A preparation method of MoCoB-WCoB based composite material

By using the endogenous WCoB reinforcement phase in MoCoB-based composite materials, the problems of limited hardness improvement and reduced interface strength in the existing technology are solved, and the high hardness and density of MoCoB-WCoB-based composite materials are achieved, maintaining a high Interface bonding strength and surface cleanliness.

CN116121579BActive Publication Date: 2024-10-15XIAN MODERN CHEM RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211489844.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-25
Publication Date
2024-10-15
Estimated Expiration
2042-11-25

AI Technical Summary

Technical Problem

The hardness improvement of existing MoCoB-based composite materials is limited. Adding an external ceramic reinforcement phase will reduce the interface strength and service life, and the reinforcement effect is limited.

Method used

A mixed powder of Mo, Co, B and W powder is used for ball milling and pressing, and MoCoB-WCoB-based composite materials are prepared through vacuum carbon tube furnace sintering to generate endogenous WCoB reinforcement phase, forming MoCoB hard phase, Co bonding phase and Three-phase structure of WCoB reinforcement phase.

Benefits of technology

The hardness and density of MoCoB-WCoB-based composite materials are improved, ensuring high interface bonding strength and no pollution on the surface. The microstructure is dense and the grains are fine, which significantly improves the hardness and density of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116121579B_ABST
    Figure CN116121579B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a MoCoB-WCoB-based composite material. The disclosed method comprises: pressing and molding a mixed powder of Mo, Co, B and W powder after ball milling to obtain a green body, and then sintering the green body in a vacuum carbon tube furnace to prepare a MoCoB-WCoB-based composite material; by mass percentage: the Mo is 34.0% to 46.0%, the Co is 38.0% to 52.0%, the B is 3.0% to 7.0%, and the W is 5.0% to 15.0%. The present invention generates two hard phases, MoCoB and WCoB, by solid phase in-situ reaction during the sintering process. WCoB, as an "endogenous" reinforcing phase, has the advantages of no surface pollution and high interface bonding strength; the prepared MoCoB-WCoB-based composite material has a dense microstructure, fine grains, good density, high hardness and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a MoCoB-WCoB-based composite material, belonging to the field of structural functional materials, and provides a new method for preparing MoCoB-based metal ceramics with a short preparation cycle, stable process and easy industrialization. Background Art

[0002] Ternary boride-based cermets are boride-based composite materials prepared according to the "reaction boriding sintering principle". They have the advantages of high hardness, good wear resistance and corrosion resistance of ceramics and high strength and good plasticity and toughness of metals. They are widely used in the fields of cutting tools, lathe molds, etc. The hard phase in ternary boride-based cermets is not added as a raw material, but is generated by the solid-phase in-situ reaction of the intermediate binary boride and metal. It is an "endogenous" hard phase with no pollution on the surface, avoiding the problem of poor compatibility with the matrix, and has high interface bonding strength. MoCoB-based cermets are a new type of ternary boride-based cermets developed in recent years. They are composed of MoCoB hard phase and Co bonding phase. They have the advantages of high hardness, good wear resistance and strong resistance to high-temperature oxidation. They have great potential in the field of wear-resistant materials.

[0003] The hardness of the MoCoB-based cermets currently prepared is good and can be used as wear-resistant parts for door molds, turning tools, milling cutters, etc. However, with the rapid development of science and technology, high-performance materials emerge in an endless stream, and the performance of materials to be processed is gradually improving. MoCoB-based cermets need to further improve their hardness to maintain market competitiveness. Adding a second phase ceramic to cermets to form a dual-phase ceramic-based composite material can improve its hardness. For example:

[0004] The paper "The Effect of TiB2 Addition on the Microstructure and Properties of MoCoB-based Metal Ceramics" in the journal "Cemented Carbide" studied the effect of adding second phase TiB2 particles on the microstructure and mechanical properties of MoCoB-Co metal ceramics. The results showed that the addition of TiB2 increased the hardness of the composite material, with the maximum hardness reaching 88.9HRA. Although the addition of TiB2 in this prior art study can increase the hardness of the composite material, the TiB2 reinforcement phase is an "external" reinforcement phase, not an "endogenous" reinforcement phase, which will reduce the wettability between the original MoCoB hard phase and the Co bonding phase, causing the interface strength to decrease, affecting its service safety and service life. In addition, the effect of adding TiB2 on improving the hardness of the composite material is relatively limited. Summary of the invention

[0005] In view of the defects or shortcomings of the prior art, the present invention provides a method for preparing a MoCoB-WCoB based composite material.

[0006] To this end, the preparation method provided by the present invention comprises: ball milling and pressing a mixed powder of Mo, Co, B and W powders in sequence to obtain a green body, and then sintering the green body in a vacuum carbon tube furnace to prepare a MoCoB-WCoB based composite material;

[0007] Calculated by mass percentage: the Mo is 34.0% to 46.0%, the Co is 38.0% to 52.0%, the B is 3.0% to 7.0%, and the W is 5.0% to 15.0%.

[0008] Optionally, the sintering process parameters are: raising the temperature from room temperature to 1350-1450° C. at a heating rate of 5-15° C. / min, and keeping the temperature for 0-60 min, and then cooling the furnace to room temperature.

[0009] Furthermore, the MoCoB-WCoB-based composite material contains three phases: a MoCoB hard phase, a Co-based bonding phase, and a WCoB reinforcing phase. The MoCoB-WCoB-based composite material has a hardness of 88.8 to 90.6 HRA and a density of 97.73% to 98.91%.

[0010] Compared with the prior art, ① the composite material generated by the present invention contains three phases: a MoCoB hard phase, a Co-based bonding phase, and a WCoB reinforcing phase; ② the WCoB reinforcing phase in the present invention is not directly added to the raw material, but is generated by a solid-phase in-situ reaction of the raw material powder, and is an "endogenous" reinforcing phase, so it has the advantages of no surface pollution and high interface bonding strength; ③ the prepared MoCoB-WCoB-based composite material has a dense microstructure, fine grains, good density, high hardness, and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 is the XRD pattern of the MoCoB-WCoB based composite material in Example 2 of the present invention;

[0012] Figure 2 This is a microstructure photograph of the MoCoB-WCoB-based composite material in Example 2 of the present invention. DETAILED DESCRIPTION

[0013] Unless otherwise specified, the scientific and technological terms and methods herein are understood according to the knowledge of ordinary technicians in the relevant field or implemented using existing relevant methods. It should also be understood that the temperature and insulation time involved in this article are approximate values ​​for illustrative purposes. Although methods and materials similar or equivalent to the methods and materials described herein can be used for the implementation of the present disclosure, some suitable methods and materials are described below. The publications, patent applications, patents and other references mentioned herein are partially incorporated herein by reference. In the event of a conflict, this article shall prevail. In addition, the materials, methods, material ratios and embodiments are merely exemplary and are not intended to be limiting. In a specific scheme, those skilled in the art can optimize the material ratios and operating parameter values ​​involved in the method according to the disclosure of the present invention using conventional experimental time periods to achieve the purpose of the present invention.

[0014] The purpose of the compression molding of the present invention is to make the powdered raw material preliminarily dense, and the shape and size of the obtained green body depends on the shape of the mold. Existing molds used in the ceramic field, such as molds with a volume size greater than 3mm*3mm, are suitable for the present invention.

[0015] In the process of the present invention, sintering is carried out in a vacuum carbon tube furnace. Based on the disclosure of the present invention, those skilled in the art can use conventional experimental means to optimize the specific sintering for different formula materials and the effects of the present invention. The specific sintering process adopted in the following embodiments is only a specific example to explain the scheme of the present invention, and the sintering process of the present invention is not limited thereto. The sintering process conditions are exemplified by raising the temperature from room temperature to 1350-1450°C at a heating rate of 5-15°C / min, and keeping the temperature for 0-60min, and then cooling the furnace to room temperature.

[0016] The present invention is further described in detail by way of examples. The raw materials Mo, W, Co and B powder used in the examples of the present invention are all commercially available chemically pure powder reagents, and the ball milling adopts a planetary ball mill (QM-3SP4). However, the present invention is not limited to these specific equipments.

[0017] In the present invention, the density of the MoCoB-WCoB-based composite material is tested by the Archimedes drainage method; and the hardness of the MoCoB-WCoB-based composite material is measured by a HRS-150 Rockwell hardness tester.

[0018] Embodiment 1:

[0019] In this embodiment, Mo, Co, B and W powders with a purity of not less than 99.0% are selected as raw materials, and the mass percentages are: Mo is 46.0%, Co is 46%, B is 3.0%, and W is 5.0%;

[0020] The mixed powder is ball-milled and pressed into a cylindrical body (diameter 44 mm, height 8-9 mm);

[0021] The green body was then placed in a vacuum carbon tube furnace for sintering. The sintering process parameters were: the temperature was raised from room temperature to 1350°C at a heating rate of 5°C / min, and kept at that temperature for 0 min, and then the furnace was cooled to room temperature.

[0022] The MoCoB-WCoB-based composite material prepared in this embodiment comprises a MoCoB hard phase, a Co-based bonding phase and a WCoB reinforcement phase, and has a hardness of 89.2 HRA and a density of 97.73%.

[0023] Embodiment 2:

[0024] In this embodiment, Mo, Co, B and W powders with a purity of not less than 99.0% are selected as raw materials, and the mass percentages are: Mo is 40.0%, Co is 45%, B is 5%, and W is 10.0%;

[0025] The mixed powder is ball-milled and pressed into a cylindrical body (diameter 44 mm, height 8-9 mm);

[0026] The green body was then placed in a vacuum carbon tube furnace for sintering. The sintering process parameters were as follows: the temperature was raised from room temperature to 1400°C at a heating rate of 10°C / min, and kept at that temperature for 30 minutes, and then the furnace was cooled to room temperature.

[0027] The MoCoB-WCoB composite material prepared in this example comprises a MoCoB hard phase, a Co-based binder phase and a WCoB reinforcement phase (see XRD pattern). Figure 1 ), microstructure see Figure 2 ; The hardness of the composite material is 90.6HRA and the density is 98.54%.

[0028] Embodiment 3:

[0029] In this embodiment, Mo, Co, B and W powders with a purity of not less than 99.0% are selected as raw materials, and the mass percentages are: Mo is 34.0%, Co is 44.0%, B is 7.0%, and W is 15.0%;

[0030] The mixed powder is ball-milled and pressed into a cylindrical body (diameter 44 mm, height 8-9 mm);

[0031] The green body was then placed in a vacuum carbon tube furnace for sintering. The sintering process parameters were as follows: the temperature was raised from room temperature to 1450°C at a heating rate of 15°C / min, and kept at that temperature for 60 minutes, and then the furnace was cooled to room temperature.

[0032] The MoCoB-WCoB-based composite material prepared in this example comprises a MoCoB hard phase, a Co-based bonding phase and a WCoB reinforcement phase, and has a hardness of 88.8 HRA and a density of 98.91%.

[0033] Comparative Example:

[0034] The quality of this comparative example is different from that of Example 2 in that the raw material does not contain W powder.

[0035] The MoCoB-based cermet obtained in this comparative example comprises a MoCoB hard phase and a Co-based bonding phase, and has a hardness of 87.6 HRA and a density of 97.39%.

[0036] The test properties of the composite materials of the above embodiments and comparative examples are shown in Table 1.

[0037] Table 1 Microstructure and mechanical properties of composite materials

[0038] sample Hardness / HRA Density Comparative Example 87.6 97.39% Example 1 89.2 97.73% Example 2 90.6 98.54% Example 3 88.8 98.91%

[0039] It can be seen from the test results in Table 1 that, compared with the comparative example, the hardness and density of the MoCoB-WCoB-based composite material prepared by the present invention are increased, the density increases by about 1.5%, and the hardness reaches a maximum of 90.6HRA, an increase of 3.0HRA, which is a major breakthrough.

Claims

1. A method for preparing a MoCoB-WCoB based composite material, characterized in that: The preparation method comprises: ball milling and pressing a mixed powder of Mo, Co, B and W powders in sequence to obtain a green body, and then sintering the green body in a vacuum carbon tube furnace to prepare a MoCoB-WCoB-based composite material; By mass percentage: the Mo is 34.0% to 46.0%, the Co is 38.0% to 52.0%, the B is 3.0% to 7.0%, and the W is 5.0% to 15.0%; The sintering process parameters are: raising the temperature from room temperature to 1350-1450°C at a heating rate of 5-15°C / min, and keeping the temperature for 0-60min, and then cooling the furnace to room temperature; The MoCoB-WCoB-based composite material contains three phases: a MoCoB hard phase, a Co-based bonding phase, and a WCoB reinforcing phase.