A method for improving the color difference defect of nitriding oriented silicon steel
By using low-carbon steel protective plates and optimizing atmosphere treatment during the high-temperature annealing process, the problem of color difference defects in finished oriented silicon steel plates was solved, crystallization water removal and atmosphere purification were achieved, and the quality of the product surface was significantly improved.
Patent Information
- Application Number
- CN202310060901.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-18
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-01-18
AI Technical Summary
In the production of grain-oriented silicon steel, the presence of water vapor during the high-temperature annealing process causes excessive oxidation of the steel coil and generates more local iron oxides, which hinders the reaction between SiO2 and MgO and prevents the formation of a magnesium silicate bottom layer, resulting in color defects on the surface of the finished plate.
When using a ring furnace for high-temperature annealing, place a 0.3-0.8mm thick circular low-carbon steel protective plate above the steel coil, pass in the mixed gas of N2+H2, quickly heat up to remove crystal water, control the dew point of the atmosphere to be less than zero, and slowly heat up. A bottom layer of magnesium silicate is formed, and after high-temperature annealing, it is replaced with a pure H2 atmosphere to purify S and N in the matrix.
It effectively reduces the contact between the top of the steel coil and water vapor, reduces the temperature difference between the inner and outer rings, removes crystal water, significantly improves the color difference defects of the finished oriented silicon steel plates, and ensures the formation of the magnesium silicate bottom layer and product quality.
Smart Images

Figure BDA0004061211590000041
Abstract
Description
Technical Field
[0001] The invention relates to the production of cold-rolled oriented silicon steel, and in particular to a method for improving the color difference defect of oriented silicon steel produced by nitriding process. Background Art
[0002] Cold-rolled oriented silicon steel is a soft magnetic material widely used in the fields of electricity, electronics, etc. Due to the complex manufacturing process and equipment of oriented silicon steel, strict composition control, extremely low impurity content requirements, long manufacturing process and many factors affecting performance, its product quality is often considered to be an important indicator of a country's special steel manufacturing level.
[0003] At the same time, in the current context of scarce resources, serious environmental pollution and fierce market competition, the manufacturing of oriented silicon steel products must not only meet the requirements of magnetic properties, but also focus on reducing costs, reducing pollution and improving production efficiency. Therefore, a more energy-saving, environmentally friendly and low-cost low-temperature production process has become the goal pursued by major silicon steel manufacturers in the world. After decarburization annealing is completed, nitriding treatment is carried out to form (A1, Si) N precipitates with inhibitor function before the final secondary recrystallization begins. Using the nitriding annealing process, the heating temperature of the slab can be reduced to 1150-1200C, which is the lowest temperature used for slab heating in the current industrial production of oriented silicon steel.
[0004] In the production of oriented silicon steel, in order to prevent the steel strips from sticking to each other during high-temperature annealing, a thin layer of high-temperature resistant MgO isolating agent needs to be coated on the surface of the steel strip. During high-temperature annealing, MgO reacts with the SiO2 oxide layer on the surface of the silicon steel to form a magnesium silicate bottom layer. The quality of the magnesium silicate bottom layer directly determines the performance of the silicon steel surface, and the surface quality directly determines the lamination and insulation of the silicon steel plate, which has an important impact on product quality. The magnesium silicate bottom layer also has a certain anti-rust effect, and the expansion coefficient of magnesium silicate is also smaller than that of silicon steel, which will cause a certain tension on the surface of the steel strip and reduce the magnetostriction of the steel strip.
[0005] During high-temperature annealing, if there is water in the atmosphere, the steel strip will produce additional oxidation. The water in the atmosphere is mainly related to MgO. 400-600℃ is the drainage stage when the MgO coated on the steel coil releases chemical water during high-temperature annealing. The hydration rate of MgO is high, that is, the Mg(OH)2 content is high. During the high-temperature annealing process, Mg(OH)2 decomposes to produce more chemical water, which increases the dew point in the high-temperature annealing atmosphere, and then causes the steel strip to be over-oxidized, generating more local iron oxides. This oxide will hinder the reaction of SiO2 and MgO, and it is impossible to form a magnesium silicate bottom layer. The consequence is often that the bottom layer falls off in a large area. After the high-temperature annealed plate is coated with an insulating coating, color difference defects appear on the surface of the finished plate.
[0006] When a ring furnace is used for high-temperature annealing, the temperature difference between the inner and outer rings of the steel coil can reach 100-200°C during the heating process. When the outer temperature of the steel coil reaches the set temperature, the lower part of the steel coil and the inner ring may still not reach the temperature at the end of the insulation, resulting in incomplete removal of moisture, oxidation of the steel coil at high temperature, and color defects on the surface of the finished plate. Summary of the invention
[0007] The technical problem to be solved by the present invention is to provide a method for improving the color difference defects of oriented silicon steel produced by nitriding process, thereby significantly improving the color difference defects of oriented silicon steel finished plates.
[0008] To achieve the above object, the present invention adopts the following technical solutions:
[0009] A method for improving the color difference defect of oriented silicon steel by nitriding method, the process includes: smelting, continuous casting, hot rolling, normalizing, cold rolling, decarburization annealing, MgO coating, nitriding, high temperature annealing; the specific process of high temperature annealing is:
[0010] (1) Use a ring furnace for high temperature annealing. When loading the furnace, place a 0.3-0.8mm thick circular low-carbon steel protective plate above the steel coil. The diameter of the protective plate is the same as the diameter of the steel coil.
[0011] (2) introducing a mixed gas of N2+H2, with a N2 volume percentage of 55-85%, rapidly heating the chamber to 350-400°C at a rate greater than 60°C / h, slowly heating the chamber to 650-750°C at a rate of 20-30°C / h, keeping the chamber warm for 3-10 hours to remove crystal water, measuring the atmosphere dew point, and controlling the dew point to be less than zero;
[0012] (3) After that, the atmosphere remains unchanged and the temperature is slowly raised to 950-1050°C at a rate of 10-20°C / h to cause secondary recrystallization; the temperature is raised to 980-1080°C to form a magnesium silicate bottom layer; after the temperature is raised to 1200°C, it is replaced with a pure H2 atmosphere and kept at this temperature for 3-10 hours to purify S and N in the matrix;
[0013] (4) High temperature annealed coils are heat stretched, flattened and annealed before being coated with an insulating coating.
[0014] The specific process of smelting and continuous casting is as follows:
[0015] (1) The mass percentages of the elements in the designed Hi-B steel are as follows: 0.031% ≤ C ≤ 0.074%, 2.620%
[0016] ≤Si≤3.700%、0.003%≤Mn≤0.100%、0.001%≤S≤0.015%、0.001%≤P≤0.015%、0.001%≤Als≤0.040%、0.0010%≤N≤0.0150%,the rest are Fe and impurities;
[0017] (2) Using converter smelting and RH refining, molten steel is poured when the superheat is less than 25°C, and the ingot is hot-sent after continuous casting. The thickness of the slab is 180-230 mm.
[0018] The specific processes of hot rolling, normalizing and cold rolling are as follows:
[0019] (1) The heating temperature of the ingot is designed to be 1150-1250°C, the heating time is 180-240 min, and the target thickness of the hot-rolled plate is 1.80-2.50 mm;
[0020] (2) Select 980-1150℃ as the normalizing heating temperature, keep warm for 1-4 minutes, start air cooling, and start quenching in 100-120℃ water for rapid cooling when the temperature reaches 890±10℃;
[0021] (3) The cold rolled plate is rolled in 5 passes using a Sendzimir single-stand twenty-roller reversible rolling mill, and the thickness of the cold rolled plate is 0.10 to 0.29 mm.
[0022] The specific processes of decarburization annealing, MgO coating and nitriding are as follows:
[0023] (1) Decarburization annealing temperature is 780-880°C, time is 1-5 min, protective atmosphere is 75% H2+25% N2 mixed gas through water, water temperature is 55-75°C;
[0024] (2) Nitriding annealing and decarburization annealing are carried out on the same continuous furnace production line, the nitriding temperature is 650-780°C, the nitriding time is 10-50s, and the nitriding atmosphere is as follows by volume percentage: first, a 75% N2+25% H2 mixed gas is introduced, and then NH3 is introduced, and NH3 is 5-13% of the mixed gas;
[0025] (3) After nitriding annealing, MgO is applied as a separator by roller coating, and the MgO drying temperature is 450-550°C.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The present invention adopts a protective plate on the top of the high-temperature annealing steel coil and optimizes the high-temperature annealing process to reduce the contact between the top of the steel coil and water vapor, reduce the temperature difference between the inner and outer circles of the steel coil, effectively remove crystallization water, and significantly improve the color difference defects of the oriented silicon steel finished plate.
[0028] (1) When the high-temperature annealing steel coil is loaded into the furnace, a protective plate is placed on the top of the steel coil to prevent the inner and outer circles of the top of the steel coil from being in contact with the high dew point atmosphere for a long time, thereby improving the color difference defect at the top of the steel coil.
[0029] (2) In the high-temperature annealing process, the temperature is slowly increased during the crystallization water removal stage to reduce the temperature difference between the inner and outer rings of the steel coil, and the insulation process is increased to reduce the temperature difference between the inner and outer rings of the steel coil, fully remove the crystallization water in the MgO coating, and reduce the oxidation of the steel coil at high temperature. DETAILED DESCRIPTION
[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] A method for improving the color difference defect of oriented silicon steel by nitriding method, the process includes: smelting, continuous casting, hot rolling, normalizing, cold rolling, decarburization annealing, MgO coating, nitriding, high temperature annealing; specifically including:
[0032] 1. Composition, smelting and continuous casting
[0033] (1) The mass percentages of the designed Hi-B steel elements are: 0.044% C, 3.420% Si, 0.073% Mn, 0.006% S, 0.010% P, 0.026% Als, 0.0066% N, and the rest are Fe and impurities.
[0034] (2) Converter smelting and RH refining are adopted. The molten steel is poured when the superheat degree is 20°C. The ingot is hot-sent after continuous casting. The thickness of the slab is 210 mm.
[0035] 2. Hot rolling, normalizing and cold rolling
[0036] (1) The heating temperature of the ingot is designed to be 1220°C, the heating time is 220 min, and the thickness of the hot-rolled plate is 2.30 mm.
[0037] (2) Select 1140°C as the normalizing heating temperature, keep it at this temperature for 2.5 min, then start air cooling. When the temperature drops to 890°C, start quenching in water at 100-120°C for rapid cooling.
[0038] (3) A Sendzimir single-stand twenty-roller reversible rolling mill is used, with 5 passes and a cold-rolled plate thickness of 0.23 mm.
[0039] 3. Decarburization annealing, MgO coating and nitriding
[0040] (1) Decarburization annealing temperature is 800°C, time is 3.5 min, protective atmosphere is wet (through water) 75% H2+25% N2 mixed gas, water temperature is 65°C.
[0041] (2) Nitriding annealing and decarburization annealing are carried out on the same continuous furnace production line. The nitriding temperature is 720°C, the nitriding time is 30s, and the nitriding atmosphere is as follows by volume percentage: first, a dry 75% N2+25% H2 mixed gas is introduced, and then NH3 is introduced, and NH3 accounts for 8% of the mixed gas.
[0042] (3) After nitriding annealing, MgO is applied as a separator by roller coating, and the drying temperature of MgO is 470°C. The nitriding process can increase the inhibitor's inhibitory capacity and reduce the heating temperature of the ingot, saving energy.
[0043] 4. Use ring furnace for high temperature annealing
[0044] (1) When loading the furnace, place a 0.5mm thick circular low-carbon steel protective plate with the same size as the diameter of the steel coil on the top of the steel coil.
[0045] (2) First, introduce a mixed gas of 80% N2 + 20% H2, quickly raise the temperature to 380°C at a rate of 65°C / h, then slowly raise the temperature to 680°C at a rate of 22°C / h, keep warm for 8 hours to remove crystal water, measure the dew point of the atmosphere, and control the dew point to be less than zero. In the process of removing crystal water, the protective plate prevents the upper part, inner ring and outer ring of the steel coil from being in contact with the high dew point atmosphere generated by the crystal water for a long time.
[0046] (3) After that, the atmosphere remains unchanged and the temperature is slowly raised to 1000°C at a rate of 14°C / h to cause secondary recrystallization; the temperature is raised to 1050°C to form a magnesium silicate bottom layer; after the temperature is raised to 1200°C, it is switched to a pure H2 atmosphere and kept at this temperature for 10 hours to purify the S and N in the matrix.
[0047] (4) After the high temperature annealing coil is hot stretched and flattened, an insulating coating is applied and the surface quality of the finished board is tested.
[0048] In order to compare the effects of the temperature rise rate and the holding time in the protection plate and the crystal water removal stage on the color difference defects, the color difference defects of different implementation schemes are compared. The comparison results are shown in Table 1.
[0049] Table 1 Comparison of Examples and Comparative Examples
[0050]
[0051] From Table 1, we can know that adding protective plates when high-temperature annealing steel coils are loaded into the furnace, slowing down the heating rate in the high-temperature annealing process to remove crystal water and increasing the holding time can effectively reduce the color difference defects of oriented silicon steel finished plates.
[0052] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and basic spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for improving the color difference defect of nitriding oriented silicon steel, characterized in that: Process: smelting, continuous casting, hot rolling, normalizing, cold rolling, decarburization annealing, MgO coating, nitriding, high temperature annealing; the specific process of high temperature annealing is: (1) Use a ring furnace for high temperature annealing. When loading the furnace, place a 0.3-0.8mm thick circular low-carbon steel protective plate above the steel coil. The diameter of the protective plate is the same as the diameter of the steel coil. (2) introducing a mixed gas of N2+H2, with a N2 volume percentage of 55-85%, rapidly heating the chamber to 350-400°C at a rate greater than 60°C / h, slowly heating the chamber to 650-750°C at a rate of 20-30°C / h, keeping the chamber warm for 3-10 hours to remove crystal water, measuring the atmosphere dew point, and controlling the dew point to be less than zero; (3) After that, the atmosphere remains unchanged and the temperature is slowly raised to 950-1050°C at a rate of 10-20°C / h to cause secondary recrystallization; the temperature is raised to 980-1080°C to form a magnesium silicate bottom layer; after the temperature is raised to 1200°C, it is replaced with a pure H2 atmosphere and kept at this temperature for 3-10 hours to purify S and N in the matrix; (4) High temperature annealed coils are heat stretched, flattened and annealed before being coated with an insulating coating.
2. The method for improving the color difference defect of nitrided grain-oriented silicon steel according to claim 1, characterized in that: The specific process of smelting and continuous casting is as follows: (1) The mass percentages of the elements in the designed Hi-B steel are as follows: 0.031% ≤ C ≤ 0.074%, 2.620% ≤Si≤3.700%、0.003%≤Mn≤0.100%、0.001%≤S≤0.015%、0.001%≤P≤0.015%、0.001%≤Als≤0.040%、0.0010%≤N≤0.0150%,the rest are Fe and impurities; (2) Using converter smelting and RH refining, molten steel is poured when the superheat is less than 25°C, and the ingot is hot-sent after continuous casting. The thickness of the slab is 180-230 mm.
3. The method for improving the color difference defect of nitrided grain-oriented silicon steel according to claim 1, characterized in that: The specific processes of hot rolling, normalizing and cold rolling are as follows: (1) The heating temperature of the ingot is designed to be 1150-1250°C, the heating time is 180-240 min, and the target thickness of the hot-rolled plate is 1.80-2.50 mm; (2) Select 980-1150℃ as the normalizing heating temperature, keep warm for 1-4 minutes, start air cooling, and start quenching in 100-120℃ water for rapid cooling when the temperature reaches 890±10℃; (3) The cold rolled plate is rolled in 5 passes using a Sendzimir single-stand twenty-roller reversible rolling mill, and the thickness of the cold rolled plate is 0.10 to 0.29 mm.
4. The method for improving the color difference defect of nitrided grain-oriented silicon steel according to claim 1, characterized in that: The specific processes of decarburization annealing, MgO coating and nitriding are as follows: (1) Decarburization annealing temperature is 780-880°C, time is 1-5 min, protective atmosphere is 75% H2+25% N2 mixed gas through water, water temperature is 55-75°C; (2) Nitriding annealing and decarburization annealing are carried out on the same continuous furnace production line, the nitriding temperature is 650-780°C, the nitriding time is 10-50s, and the nitriding atmosphere is as follows by volume percentage: first, a 75% N2+25% H2 mixed gas is introduced, and then NH3 is introduced, and NH3 is 5-13% of the mixed gas; (3) After nitriding annealing, MgO is applied as a separator by roller coating, and the MgO drying temperature is 450-550°C.