invention is to provide a shale fracturing method.
[0008] To achieve the above-mentioned purpose, on the one hand, the present invention provides a long-lasting anti-settling fracturing proppant, wherein the fracturing proppant comprises a particle core and a coating layer coated outside the core; the core is mainly composed of a hard material, and the coating layer is mainly composed of a pressure-soluble material.
[0009] The fracturing proppant of the present invention is a long-acting anti-sinking shale fracturing proppant.
[0010] The fracturing proppant of the present invention is particularly suitable for fracturing construction of unconventional oil and gas reservoirs.
[0011] The unconventional oil and gas reservoirs include shale reservoirs, tight sandstone reservoirs, etc.
[0012] According to some specific embodiments of the present invention, the core is spherical or nearly spherical.
[0013] According to some specific embodiments of the present invention, the hard material is selected from a combination of one or more of ceramsite materials, quartz sand materials and resin sand materials.
[0014] The proppant particle core of the present invention is used to bear the closing stress applied by the artificial fracture to the proppant particles, keep the proppant particles from breaking and deforming, form a pore network in the supported artificial fracture, and maintain the conductivity of the artificial fracture.
[0015] Pressure-soluble materials are also called dissolution creep materials. Pressure-soluble materials that are separated from each other maintain a certain stress through contact.
[0016] According to some specific embodiments of the present invention, the critical pressure of pressure dissolution of the pressure-soluble material is not higher than the ground stress.
[0017] According to some specific embodiments of the present invention, the hardness of the pressure-soluble material after pressure dissolution and hardening is greater than the hardness of the shale after softening.
[0018] According to some specific embodiments of the present invention, the pressure-soluble material is selected from polyetherthiourea (PETG) compounds.
[0019] According to some specific embodiments of the present invention, the polyetherthiourea compound is represented by the following formula (I):
[0020]
[0021] Where n is the number of thiourea groups.
[0022] In the present invention, the proppant coating under formation conditions is a large single crystal formed by the combination of countless thiourea groups, and n is the number of thiourea groups interconnected in the large single crystal.
[0023] The proppant particle coating of the present invention is used to bond adjacent proppant particles together under the downhole temperature and pressure environment and stress after the proppant enters the artificial fracture.
[0024] The coating of the proppant particles of the present invention can be tightly coated on the surface of the proppant core without falling off.
[0025] The adjacent proppant particle coatings of the present invention can be pressure-dissolved together under the downhole temperature and pressure environment and stress. The critical pressure for pressure dissolving the proppant particle coatings together should not be higher than the ground stress.
[0026] The hardness of the coating of the proppant particles that are pressure-dissolved together in the present invention should be greater than the hardness of the softened shale.
[0027] According to some specific embodiments of the present invention, the diameter of the core is 50-60 mesh.
[0028] According to some specific embodiments of the present invention, the thickness of the coating layer is 1 / 15-1 / 10 of the core diameter.
[0029] According to some specific embodiments of the present invention, the polyetherthiourea compound is prepared by a method comprising the following steps: using 1,2-bis(2-aminoethoxy)ethane and 1,1'-thiocarbonyldiimidazole as raw materials to prepare the polyetherthiourea coating.
[0030] According to some specific embodiments of the present invention, the molar ratio of 1,2-bis(2-aminoethoxy)ethane to 1,1'-thiocarbonyldiimidazole is (1-10):(1-10).
[0031] According to some specific embodiments of the present invention, the molar ratio of 1,2-bis(2-aminoethoxy)ethane to 1,1'-thiocarbonyldiimidazole is 1:(0.9-1.1).
[0032] According to some specific embodiments of the present invention, the molar ratio of 1,2-bis(2-aminoethoxy)ethane to 1,1'-thiocarbonyldiimidazole is 1:1.
[0033] According to some specific embodiments of the present invention, the reaction of 1,2-bis(2-aminoethoxy)ethane and 1,1'-thiocarbonyldiimidazole is carried out at room temperature.
[0034] According to some specific embodiments of the present invention, the polyetherthiourea compound is prepared by a method comprising the following steps:
[0035] Weigh 155g of 1,2-bis(2-aminoethoxy)ethane and dissolve it in 500mL of dimethylformamide (DMF) solvent. Add 178g of 1,1'-thiocarbonyldiimidazole gradually while stirring. After stirring for 24 hours at room temperature, dilute the reaction mixture with 1L of chloroform, and then pour the diluted reaction mixture into 15L of ether to see the precipitation of a white colloidal precipitate. Pour out the supernatant and add 500mL of chloroform to dissolve the white colloidal precipitate. Transfer the solution to a centrifuge, add 1L of methanol to precipitate the product, separate the product by centrifugation, and then add 500ml of methanol to wash the product. Then leave the product at room temperature for 2 hours to volatilize the residual liquid.
[0036] On the other hand, the present invention also provides a method for preparing the fracturing proppant, wherein the method comprises the following steps:
[0037] (1) a step of preparing a thiourea polymerization monomer using 1,2-bis(2-aminoethoxy)ethane and 1,1'-thiocarbonyldiimidazole as raw materials;
[0038] (2) mixing the obtained thiourea polymerization monomer with a hard material and then performing a polymerization reaction to obtain a mixture of polyether thiourea and the hard material;
[0039] (3) cooling the obtained mixture until it is completely solidified and then crushing it into particles;
[0040] (4) ball milling the obtained particles;
[0041] (5) Screening the ball-milled particles to obtain the fracturing proppant.
[0042] According to some specific embodiments of the present invention, the method further comprises repeating steps (3) to (5) with the particles obtained in step (5) that do not meet the particle size requirements until the particle size meets the particle size requirements.
[0043] According to some specific embodiments of the present invention, in step (2), the mass ratio of the thiourea polymerization monomer to the hard material is 1:(5-6).
[0044] According to some specific embodiments of the present invention, step (1) comprises reacting 1,2-bis(2-aminoethoxy)ethane and 1,1'-thiocarbonyldiimidazole as raw materials at room temperature for 20-30 hours to obtain a thiourea polymerization monomer.
[0045] According to some specific embodiments of the present invention, step (1) comprises reacting 1,2-bis(2-aminoethoxy)ethane and 1,1'-thiocarbonyldiimidazole as raw materials at room temperature for 24 hours to obtain a thiourea polymerization monomer.
[0046] According to some specific embodiments of the present invention, after the reaction is completed, step (1) further comprises using an ether solvent to precipitate, dissolving the precipitate with a first organic solvent and then precipitating it with an alcohol solvent, and centrifuging to obtain a precipitated product, which is the thiourea polymerization monomer.
[0047] According to some specific embodiments of the present invention, the ether solvent is diethyl ether.
[0048] According to some specific embodiments of the present invention, the alcohol solvent is methanol, ethanol or n-butanol.
[0049] According to some specific embodiments of the present invention, the first organic solvent is dichloromethane or chloroform.
[0050] According to some specific embodiments of the present invention, after the reaction is completed, step (1) further comprises using an ether solvent to precipitate, dissolving the precipitate with a first organic solvent and then precipitating it with an alcohol solvent, centrifuging to obtain a precipitated product, and then washing it with an alcohol solvent to obtain the thiourea polymerization monomer.
[0051] According to some specific embodiments of the present invention, step (1) further comprises, after the reaction is completed, diluting the reaction solution with a second organic solvent, then adding an ether solvent to precipitate, dissolving the precipitate with a first organic solvent and then precipitating it with an alcohol solvent, centrifuging to obtain a precipitated product, and then washing it with an alcohol solvent to obtain the thiourea polymerization monomer.
[0052] According to some specific embodiments of the present invention, the second organic solvent is dichloromethane or chloroform.
[0053] According to some specific embodiments of the present invention, step (1) further comprises placing the obtained thiourea polymerization monomer at room temperature for 1.5-2.5 hours to volatilize the residual solvent.
[0054] According to some specific embodiments of the present invention, step (1) further comprises placing the obtained thiourea polymerization monomer at room temperature for 2 hours to volatilize the residual solvent.
[0055] According to some specific embodiments of the present invention, step (1) is carried out using DMF as solvent.
[0056] According to some specific embodiments of the present invention, step (2) is to carry out a polymerization reaction at 130-150° C. to obtain a mixture of polyether thiourea and a hard material.
[0057] According to some specific embodiments of the present invention, step (2) is to carry out a polymerization reaction at 140° C. to obtain a mixture of polyether thiourea and a hard material.
[0058] According to some specific embodiments of the present invention, step (2) is a polymerization reaction for 10-15 hours to obtain a mixture of polyether thiourea and hard material.
[0059] According to some specific embodiments of the present invention, step (2) is a polymerization reaction for 12 hours to obtain a mixture of polyether thiourea and hard material.
[0060] According to some specific embodiments of the present invention, step (2) is to mix the obtained thiourea polymerization monomer with the hard material and then put it into a drying oven to obtain a mixture of polyether thiourea and hard material.
[0061] The polymerization reaction is carried out at 140° C. to obtain a mixture of polyether thiourea and a hard material.
[0062] According to some specific embodiments of the present invention, the method for preparing a fracturing proppant comprises:
[0063] Weigh 155g of 1,2-bis(2-aminoethoxy)ethane and dissolve it in 500mL of dimethylformamide (DMF) solvent. Add 178g of 1,1'-thiocarbonyldiimidazole gradually while stirring. After stirring for 24 hours at room temperature, dilute the reaction mixture with 1L of chloroform, and then pour the diluted reaction mixture into 15L of ether to see the precipitation of a white colloidal precipitate. Pour out the supernatant and add 500mL of chloroform to dissolve the white colloidal precipitate. Transfer the solution to a centrifuge, add 1L of methanol to precipitate the product, separate the product by centrifugation, and then add 500ml of methanol to wash the product. Then leave the product at room temperature for 2 hours to volatilize the residual liquid.
[0064] The product and the hard material core are mixed and stirred evenly, and then placed in a vacuum drying oven and vacuum dried at 140° C. for 12 hours to prepare a hard material core-polyether thiourea mixture.
[0065] The resulting mixture was cooled to room temperature and then broken into particles.
[0066] The obtained particles were ball-milled into a nearly spherical shape.
[0067] The ball-milled particles are sieved to obtain the fracturing proppant.
[0068] In another aspect, the present invention also provides a shale fracturing method, the method comprising first preparing a fracturing fluid containing 1% to 5% by volume of a shale enhancer, and then using no less than 2m 3 / m high-strength sand-added fracturing process is used to lay the long-acting anti-settling fracturing proppant of the present invention.
[0069] The shale enhancer is a soluble high molecular polymer.
[0070] The shale enhancer used in the present invention may be any shale enhancer conventionally available on the market, for example, it may be a shale enhancer produced by China National Petroleum Corporation Engineering Technology Research Institute Co., Ltd.
[0071] For another example, the composition structure of the shale enhancer is as shown below:
[0072]
[0073] Where x and y are the number of polymers linked by Si-O bonds.
[0074] The shale enhancer can change the wettability of the fracturing fluid to prevent the fracturing fluid from entering the shale pores and contacting the shale minerals, thereby delaying the softening of the shale.
[0075] The shale enhancer can be adsorbed on the surface of shale minerals, making the shale hydrophobic and delaying the time for the fracturing fluid to erode the shale.
[0076] The shale enhancer has a stronger polarity than the fracturing fluid.
[0077] In summary, the present invention provides a fracturing proppant and a preparation method and application thereof. The proppant of the present invention has the following advantages:
[0078] When the fracturing proppant is used to carry out fracturing construction, adjacent fracturing proppant particles can be bonded together before the shale softens. The mutually bonded proppant particles can share the compressive stress of a single proppant particle on the shale surface, and even after the shale softens, the critical compressive stress required for shale deformation will not be reached. The effect of preventing the fracturing proppant from sinking is achieved in a "grouping together for warmth". BRIEF DESCRIPTION OF THE DRAWINGS
[0079] Figure 1 This is a schematic diagram of the structure of the fracturing proppant according to Example 1 of the present invention;
[0080] Figure 2 Schematic diagram of the stress exerted on shale by proppant particles of common fracturing fluid;
[0081] Figure 3 It is a schematic diagram of the supporting effect of common fracturing fluid proppant after shale softening;
[0082] Figure 4 A schematic diagram of the fracturing proppant provided by the present invention applying stress to shale;
[0083] Figure 5 It is a schematic diagram of the supporting effect of the fracturing proppant of the present invention after the shale is softened. DETAILED DESCRIPTION
[0084] The implementation process of the present invention and the beneficial effects produced are described in detail below through specific embodiments, which is intended to help readers better understand the essence and characteristics of the present invention, and is not intended to limit the scope of implementation of the present invention.
[0085] Example 1
[0086] (1) This embodiment provides a fracturing proppant having a structure as follows: Figure 1 The proppant particles are divided into two parts: the first part is the particle core of the proppant, which is spherical or nearly spherical and is composed of quartz sand with a particle size of 50-60 mesh (300-250 μm); the second part is the coating layer, which is composed of polyether thiourea materials.
[0087] In this embodiment, the thickness of the coating layer is 1 / 10 of the diameter of the proppant particle core.
[0088] (2) This embodiment also provides a method for preparing the fracturing proppant:
[0089] (a) Weigh 155g of 1,2-bis(2-aminoethoxy)ethane and dissolve it in 500mL of dimethylformamide (DMF) solvent. Add 178g of 1,1'-thiocarbonyldiimidazole gradually while stirring. After stirring for 24h at room temperature, dilute the reaction mixture with 1L of chloroform, and pour the diluted reaction mixture into 15L of ether to see the precipitation of white colloidal precipitate. Pour out the supernatant and add 500mL of chloroform to dissolve the white colloidal precipitate. Transfer the solution to a centrifuge, add 1L of methanol to precipitate the product, separate the product by centrifugation, and then add 500ml of methanol to wash the product. Then place the product at room temperature for 2h to volatilize the residual liquid, mix it with quartz sand in a weight ratio of 1:5, stir it evenly, and send it into a vacuum drying oven. Dry it in vacuum at 140°C for 12 hours to prepare a quartz sand-polyether thiourea mixture.
[0090] (b) The quartz sand-polyether thiourea mixture is taken out and cooled to room temperature and then crushed into particles.
[0091] (c) The crushed quartz sand-polyether thiourea particles are ball-milled into a nearly spherical shape using a ball mill modification machine.
[0092] (d) Using a 40-50 mesh (425-300 μm) vibrating screen, quartz sand-polyetherthiourea particles with a suitable particle size are screened out as a long-term anti-sinking fracturing proppant described in this embodiment.
[0093] (e) The quartz sand-polyether thiourea particles that are not screened out can be recycled and reused to repeat steps (a) to (d) to re-prepare the long-lasting anti-sinking fracturing proppant.
[0094] Test Case
[0095] This test example evaluates the use effect of the fracturing proppant of the present invention. A triaxial stress-pore permeability joint measuring device is used to simulate the mutual bonding process of the fracturing proppant of Example 1 of the present invention under real formation conditions, measure its conductivity, and evaluate its anti-sinking effect. The specific steps include:
[0096] (1) Take a heat shrink tube with an inner diameter of 1.5 cm and a height of about 5 cm, and install a cylindrical metal pad with a diameter of 1.5 cm and a height of 1 cm at the bottom. A small hole is left in the middle of the metal pad for gas to pass through. The middle of the heat shrink tube is filled with a long-acting anti-sinking shale fracturing proppant to a height of about 3 cm. Leave about 0.5 cm on the upper and lower ends of the heat shrink tube for connecting the upper and lower end caps of the triaxial stress-pore permeability joint measurement device.
[0097] (2) Connect the heat shrink tube loaded with the metal pad and the fracturing proppant of Example 1 to the upper and lower end caps of the triaxial stress-pore permeability measurement device, and use a hair dryer to heat the heat shrink tube at the upper and lower end caps to make them fit tightly.
[0098] (3) According to the in-situ stress of the formation to be fractured, a triaxial stress-pore permeability measurement device is used to apply radial and axial stresses of 100 MPa to the heat shrink tube for more than 30 minutes.
[0099] (4) The permeability K1 in the heat shrink tube was measured by the gas permeability method using a triaxial stress-pore permeability measurement device, and the result was 0.55 mD, which can be regarded as the permeability of the fracturing proppant of Example 1 under the ground stress environment. Since K1 is higher than the permeability of the formation to be fractured (10 -3 ~10 -1 mD), indicating that the fracturing proppant of Example 1 can improve the reservoir permeability under the ground stress environment and play a role in fracturing and increasing production.
[0100] (5) The radial and axial stresses are removed, the heat shrink tube is removed from the upper and lower end caps, and the long-term anti-subsidence shale fracturing proppant filled in the heat shrink tube is taken out. It can be observed that the particles of the long-term anti-subsidence shale fracturing proppant are firmly bonded together, and the core of the proppant is not seen to fall off, and there is no overall damage or cracks.
[0101] (6) A long-term anti-sinking shale fracturing proppant bonded together is placed in a new heat shrink tube with an inner diameter of 1.5 cm and a height of about 5 cm, and the bottom is filled with clay with a height of about 1 cm. The clay material or mixture with a Young's modulus (about 10 GPa) similar to that of softened shale in the compacted state is selected. Use a vernier caliper to measure the length L1 from the top of the fracturing proppant of Example 1 filled in the heat shrink tube to the metal pad.
[0102] (7) Connect the heat shrink tube containing the fracturing proppant and clay of Example 1 to the triaxial stress-pore permeability measurement device, and use a hair dryer to heat the heat shrink tube at the upper and lower end caps to make them fit tightly.
[0103] (8) According to the in-situ stress of the formation to be fractured, a triaxial stress-pore permeability measurement device is used to apply radial and axial stresses of 100 MPa to the heat shrink tube for more than 30 minutes.
[0104] (9) Remove radial and axial stresses, remove the heat shrink tube from the upper and lower end caps, and use a vernier caliper to measure the length L2 from the top of the fracturing proppant of Example 1 filled with the heat shrink tube to the clay. The proppant sinking depth L1-L2 is calculated to be 1 mm. This indicates that the fracturing proppant of Example 1 can effectively prevent crack closure caused by proppant sinking in softened shale formations.
[0105] In order to explain the technical principles and advantages of the present invention more clearly, Figure 2 The effect of ordinary fracturing fluid proppant particles on shale stress is shown. Figure 2 As shown, the proppant particles of ordinary fracturing fluids are not bonded to each other, and the compressive stress exerted by a single proppant particle on the shale surface is equivalent to the fracture closure stress.
[0106] Figure 3 The supporting effect of common fracturing fluid proppant after shale softening is demonstrated. Figure 3 As shown, after the shale softens, due to the large compressive stress exerted on the shale surface by the proppant particles of the ordinary fracturing fluid and the lack of connection between the particles, each particle sinks into the softened shale one after another and loses the supporting effect.
[0107] Figure 4 The effect of the fracturing proppant provided by the present invention on the stress of shale is demonstrated. Figure 4 As shown, in the early stage of shale mining, the shale basically maintains its original hardness under the action of the fracturing fluid enhancer, and a closing stress is applied to the long-term anti-subsidence shale fracturing proppant particles provided by the present invention. The coatings of adjacent proppant particles are pressure-dissolved together under the action of the closing stress. Adjacent proppant particles are bonded to each other, sharing the compressive stress of each proppant particle on the shale surface. The compressive stress of each proppant particle on the shale surface is reduced to 1 / n of that of ordinary fracturing fluid proppant particles, where n is the number of proppant particles that are bonded to each other and in contact with the shale surface. The core hardness of the fracturing proppant particles is relatively large, and they do not break or deform, which maintains the support of the proppant skeleton and the conductivity of the artificial fracture.
[0108] Figure 5 The supporting effect of the fracturing proppant of the present invention after shale softening is demonstrated. Figure 5As shown, the compressive stress of each proppant particle on the shale surface is shared by the mutually bonded proppant particles. The compressive stress applied by the fracturing proppant particles of the present invention on the shale surface does not reach the compressive stress required for shale deformation after the shale softens, effectively avoiding the proppant sinking caused by shale softening. The conductivity of the artificial fracture is maintained, and the high yield time of shale gas is extended.
Claims
1. A long-lasting anti-settling fracturing proppant, wherein: The fracturing proppant comprises a particle core and a coating layer coated on the outside of the core; the core is mainly composed of a hard material, and the coating layer is mainly composed of a pressure-soluble material; the thickness of the coating layer is 1 / 15-1 / 10 of the diameter of the core; the critical pressure of the pressure-soluble material for pressure dissolution is not higher than the ground stress; the hardness of the pressure-soluble material after pressure dissolution is greater than the hardness of the softened shale; the pressure-soluble material is selected from the polyether thiourea compound of the following formula (I): Where n is the number of thiourea groups.
2. The long-acting anti-settling fracturing proppant according to claim 1, wherein: The hard material is selected from one or more combinations of ceramsite materials, quartz sand materials and resin sand materials.
3. The long-acting anti-settling fracturing proppant according to claim 1 or 2, wherein: The diameter of the core is 50-60 mesh.
4. The method for preparing the long-acting anti-settling fracturing proppant according to any one of claims 1 to 3, wherein: The method comprises the following steps: (1) a step of preparing a thiourea polymerization monomer using 1,2-bis(2-aminoethoxy)ethane and 1,1'-thiocarbonyldiimidazole as raw materials; (2) mixing the obtained thiourea polymerization monomer with a hard material and then performing a polymerization reaction to obtain a mixture of polyether thiourea and the hard material; (3) a step of crushing the obtained mixture into particles after cooling to room temperature; (4) ball milling the obtained particles; (5) Screening the ball-milled particles to obtain the fracturing proppant.
5. The preparation method according to claim 4, wherein The method further comprises repeating steps (3) to (5) with the particles obtained in step (5) that do not meet the particle size requirements until the particle size meets the particle size requirements.
6. The preparation method according to claim 4, wherein Step (1) comprises taking 1,2-bis(2-aminoethoxy)ethane and 1,1'-thiocarbonyldiimidazole as raw materials and reacting them at room temperature for 20-30 hours to obtain a thiourea polymerization monomer.
7. The preparation method according to claim 6, wherein: After the reaction is completed, step (1) further comprises using an ether solvent to precipitate, dissolving the precipitate with a first organic solvent and then precipitating it with an alcohol solvent, and centrifuging to obtain a precipitated product, which is the thiourea polymerization monomer.
8. The preparation method according to any one of claims 4 to 7, wherein: Step (2) is to carry out polymerization reaction at 130-150° C. to obtain a mixture of polyether thiourea and hard material.
9. A shale fracturing method, wherein: The method comprises first preparing a fracturing fluid containing 1% to 5% by volume of a shale enhancer, and then using no less than 2 m 3 / m high-strength sand fracturing process to lay the long-acting anti-settling fracturing proppant described in any one of claims 1 to 3; the shale enhancer is a soluble high molecular polymer shale enhancer produced by China National Petroleum Corporation Engineering Technology Research Institute Co., Ltd.
Citation Information
Patent Citations
Acrylic acid-acrylamide copolymerization combined expansion material for self-tackifying particles and preparation method of self-tackifying particles
CN112300775A