A high-toughness mining circular saw blade steel plate and its manufacturing method

By optimizing chemical composition and process flow, the problem of easy failure at high temperatures and high cost and environmental protection in the production process is solved, and the saw blade steel plate with high toughness and heat resistance is achieved, reducing production costs and avoiding Quenching cracks and fume pollution.

CN116121644BActive Publication Date: 2024-11-29JIANGYIN XINGCHENG SPECIAL STEEL WORKS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211663161.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-23
Publication Date
2024-11-29
Estimated Expiration
2042-12-23

AI Technical Summary

Technical Problem

Existing mining disc saw blade steel is prone to failure at high temperatures, lacks toughness, and has high cost and environmental protection problems during production. Especially, medium and high carbon saw blade steel is prone to cracks and oil fume pollution during heat treatment.

Method used

Chemical components are C: 0.47-0.52%, Si: 0.40-0.60%, Mn: 1.30-1.50%, V: 0.08-0.12%, Al: 0.03-0.06%, Cr: 0.10-0.30%, Ca: 0.0010- 0.0030% steel plates are directly quenched by low-overheat smelting, continuous casting, hot-sending rolling, slow-cooling quenching and tempering processes to avoid laminar cooling and oil quenching.

Benefits of technology

The high toughness and heat resistance of the steel plate are achieved, the production cost is reduced, the quenching cracks and oil fume pollution is avoided, and the saw blade steel with excellent impact toughness and long service life is produced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004014777500000051
    Figure BDA0004014777500000051
  • Figure BDA0004014777500000052
    Figure BDA0004014777500000052
  • Figure BDA0004014777500000053
    Figure BDA0004014777500000053
Patent Text Reader

Abstract

The invention relates to a high-toughness mining circular saw blade steel plate and a production method thereof. The chemical composition of the steel plate contains, by weight wt%, C: 0.47-0.52%, Si: 0.40-0.60%, Mn: 1.30-1.50%, V: 0.08-0.12%, Al: 0.03-0.06%, Cr: 0.10-0.30%, P: ≤0.012%, S: ≤0.002%, Ca: 0.0010-0.0030%, O: ≤0.002%, N: ≤0.004%, H: ≤0.0002%, and the balance is Fe and inevitable impurity elements. The production process steps are: converter steelmaking -> LF refining -> VD or RH vacuum degassing -> Ca treatment -> continuous casting -> hot delivery -> heating -> rolling -> steel plate slow cooling -> quenching -> tempering. The steel plate of the invention has a thickness of ≤12mm and a width of up to 4000mm, has excellent toughness, an impact Akv of ≥27J at 20°C, and a hardness of 30-40HRC. The saw blade can operate stably within the range of 400-500°C and has a long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of special steel smelting, and particularly relates to a high-toughness mining circular saw blade steel plate and a manufacturing method thereof. Background Art

[0002] Mining circular saw blade steel is mainly used for cutting granite, marble and other stone materials. During the cutting process, the saw blade will vibrate to a certain extent, so the saw blade steel must have high hardness and high wear resistance, as well as excellent toughness to resist impact loads to avoid brittle fractures such as tooth collapse. In addition, the saw blade will generate a lot of heat during high-speed rotation, and the working temperature will rise rapidly, so the saw blade steel must also have a certain degree of heat resistance.

[0003] With the development of my country's steel industry, in recent years, the production and application of domestic saw blade steel have gradually been in line with international standards. Chinese patent CN110284061A discloses a high temperature deformation resistant 75Cr1 saw blade steel and its production method. The invention has a high carbon content of 0.72-0.80%, and is prone to produce needle-shaped martensite after quenching. Although it has high strength and good wear resistance, its toughness is insufficient. The invention is delivered by hot rolling, laminar cooling is adopted, and curling is performed at about 700°C. The hardness of the steel plate is ≤325HB, and it needs to be flattened and oil quenched before subsequent application, which increases the application cost. At the same time, due to the limitations of continuous rolling and curling equipment, large-diameter saw blade steel with a diameter of more than 3000mm cannot be produced.

[0004] Chinese patent CN105063478B discloses a 50Mn2V steel plate for saw blades and its production method. The steel plate is rolled by continuous casting billets for secondary slab opening, and the problem of steel plate flatness is solved by multiple straightening. This invention can only provide hot-rolled semi-finished products, and customers need to perform subsequent heat treatment, which increases the cost of use.

[0005] Chinese patent CN104532150A discloses an ultra-wide saw blade steel and its manufacturing method. The invention adopts a 0.35-0.45% medium carbon design, combined with Nb / V / Ti microalloying, and adds precious metals such as Mo and Ni to increase the toughness of the steel plate. In order to reduce costs, the steel plate is produced by online quenching + offline tempering, but online quenching will cause uneven performance at the head and tail of the steel plate, affecting the service life of the saw blade.

[0006] Chinese patent CN113684421A discloses a method for producing steel for ultra-wide circular saw blades in mines. The steel plate adopts a low-carbon design of 0.17-0.20%, and B element is added to increase the hardenability of the steel plate. The steel plate is quenched at 870℃ and tempered at 250-300℃, and the structure is tempered martensite. This invention adds elements such as Cr / Mo / V, and does not have heat resistance and tempering resistance. When working above 300℃, the hardness of the saw blade will drop sharply, resulting in failure.

[0007] At present, saw blade steel has gradually formed a series of products from high carbon to low carbon. Low carbon steel can be water quenched, which has good toughness, but poor heat resistance and cannot be used at higher temperatures. Medium and high carbon steels have high hardness and good wear resistance, but have problems of poor toughness and easy cracking. At the same time, in order to avoid quenching cracking, medium and high carbon saw blade steel mills generally only make hot-rolled semi-finished products, and customers perform salt bath heating and oil quenching. The heat treatment process is complicated and costly, and the oil smoke generated during oil quenching is not conducive to environmental protection. Summary of the invention

[0008] The technical problem to be solved by the present invention is to provide a high-toughness mining circular saw blade steel plate and a manufacturing method thereof in view of the above-mentioned prior art, which directly adopts water quenching, has low cost and is beneficial to the environment.

[0009] The technical solution adopted by the present invention to solve the above problems is: a high-toughness mining circular saw blade steel plate, the chemical composition of the steel plate is C: 0.47-0.52%, Si: 0.40-0.60%, Mn: 1.30-1.50%, V: 0.08-0.12%, Al: 0.03-0.06%, Cr: 0.10-0.30%, P: ≤0.012%, S: ≤0.002%, Ca: 0.0010-0.0030%, O: ≤0.002%, N: ≤0.004%, H: ≤0.0002%, and the remainder is Fe and unavoidable impurity elements.

[0010] The high-toughness mining circular saw blade steel plate of the present invention has a thickness of ≤12 mm and a maximum width of 4000 mm.

[0011] The reasons for limiting the steel composition in the present invention are as follows:

[0012] C: Carbon as a solid solution element can significantly improve the strength and hardness of the steel plate, but it has an adverse effect on the plasticity and welding performance of the steel plate. Based on the hardness requirements of the steel plate, the carbon content in the present invention is controlled to be 0.47-0.52%.

[0013] Si: Silicon enters ferrite to strengthen the steel by solid solution, which can significantly improve the elastic limit, yield strength and fatigue strength of steel, and improve the wear resistance and service life of saw blade steel. At the same time, Si element has the effect of reducing the volume change when austenite transforms to martensite, thereby effectively controlling the generation of quenching cracks. However, when the content is high, it can reduce the plastic toughness of steel. The Si content of the present invention is controlled to be 0.40-0.60%.

[0014] Mn: reduces the critical transition temperature Ar3, improves the hardenability of steel, plays a role in solid solution strengthening in the steel, and significantly improves the strength of the steel. If the Mn content is too high, segregation is likely to occur, reducing the toughness of the steel plate. The present invention stipulates that the amount of manganese added is within the range of 1.30-1.50%.

[0015] V: a grain-refining element. During tempering, V (C / N) precipitates, which can play a significant role in precipitation strengthening and heat resistance. If the V content is too low, the saw blade steel will soften at high temperatures and fail; if the V content is too high, the toughness and welding performance of the steel plate will deteriorate. Therefore, the V content of the present invention is controlled to be 0.08-0.12%.

[0016] Al: deoxidation and grain refinement element. The present invention eliminates the addition of Nb and Ti, and mainly uses Al to refine grains above 900°C. If the content is too low, the grain refinement effect is not obvious, and if the content is too high, Al2O3 inclusions are easily formed, which is not conducive to toughness. The present invention stipulates that the Al content is 0.03-0.06%.

[0017] Cr: It is an element that improves the hardenability of steel, promotes the transformation of martensite, and improves the strength of steel. However, too high a Cr content will affect the toughness of the steel and reduce the welding performance of the steel plate. The chromium content of the present invention is controlled at 0.10-0.30%.

[0018] Ca: inclusion modification element, which can react with long strip MnS to generate spherical CaS, change the anisotropy of the steel plate, and can also modify the Al2O3 inclusions generated by Al deoxidation into spherical low-melting-point inclusions, promote the floating removal of inclusions, and improve the toughness of the steel plate. The present invention controls the Ca content to 0.0010-0.0030%.

[0019] P: Harmful element in steel, easy to segregate, and has an adverse effect on the plasticity and toughness of the material. High P content increases the brittleness of the steel plate and easily causes cold bending cracking of the steel plate. The present invention stipulates that P: ≤ 0.012%

[0020] S: A harmful element in steel, which is easy to segregate and easily forms MnS segregation inclusions with Mn elements, resulting in delamination and cracking of the steel plate, significantly reducing the cold bending performance of the steel plate. Since the present invention adopts a high Mn design, the S content must be controlled at a low level, and S is specified to be ≤0.002%.

[0021] O, N, H: harmful gas elements, high content, many inclusions, reduce the plastic toughness of steel plates, and have a high risk of cracking of steel plates. The present invention strictly controls the O content to be no higher than 0.002%; the N content to be no higher than 0.004%; and the H content to be no higher than 0.0002%.

[0022] The present invention further provides a method for preparing the above-mentioned high-toughness mining circular saw blade steel plate, and the specific process is as follows:

[0023] Smelting and continuous casting process: Pre-treat the molten iron, smelt in an electric furnace or converter, then send it to the LF refining furnace for refining, and undergo VD or RH vacuum treatment. After the molten steel is degassed, trace Ca treatment is performed. Continuous casting adopts low superheat pouring, argon protection pouring throughout the process, and dynamic light pressure control. The superheat of the molten steel is controlled at 5-20℃, the center segregation is not higher than C1.0 level, and the center looseness is not higher than 1.0 level.

[0024] Heating process: Due to the high C content of the billet, cracks are easily generated. The billet is quickly lowered and directly sent to the walking beam heating furnace without slow cooling. The temperature of the billet sent into the furnace is not less than 400℃, and the heating rate is ≤8.5min / cm. In order to avoid decarburization on the billet surface during the heating process, the billet adopts a low-temperature soaking process, with a soaking temperature of 1150~1180℃ and a soaking time of 25~50min.

[0025] Steel rolling process: After the ingot is removed from the furnace, it is descaled by high-pressure water and then rolled in the furnace coil mill or wide and thick plate mill. The maximum width can reach 4000mm. The steel plate adopts high-temperature hot rolling, with the starting rolling temperature between 1000 and 1100℃ and the final rolling temperature ≥900℃. After the steel plate is rolled, it is quickly stacked and slowly cooled. The slow cooling time is ≥48 hours to avoid the generation of cooling stress.

[0026] Quenching process: The steel plate is quenched offline after slow cooling. In order to increase the toughness of the saw blade steel and avoid quenching cracks, the steel plate is quenched in the Ac1-Ac3 two-phase region, the quenching temperature is 720-780℃, and the heat preservation time is 30-60min after the core of the steel plate reaches the temperature.

[0027] Tempering process: After quenching, the steel plate needs to be tempered at 400-500℃. After the core of the steel plate reaches the temperature, the tempering holding time is 30-90min.

[0028] Compared with the prior art, the advantages of the present invention are:

[0029] The invention adopts an economical component design, only contains low-cost metal elements such as C, Si, Mn, Cr, V and Ca, and has low cost.

[0030] The present invention adopts hot delivery and hot loading process for rolling, the temperature of the hot billet into the furnace is not less than 400°C, and the heating rate is ≤8.5min / cm, which solves the problem of cracks in the medium and high carbon saw blade steel billet and utilizes the heat of the billet, reduces heating energy consumption, speeds up the production rhythm, is conducive to mass production, and further reduces costs.

[0031] The steel plate is rolled by furnace coil or wide and thick plate mill. Compared with the traditional hot rolling production process of saw blade steel, the diameter of the saw blade produced is larger, up to 4000mm. At the same time, the steel plate is rolled flat, without curling, which reduces the subsequent flattening process for customers, with high straightness and low cost.

[0032] The present invention eliminates laminar cooling and adopts high-temperature hot rolling and post-rolling slow cooling processes, thereby reducing the internal stress of the steel plate and avoiding the generation of quenching cracks.

[0033] Unlike the traditional oil quenching heat treatment of saw blade steel, the present invention directly uses water quenching, which is low-cost and environmentally friendly. The steel plate is quenched in the two-phase region to obtain a two-phase structure of martensite and ferrite. The martensite matrix provides high hardness and high strength, and the ferrite matrix greatly improves the toughness of the saw blade steel, reducing the risk of brittle fracture during subsequent use.

[0034] The steel plate has excellent toughness, 20℃ impact Akv≥27J, hardness 30~40HRC. The saw blade made of it can operate stably in the range of 400~500℃ and has a long service life.

[0035] The method of the present invention can be extended and applied to the production of other high-carbon or low-carbon saw blade steels. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a typical quenched microstructure metallographic picture of the test steel of Example 1 of the present invention. DETAILED DESCRIPTION

[0037] The present invention will be further described below with reference to examples.

[0038] The production process of the high-strength steel of the present invention is: converter or electric furnace steelmaking->LF refining->VD or RH vacuum degassing->Ca treatment->continuous casting->hot transport->heating->rolling->steel plate slow cooling->quenching->tempering.

[0039] The method for producing the high-toughness mining circular saw blade steel plate of Embodiment 1-2 of the present invention comprises the following steps:

[0040] (1) Steelmaking and continuous casting: 150-ton converter is used for smelting, then sent to LF furnace for refining and RH vacuum degassing treatment, and Ca treatment is performed by breaking the air. Molten steel is cast into 150 mm thick continuous casting billets. The casting temperature is controlled at 5-20 °C above the liquidus. Dynamic soft reduction is implemented during the casting process. The center segregation is not higher than C1.0 level, and the center porosity is not higher than 1.0 level. The final composition control of molten steel is shown in Table 1.

[0041] (2) Heating and rolling: The continuous casting billet obtained in step (1) is hot-transferred to a walking beam heating furnace. The temperature of the billet when hot-transferred into the furnace is not less than 400°C, and the heating rate is ≤8.5min / cm. The billet is subjected to a low-temperature soaking process, with a soaking temperature of 1150-1180°C and a soaking time of 25-50min. After the billet is removed from the furnace, it is descaled by high-pressure water and then rolled into a furnace coil mill or a wide and thick plate mill. The steel plate is subjected to high-temperature hot rolling, with a starting rolling temperature between 1000 and 1100°C and a final rolling temperature ≥900°C.

[0042] (3) Slow cooling: After the steel plate is rolled, it is quickly stacked and slowly cooled down. The slow cooling time is ≥ 48 hours to avoid the generation of cooling stress.

[0043] (4) Quenching: After the steel plate is slowly cooled, it is subjected to offline quenching treatment. In order to increase the toughness of the saw blade steel and avoid quenching cracks, the steel plate is quenched in the Ac1-Ac3 two-phase region, with a quenching temperature of 720-780°C. After the core of the steel plate reaches the temperature, the holding time is 30-60 minutes.

[0044] (5) Tempering: After quenching, the steel plate needs to be tempered at 400-500°C. After the core of the steel plate reaches temperature, the tempering holding time is 30-90 minutes.

[0045] The specific composition and process parameters are shown in Tables 1 to 3. The corresponding properties of each example sample are shown in Table 4.

[0046] Table 1 Chemical composition of the super-strong steel plate of the embodiment (wt%)

[0047] Example C Si Mn P S Al V Cr Ca O N H 1 0.51 0.50 1.45 0.010 0.001 0.040 0.11 0.25 0.0015 0.0010 0.0030 0.0001 2 0.49 0.55 1.40 0.010 0.001 0.045 0.09 0.15 0.0012 0.0008 0.0028 0.0001

[0048] Table 2 Rolling process control

[0049]

[0050] Table 3 Heat treatment process control

[0051]

[0052] Table 4 Tensile, impact and bending properties of the embodiments of the present invention

[0053]

[0054]

[0055] Figure 1 The metallographic photographs of the typical quenched structure of the test steel of Example 1 are given. The quenched structure of the steel plate is a dual-phase structure consisting of martensite and ferrite, which ensures that the steel plate has excellent impact toughness.

[0056] The present invention adopts high-cleanliness steelmaking continuous casting process, hot delivery hot rolling and tempering heat treatment process, and controls from the perspectives of chemical composition design, parent material structure, rolling deformation, heat treatment temperature and time, to ensure that the steel plate has high wear resistance, high toughness and excellent heat resistance, and provides a solution for improving the impact toughness of medium and high carbon saw blade steel.

[0057] Although the preferred embodiments of the present invention are described in detail above, it should be clearly understood that various modifications and variations are possible for those skilled in the art. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A high-toughness mining circular saw blade steel plate, characterized by: The steel plate is composed of the following components in weight percentage: C: 0.47-0.52%, Si: 0.40-0.60%, Mn: 1.30-1.50%, V: 0.08-0.12%, Al: 0.03-0.06%, Cr: 0.10-0.30%, P: ≤0.012%, S: ≤0.002%, Ca: 0.0010-0.0030%, O: ≤0.002%, N: ≤0.004%, H: ≤0.0002%, and the balance is Fe and unavoidable impurity elements; The steel plate has an impact value of 27J or higher at 20°C and a hardness of 30-40HRC. The saw blade made of the steel plate can operate stably in the range of 400-500°C. The quenched structure of the steel plate is a dual-phase structure consisting of fine martensite structure and ferrite structure.

2. The high-toughness mining circular saw blade steel plate according to claim 1, characterized in that The thickness of the steel plate is ≤12 mm and the width is up to 4000 mm.

3. A method for manufacturing a high-toughness mining circular saw blade steel plate as claimed in claim 1, characterized in that: The entire process is: smelting, continuous casting, heating, rolling, slow cooling, quenching and tempering. The specific steps are: (1) Smelting and continuous casting According to the specified chemical composition, it is smelted by converter method, and further fine-tuned by off-furnace refining and vacuum treatment; (2) Heating rolling The ingot after continuous casting is directly sent to the heating furnace with a temperature of not less than 400℃ and a heating rate of ≤8.5min / cm. After the ingot is removed from the furnace, it is descaled by high-pressure water and then sent to the furnace coil mill or wide and thick plate mill for rolling. (3) Slow cooling After the steel plate is rolled, it is quickly taken off the production line for stacking and slow cooling, and the slow cooling time is ≥48 hours; (4) Quenching: After slow cooling, the steel plate is quenched in the Ac1-Ac3 two-phase region at a quenching temperature of 720-780°C. After the core of the steel plate reaches the temperature, the holding time is 30-60 minutes. (5) Tempering: After quenching, the steel plate is tempered at 400-500°C. After the core of the steel plate reaches temperature, the tempering holding time is 30-90 minutes.

4. The method for manufacturing a high-toughness mining circular saw blade steel plate according to claim 3, characterized in that: The smelting and continuous casting process is specifically as follows: pre-treating the molten iron, smelting in an electric furnace or a converter, then sending it to a LF refining furnace for refining, and undergoing VD or RH vacuum treatment. After the molten steel is degassed, trace Ca treatment is performed, and continuous casting adopts low superheat pouring, argon protection pouring throughout the process, and dynamic light pressure control. The superheat of the molten steel is controlled at 5 to 20°C, the center segregation is not higher than C1.0 level, and the center porosity is not higher than 1.0 level.

5. The method for manufacturing a high-toughness mining circular saw blade steel plate according to claim 3, characterized in that: In the step (2), in order to avoid decarburization on the surface of the ingot during the heating process, the ingot is subjected to a low-temperature soaking process, the soaking temperature of the ingot is 1150-1180° C., and the soaking time is 25-50 min.

6. The method for manufacturing a high-toughness mining circular saw blade steel plate according to claim 3, characterized in that: In the step (2), the steel plate is hot rolled at a high temperature, with the starting rolling temperature being between 1000°C and 1100°C and the final rolling temperature being ≥900°C.

Citation Information

Patent Citations

  • 50Mn2V Steel Plate for Saw Blade and Its Production Method

    CN105063478B

  • High temperature deformation resistant 75Cr1 saw steel and production technology thereof

    CN110284061A

  • Production method of steel for mine ultra-wide disk saw blade

    CN113684421A

  • Production method of high-strength saw bit steel coil

    CN103173685A

  • Economical and ultra-wide saw steel and preparation method thereof

    CN104532150A