Acrylic rubber with excellent roll processability, strength characteristics, and compression set resistance
By using specific monomers containing ion reactive groups in acrylic rubber and extrusion drying process with high shear conditions in the prior art, the problems of poor processability of acrylic rubber rollers and poor water resistance of crosslinkers are solved, and the problem of poor processability of crosslinkers in the prior art is achieved. High strength and good compression resistance to permanent deformation.
Patent Information
- Application Number
- CN202180057906.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-25
- Filing Date
- 2021-06-04
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-06-04
AI Technical Summary
The existing acrylic rubbers have shortcomings in roll processing properties, crosslinking properties, compression resistance, and storage stability, especially in roll processing properties, and poor water resistance and strength characteristics of crosslinking objects.
The composition and manufacturing process of acrylic rubber are optimized by the GPC-MALS method using specific monomer components containing ion reactive groups, and the absolute molecular weight and molecular weight distribution are measured by the GPC-MALS method. Improves its roller processability, strength characteristics of crosslinked objects and permanent deformation resistance to compression.
The roller processability, crosslinking, water resistance and storage stability of acrylic rubber is significantly improved, and the high strength of the crosslinked object and good compression resistance are achieved.
Smart Images

Figure GDA0004113506750000681 
Figure GDA0004113506750000711 
Figure GDA0004113506750000721
Abstract
Description
Technical Field
[0001] The present invention relates to an acrylic rubber, a method for producing the same, a rubber molded product, a rubber composition, and a rubber cross-linked product. More specifically, the present invention relates to an acrylic rubber having excellent roll processability and cross-linkability and excellent strength characteristics and compression set resistance of a cross-linked product, a method for producing the same, an acrylic rubber molded product obtained by molding the acrylic rubber, a rubber composition containing the acrylic rubber, and a rubber cross-linked product obtained by cross-linking the acrylic rubber. Background Art
[0002] Acrylic rubber is a polymer mainly composed of acrylic acid esters, and is generally known as a rubber having excellent heat resistance, oil resistance, and ozone resistance, and is widely used in automobile-related fields and the like.
[0003] For example, Patent Document 1 (International Publication No. 2019 / 188709 Pamphlet) discloses a method for manufacturing acrylic rubber, in which monomer components consisting of ethyl acrylate, butyl acrylate, methoxyethyl acrylate and monobutyl fumarate, water and sodium lauryl sulfate are added, and after repeated decompression degassing and nitrogen substitution, sodium formaldehyde sulfoxylate and isopropylbenzene hydroperoxide as an organic free radical generator are added, and emulsion polymerization is initiated at normal pressure and room temperature, and emulsion polymerization is carried out until the polymerization conversion rate reaches 95% by weight, and then it is coagulated with an aqueous solution of calcium chloride, filtered with a metal mesh, and then dehydrated and dried using an extrusion dryer with a screw to manufacture acrylic rubber. However, the acrylic rubber obtained using this method has extremely poor roll processability and Banbury processability, and also has poor storage stability and water resistance.
[0004] Patent document 2 (Japanese Patent Publication No. 2019-119772) discloses the following method: using pure water and sodium lauryl sulfate and polyoxyethylene lauryl ether as emulsifiers to prepare a monomer emulsion composed of ethyl acrylate, butyl acrylate, methoxyethyl acrylate and monobutyl maleate, a portion of the monomer emulsion is put into a polymerization reaction tank, cooled to 12°C under a nitrogen flow, and then the remaining monomer emulsion, ferrous sulfate, sodium ascorbate and as an emulsifier are continuously added dropwise for 3 hours. The aqueous solution of potassium persulfate, which is an inorganic free radical generator, is then maintained at 23°C and emulsion polymerization is continued for 1 hour. After the polymerization conversion rate reaches 97% by weight, the temperature is raised to 85°C, and then sodium sulfate is continuously added to perform coagulation and filtration separation to obtain water-containing pellets. The water-containing pellets are washed with water 4 times, washed with acid once, and washed with pure water once, and then the acrylic rubber is continuously made into a sheet using an extrusion dryer with a screw, and cross-linked using an aliphatic polyamine compound such as hexamethylenediamine carbamate. However, the sheet-like acrylic rubber obtained by this method has problems such as poor roll processability and poor water resistance of the cross-linked product.
[0005] Patent document 3 (Japanese Patent Application Laid-Open No. 1-135811) discloses a method in which 1 / 4 of a monomer mixture consisting of ethyl acrylate, caprolactone addition type acrylate, cyanoethyl acrylate and vinyl chloroacetate and n-dodecyl mercaptan as a chain transfer agent is emulsified with sodium lauryl sulfate, polyethylene glycol nonylphenyl ether and distilled water, sodium sulfite and ammonium persulfate as an inorganic free radical generator are added to initiate polymerization, the remaining monomer mixture and a 2% aqueous solution of ammonium persulfate are added dropwise over 2 hours while the temperature is maintained at 60°C, the polymerization is further continued for 2 hours after the addition, and a latex having a polymerization conversion rate of 96 to 99% is obtained, the latex is put into an aqueous sodium chloride solution at 80°C, coagulated, washed with water, and then dried to produce an acrylic rubber, which is crosslinked with sulfur. However, the acrylic rubber obtained by this method has problems such as poor roll processability and storage stability, and poor strength characteristics and water resistance of the crosslinked product.
[0006] Patent document 4 (Japanese Patent Publication No. 2018-168343) discloses the following method: preparing a monomer emulsion consisting of the following monomer components, pure water, sodium lauryl sulfate, polyethylene glycol monostearate and n-dodecyl mercaptan as a chain transfer agent, wherein the monomer components consist of ethyl acrylate, butyl acrylate and monobutyl fumarate, and then, a portion of the monomer emulsion and pure water are added to a polymerization reaction tank, cooled to 12°C, and the remaining monomer emulsion, ferrous sulfate, sodium ascorbate and potassium persulfate as an inorganic free radical generator are continuously added dropwise over 2.5 hours, and then maintained at 23°C. After continuing the reaction for 1 hour, industrial water is added, the temperature is raised to 85°C, and sodium sulfate is continuously added at 85°C to coagulate, thereby obtaining water-containing granules, which are washed with pure water three times and then dried with a hot air dryer to produce acrylic rubber, which is cross-linked with 2,2-bis[4-(4-aminophenoxy)phenyl]propane. However, although the acrylic rubber obtained by this method is excellent in stress relaxation and extrusion processability, it has problems such as insufficient roll processability and storage stability and poor strength characteristics and water resistance of the cross-linked product.
[0007] Patent document 5 (Japanese Patent Application Laid-Open No. 9-143229) discloses a method in which a monomer mixture consisting of ethyl acrylate, special acrylate and vinyl monochloroacetate, sodium lauryl sulfate as an emulsifier, n-octyl mercaptan as a chain transfer agent and water are added to a reaction vessel, nitrogen substitution is performed, ammonium hydrogen sulfite and sodium persulfate as an inorganic free radical generator are added, a polymerization reaction is initiated, copolymerization is performed at 55° C. for 3 hours at a reaction conversion rate of 93 to 96%, and acrylic rubber is produced, and crosslinking is performed with sulfur. However, the acrylic rubber obtained by this method has problems such as poor roll processability and storage stability, and poor strength characteristics and water resistance of the crosslinked product.
[0008] Patent document 6 (Japanese Patent Application Laid-Open No. 62-64809) discloses an acrylic rubber which is excellent in processability, compression set and tensile strength and can be vulcanized with sulfur. The acrylic rubber is characterized in that it is a copolymer composed of monomers consisting of 50 to 99.9% by weight of at least one compound of alkyl acrylate and alkoxyalkyl acrylate, 0.1 to 20% by weight of a dihydrodicyclopentenyl-containing ester of an unsaturated carboxylic acid having a radical reactive group, and 0 to 20% by weight of at least one other monovinyl, monovinylidene and monovinylene unsaturated compounds, and has a polystyrene-equivalent number average molecular weight (Mn) of 200,000 to 1.2 million using tetrahydrofuran as an elution solvent, and a ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of 10 or less. In addition, the following contents are also recorded: Regarding the number average molecular weight (Mn), it is 200,000 to 1,000,000, preferably 200,000 to 1,000,000. If Mn is less than 200,000, the physical properties and processability of the sulfide are poor, and when it exceeds 1,200,000, the processability is poor. In addition, regarding the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) (Mw / Mn), when it exceeds 10, the compression set is large, which is not preferred. As a specific embodiment, the following production method is disclosed: monomer components including ethyl acrylate, free radical crosslinking dihydrodicyclopentenyl acrylate, etc., an emulsifier sodium lauryl sulfate, potassium persulfate as an inorganic free radical generator, and octyl thioglycolate and tert-dodecyl mercaptan as molecular weight regulators are added as variables to produce an acrylic rubber having a polymerization number average molecular weight (Mn) of 530,000 to 1.15 million, a weight average molecular weight (Mw) of 3.54 million to 6.26 million, and a ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of 4.7 to 8, which is coagulated in a calcium chloride aqueous solution, washed thoroughly with water, and directly dried. Moreover, the comparative examples of the embodiments show that when the amount of the chain transfer agent is small, the number average molecular weight (Mn) of the obtained acrylic rubber is as high as 5 million, and the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is as narrow as 1.4. When the amount of the chain transfer agent is large, the number average molecular weight (Mn) is as low as 200,000, and the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is extremely wide, reaching 17. However, the acrylic rubber obtained by this method has the following problems: poor compression set resistance and storage stability. Since it contains free radical reactive groups, even if an appropriate molecular weight distribution (Mw / Mn) is obtained in the polymerization reaction using a free radical generator, the molecular weight (Mw, Mn) is large and becomes too complicated, and the roll processability and Banbury processability are insufficient. In addition, the acrylic rubber obtained by this method also has the following problems: in the cross-linking reaction, sulfur and a vulcanization accelerator as a cross-linking agent are added, and after mixing with a roller, it is necessary to use 100kg / cm2 The problem is that the cross-linked product obtained by performing cross-linking for a long time at 170°C for 15 minutes in a vulcanizing press and then at 175°C for 4 hours in a Girdle oven has poor compression set resistance, water resistance and strength characteristics, and also has poor changes in physical properties after thermal degradation.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: International Publication No. 2019 / 188709;
[0012] Patent document 2: Japanese Patent Application Publication No. 2019-119772;
[0013] Patent document 3: Japanese Patent Application Laid-Open No. 1-135811;
[0014] Patent Document 4: Japanese Patent Application Publication No. 2018-168343;
[0015] Patent document 5: Japanese Patent Application Laid-Open No. 9-143229;
[0016] Patent document 6: Japanese Patent Application Laid-Open No. 62-64809. Summary of the invention
[0017] Problem that the invention aims to solve
[0018] The present invention has been made in view of the actual situation of the above-mentioned prior art, and an object of the present invention is to provide an acrylic rubber having excellent roll processability and short-time crosslinking property, and a crosslinked product having highly excellent strength characteristics and compression set resistance, a production method thereof, an acrylic rubber molded product obtained by molding the acrylic rubber, a rubber composition containing the acrylic rubber, and a rubber crosslinked product obtained by crosslinking the acrylic rubber.
[0019] Solutions for solving problems
[0020] The present inventors have conducted intensive studies in view of the above problems and have found that an acrylic rubber is composed of a bonding unit of a specific monomer component including an ion-reactive group-containing monomer, and the absolute molecular weight and the weight average molecular weight (Mw) of the absolute molecular weight distribution measured by the GPC-MALS method, the z-average molecular weight (Mz) focusing on high molecular weight components, and the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) are within specific ranges. This allows excellent roll processability and short-time crosslinking properties, and highly excellent strength characteristics and compression set resistance of the crosslinked product.
[0021] The present inventors have found that an acrylic rubber having an ion reactive group such as a carboxyl group, an epoxy group, or a chlorine atom that can react with a crosslinking agent and having a weight average molecular weight (Mw) and a z average molecular weight (Mz) on the high molecular weight side as determined by a GPC-MALS method within a specific range has excellent short-time crosslinking properties, strength characteristics, and compression set resistance.
[0022] The present inventors have found that the ion-reactive group-containing high-molecular-weight acrylic rubber cannot be sufficiently dissolved in tetrahydrofuran used in the GPC measurement of the radical-reactive acrylic rubber obtained by copolymerizing ethyl acrylate, dihydrodicyclopentenyl acrylate, etc. in the above-mentioned prior art, and that each molecular weight and molecular weight distribution cannot be measured neatly and reproducibly. However, by using a specific solvent having a higher SP value than tetrahydrofuran as an elution solvent, the acrylic rubber can be sufficiently dissolved and reproducibly measured, and by making each characteristic value within a specific range, the roll processability and crosslinking property of the acrylic rubber and the strength characteristics and compression set resistance of the crosslinked product can be highly balanced.
[0023] The present inventors have found that, with respect to the roll processability of acrylic rubber, when the weight average molecular weight (Mw) of the absolute molecular weight measured by the GPC-MALS method, the z average molecular weight (Mz), and the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) as the absolute molecular weight distribution are within a specific range, the roll processability can be significantly improved without impairing the strength characteristics. In addition, the present inventors have also found that the acrylic rubber with excellent roll processability can be produced by adding a chain transfer agent in batches during emulsion polymerization, or by melt-kneading and drying the water-containing pellets generated in the coagulation step in a specific extrusion dryer under high shear conditions.
[0024] Furthermore, the present inventors have found that by reducing the amount of insoluble components of acrylic rubber in a specific solvent, the Banbury processability can be significantly improved without impairing the roll processability, crosslinking properties, and the strength characteristics and compression set resistance of the crosslinked product. In addition, the present inventors have found that the insoluble components in the specific solvent are generated during the emulsion polymerization, and particularly when the polymerization conversion rate is increased to improve the strength characteristics, the amount thereof increases sharply and is difficult to control, but can be suppressed to a certain extent by adding a chain transfer agent at the end of the polymerization process, and preferably, by melt-kneading and drying the water-containing pellets generated in the coagulation process in a state substantially free of water (water content less than 1% by weight) in a specific extrusion dryer, the sharply increased insoluble components in the specific solvent disappear, and the Banbury processability can be significantly improved without impairing the roll processability of the acrylic rubber.
[0025] In addition, the inventors have also found that by making the ash content and ash fraction of acrylic rubber within a specific range, water resistance can be significantly improved without damaging roller processability, crosslinking, and the strength characteristics and compression set resistance of the crosslinked product. In addition, the inventors have also found that the ash content of acrylic rubber using a large amount of emulsifiers and coagulants for emulsion polymerization is difficult to reduce, but the water-containing aggregates generated using a specific coagulation method have particularly excellent cleaning efficiency in hot water and ash removal efficiency during dehydration, which can greatly reduce the ash content in the manufactured acrylic rubber and significantly improve water resistance. In addition, it has been found that by making the ash content in the ash fraction into specific components, water resistance and operability can be highly improved. In addition, it has been found that when a specific emulsifier is used in the emulsion polymerization of acrylic rubber, or when a specific coagulant is used in the case of coagulating the emulsion polymerization liquid, the water resistance of the acrylic rubber is excellent, and the release property from metal molds, etc. can be significantly improved.
[0026] In addition, the inventors have also found that the acrylic rubber molded body with a high specific gravity formed by molding the acrylic rubber into a sheet or a bag shape without containing air has particularly excellent handling and storage stability and does not impair the roll processability, crosslinking property, and the strength characteristics and compression set resistance of the crosslinked product. The inventors have found that when the water-containing pellets generated in the coagulation process are dried, a large amount of air is contained in the existing acrylic rubber molded body, which deteriorates the storage stability. However, by using a high-pressure baler or the like to compress the dried rubber obtained by directly drying the water-containing pellets, the specific gravity of the molded body can be slightly increased, and the storage stability can be improved. Preferably, the water-containing pellets generated in the coagulation process are dried in a specific extrusion dryer in a state without containing air to obtain the dried dry rubber, and the dried rubber is extruded into a sheet, and the sheet-shaped dry rubber is cut and stacked at a specific temperature as needed, thereby manufacturing an acrylic rubber molded body with particularly excellent storage stability. The inventors have also found that, in particular, by melt-kneading and drying the acrylic rubber under reduced pressure, the air in the acrylic rubber can be removed, and an acrylic rubber with excellent storage stability and strength characteristics can be obtained. The present inventors have also found that the storage stability can be further improved by using an acrylic rubber having a specific pH which is polymerized under the condition that the emulsion polymerization liquid is not neutral.
[0027] The present inventors have also found that by controlling the content of ion-containing reactive groups in the acrylic rubber, the monomer composition of the acrylic rubber, the complex viscosity at 60°C ([η]60°C), the ratio of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) ([η]100°C / [η]60°C), the water content, the pH, and the Mooney viscosity (ML1+4, 100°C) within specific ranges, the roll processability, crosslinking properties, strength properties, and compression set resistance can be further highly improved. Furthermore, by using a polyvalent organic compound as a crosslinking agent, the short-term crosslinking properties and the various properties of the obtained rubber cross-linked product can be further greatly improved.
[0028] The present inventors have also found that, after emulsifying a specific monomer component with water and an emulsifier, emulsion polymerization is initiated in the presence of a redox catalyst composed of an inorganic radical generator such as potassium persulfate and a reducing agent, and a chain transfer agent is added in batches during the polymerization without initially adding a chain transfer agent, and emulsion polymerization is carried out until the polymerization conversion rate reaches 90% by weight or more. As a result, in the absolute molecular weight and absolute molecular weight distribution of the manufactured acrylic rubber measured by GPC, a high molecular weight component and a low molecular weight component can be generated, and the molecular weight distribution can be broadened while maintaining a high molecular weight, so that the roll processability, crosslinking properties, strength characteristics and compression set resistance of the acrylic rubber are highly balanced.
[0029] Furthermore, the present inventors have found that by specifying the number of batch post-additions of chain transfer, the post-addition period, the post-addition amount, the type of chain transfer agent, the type of reducing agent, not only the initial addition of the reducing agent but also batch post-addition, the quantitative ratio of the initial and post-addition reducing agents, and the polymerization temperature, an acrylic rubber having a better balance in roll processability, strength characteristics, water resistance, and compression set resistance can be produced.
[0030] The present inventors have further discovered that, when the emulsion polymerized liquid to which the chain transfer agent is added in batches is coagulated and dried, by using a specific extrusion dryer to melt-knead and dry the acrylic rubber under high shear conditions, an acrylic rubber having further improved roll processability, short-time crosslinking properties, strength characteristics and compression set resistance can be produced.
[0031] The inventors have further found that in the rubber composition comprising the acrylic rubber or acrylic rubber molded body of the present invention, a filler and a crosslinking agent, by adding carbon black and silica as fillers, the roll processability, Banbury processability and short-time crosslinking property are excellent, and the strength characteristics and compression set resistance of the crosslinked product are highly excellent, and the water resistance is also excellent. In addition, the inventors have also found that by using an organic compound, a polyvalent compound or an ionic crosslinking compound as a crosslinking agent, for example, a polyvalent ionic organic compound having a plurality of ionic reactive groups such as amine groups, epoxy groups, carboxyl groups or thiol groups that react with the ionic reactive groups of the acrylic rubber, the roll processability, Banbury processability and short-time crosslinking property can be excellent, and the strength characteristics and compression set resistance of the crosslinked product are highly excellent, and the water resistance is also excellent.
[0032] The present inventors have completed the present invention based on these findings.
[0033] As described above, according to the present invention, there is provided an acrylic rubber comprising a bonding unit derived from a (meth)acrylic acid ester, a bonding unit derived from an ion-reactive group-containing monomer, and a bonding unit derived from other monomers used as required, wherein the (meth)acrylic acid ester is at least one selected from a (meth)acrylic acid alkyl ester and a (meth)acrylic acid alkoxyalkyl ester, and the acrylic rubber has a weight average molecular weight (Mw) in the range of 1,000,000 to 3,500,000, a z average molecular weight (Mz) in the range of 1,500,000 to 6,000,000, and a ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) in the range of 3.7 to 6.5, based on the absolute molecular weight and the absolute molecular weight distribution measured by the GPC-MALS method.
[0034] In the acrylic rubber of the present invention, it is preferred that the measurement solvent of the GPC-MALS method is a dimethylformamide-based solvent.
[0035] In the acrylic rubber of the present invention, the ion-reactive group content is preferably in the range of 0.001 to 5% by weight.
[0036] In the acrylic rubber of the present invention, the monomer composition of the acrylic rubber is preferably composed of 50 to 99.99 wt % of bonding units derived from (meth)acrylate, 0.01 to 10 wt % of bonding units derived from ion reactive group-containing monomers, and 0 to 40 wt % of bonding units derived from other monomers, wherein the (meth)acrylate is selected from at least one of alkyl (meth)acrylate and alkoxyalkyl (meth)acrylate.
[0037] In the acrylic rubber of the present invention, the ion-reactive group is preferably at least one functional group selected from a carboxyl group, an epoxy group and a chlorine atom, and the ion-reactive group is particularly preferably a carboxyl group or an epoxy group.
[0038] In the acrylic rubber of the present invention, the ratio (Mz / Mw) of the z-average molecular weight (Mz) to the weight-average molecular weight (Mw) is preferably in the range of 1.3 to 3.
[0039] In the acrylic rubber of the present invention, the amount of methyl ethyl ketone insoluble components is preferably 15% by weight or less.
[0040] In the acrylic rubber of the present invention, the ash content is preferably 0.5% by weight or less.
[0041] In the acrylic rubber of the present invention, the total amount of sodium, magnesium, calcium, phosphorus and sulfur in the ash is preferably 50% by weight or more.
[0042] In the acrylic rubber of the present invention, it is preferred that the complex viscosity at 60°C ([η]60°C) is 15000 [Pa·s] or less.
[0043] In the acrylic rubber of the present invention, it is preferred that the complex viscosity at 100°C ([η]100°C) is 2000 [Pa·s] or more.
[0044] In the acrylic rubber of the present invention, the ratio of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) ([η]100°C / [η]60°C) is preferably 0.5 or more, and the ratio of the complex viscosity at 100°C ([η]100°C) to the complex viscosity ([η]60°C) ([η]100°C / [η]60°C) is particularly preferably 0.8 or more.
[0045] In the acrylic rubber of the present invention, the water content is preferably less than 1% by weight.
[0046] In the acrylic rubber of the present invention, the pH is preferably 6 or less.
[0047] In addition, the acrylic rubber of the present invention is preferably obtained by emulsion polymerization using a phosphate salt or a sulfate salt as an emulsifier, and is preferably obtained by coagulating and drying a polymer solution obtained by emulsion polymerization using an alkali metal salt or a metal salt of Group 2 of the periodic table as a coagulant. In addition, the acrylic rubber of the present invention is preferably obtained by melt-kneading and drying after coagulation, and the melt-kneading and drying are preferably carried out in a state that substantially does not contain water, and the melt-kneading and drying are preferably carried out under reduced pressure. Furthermore, the acrylic rubber of the present invention is preferably obtained by cooling at a cooling rate of 40°C / hour or more after the melt-kneading and drying.
[0048] In addition, according to the present invention, there is provided a method for producing acrylic rubber, comprising the following steps: a step of emulsifying a monomer component comprising a (meth)acrylate, an ion-reactive group-containing monomer, and other copolymerizable monomers used as required, with water and an emulsifier, wherein the (meth)acrylate is selected from at least one of an alkyl (meth)acrylate and an alkoxyalkyl (meth)acrylate; a step of performing emulsion polymerization in the presence of a redox catalyst composed of an inorganic free radical generator and a reducing agent until the polymerization conversion rate reaches 90% by weight or more; and a step of post-adding a chain transfer agent in batches during the polymerization.
[0049] The method for producing an acrylic rubber of the present invention preferably produces the above-mentioned acrylic rubber.
[0050] In the method for producing the acrylic rubber of the present invention, the chain transfer agent is preferably post-added in batches within a range of 1 to 5 times.
[0051] In the method for producing the acrylic rubber of the present invention, it is preferred that the batchwise post-addition of the chain transfer agent be started at least 30 minutes after the initiation of polymerization.
[0052] In the method for producing the acrylic rubber of the present invention, the amount of the chain transfer agent added once in batches is preferably in the range of 0.00005 to 0.5 parts by weight relative to 100 parts by weight of the monomer component.
[0053] In the method for producing an acrylic rubber of the present invention, the chain transfer agent is preferably a thiol compound.
[0054] In the method for producing the acrylic rubber of the present invention, the chain transfer agent is preferably an alkyl mercaptan compound having 2 to 20 carbon atoms, and the chain transfer agent is preferably an n-alkyl mercaptan compound.
[0055] In the method for producing acrylic rubber of the present invention, the reducing agent is preferably composed of a combination of at least two reducing agents.
[0056] In the method for producing acrylic rubber of the present invention, the reducing agent preferably contains ferrous sulfate.
[0057] In the method for producing acrylic rubber of the present invention, the reducing agent is preferably ascorbic acid or a salt thereof.
[0058] In the method for producing the acrylic rubber of the present invention, it is preferred to add a reducing agent post-polymerization.
[0059] In the method for producing acrylic rubber of the present invention, post-addition of the reducing agent is preferably performed in batches.
[0060] In the method for producing acrylic rubber of the present invention, the reducing agent to be added later is preferably ascorbic acid or a salt thereof.
[0061] In the method for producing acrylic rubber of the present invention, the ratio of the amount of ascorbic acid or its salt initially added to the amount of ascorbic acid or its salt subsequently added is preferably in the range of 1 / 9 to 8 / 2 in terms of the weight ratio of "ascorbic acid or its salt initially added" / "ascorbic acid or its salt subsequently added in batches".
[0062] In the method for producing acrylic rubber of the present invention, the temperature of the emulsion polymerization is preferably controlled to 35° C. or less.
[0063] In the method for producing the acrylic rubber of the present invention, it is preferred that the emulsion polymerization be performed using a phosphate ester salt or a sulfate ester salt as an emulsifier in the emulsion polymerization step.
[0064] In the method for producing acrylic rubber of the present invention, the polymerization solution produced in the emulsion polymerization step is brought into contact with a coagulant containing an alkali metal salt or a salt of a metal of Group 2 of the periodic table to coagulate the polymerization solution.
[0065] In the method for producing acrylic rubber of the present invention, the polymerization solution produced in the emulsion polymerization step is preferably coagulated by adding the polymerization solution to an aqueous solution containing a coagulant and stirring the solution. The coagulant contains an alkali metal salt or a metal salt of Group 2 of the periodic table.
[0066] In the method for producing the acrylic rubber of the present invention, the acrylic rubber is preferably produced by coagulating and drying the acrylic rubber after emulsion polymerization.
[0067] In the method for producing the acrylic rubber of the present invention, it is preferred that the polymerization solution generated in the emulsion polymerization step is brought into contact with a coagulant to be coagulated, and then melt-kneaded and dried.
[0068] In the method for producing the acrylic rubber of the present invention, the melt-kneading and drying are preferably performed in a state where the mixture contains substantially no water.
[0069] In the method for producing the acrylic rubber of the present invention, the melt-kneading and drying are preferably performed under reduced pressure.
[0070] In the method for producing acrylic rubber of the present invention, the melt-kneading and drying are preferably performed by a screw-type twin-screw extruder dryer.
[0071] In the method for producing acrylic rubber of the present invention, it is preferred that the maximum torque of the screw-type twin-screw extruder dryer during melt-kneading and drying is 30 N·m or more.
[0072] In the method for producing acrylic rubber of the present invention, the specific energy consumption (specific energy) of the screw-type twin-shaft extrusion dryer during melt kneading and drying is preferably in the range of 0.1 to 0.25 [kw·h / kg], and the specific power of the screw-type twin-shaft extrusion dryer is particularly preferably in the range of 0.2 to 0.6 [A·h / kg].
[0073] In the method for producing acrylic rubber of the present invention, the shear rate of a screw-type biaxial extruder dryer during melt kneading and drying is preferably in the range of 40 to 150 [1 / s].
[0074] In the method for producing acrylic rubber of the present invention, the shear viscosity of the acrylic rubber in the screw-type biaxial extruder dryer during melt kneading and drying is preferably in the range of 4000 to 8000 [Pa·s].
[0075] In the method for producing the acrylic rubber of the present invention, the acrylic rubber after melt-kneading and drying is preferably cooled at a cooling rate of 40° C. / hour or more.
[0076] According to the present invention, there is also provided an acrylic rubber molded product obtained by molding the acrylic rubber.
[0077] In the acrylic rubber molded product of the present invention, the acrylic rubber molded product is preferably an acrylic rubber sheet or an acrylic rubber package.
[0078] In the acrylic rubber molded article of the present invention, the specific gravity is preferably 0.8 or more.
[0079] According to the present invention, there is also provided a rubber composition comprising a rubber component, a filler and a cross-linking agent, wherein the rubber component comprises the acrylic rubber or the acrylic rubber molded product.
[0080] In the rubber composition of the present invention, the filler is preferably a reinforcing filler. In addition, in the rubber composition of the present invention, the filler is preferably carbon black. In addition, in the rubber composition of the present invention, the filler is preferably silica.
[0081] In the rubber composition of the present invention, it is preferred that the crosslinking agent is an organic crosslinking agent. In addition, in the rubber composition of the present invention, it is preferred that the crosslinking agent is a polyvalent compound. In addition, in the rubber composition of the present invention, it is preferred that the crosslinking agent is an ionic crosslinking compound, and it is further preferred that the crosslinking agent is an ionic crosslinking organic compound or a polyvalent ionic organic compound.
[0082] In the rubber composition of the present invention, the ion of the ion-crosslinkable compound, ion-crosslinkable organic compound or polyionic organic compound as the crosslinking agent is preferably at least one ion-reactive group selected from amino, epoxy, carboxyl and thiol groups.
[0083] In the rubber composition of the present invention, the crosslinking agent is preferably at least one polyvalent ionic compound selected from the group consisting of polyvalent amine compounds, polyvalent epoxy compounds, polyvalent carboxylic acid compounds and polyvalent thiol compounds.
[0084] In the rubber composition of the present invention, the content of the cross-linking agent is preferably in the range of 0.001 to 20 parts by weight relative to 100 parts by weight of the rubber component.
[0085] The rubber composition of the present invention preferably further comprises an antioxidant. In the rubber composition of the present invention, the antioxidant is preferably an amine antioxidant.
[0086] According to the present invention, there is also provided a method for producing a rubber composition, comprising mixing a rubber component including the acrylic rubber or the acrylic rubber molded product, a filler, and an antioxidant as needed, and then mixing a crosslinking agent.
[0087] According to the present invention, a cross-linked rubber product obtained by cross-linking the rubber composition can also be provided. In the cross-linked rubber product of the present invention, the cross-linking of the rubber composition is preferably performed after molding. In addition, in the cross-linked rubber product of the present invention, the cross-linking of the rubber composition is preferably performed by primary cross-linking and secondary cross-linking.
[0088] Effects of the Invention
[0089] According to the present invention, there can be provided an acrylic rubber having excellent roll processability and short-time crosslinking property and highly excellent strength characteristics and compression set resistance of a crosslinked product, an efficient production method thereof, an acrylic rubber molded product obtained by molding the acrylic rubber, a high-quality rubber composition containing the acrylic rubber, and a rubber crosslinked product obtained by crosslinking the acrylic rubber. BRIEF DESCRIPTION OF THE DRAWINGS
[0090] Figure 1 This is a diagram schematically showing an example of an acrylic rubber production system for producing the acrylic rubber according to one embodiment of the present invention.
[0091] Figure 2 To show Figure 1 Diagram of the structure of the screw type twin-shaft extrusion dryer.
[0092] Figure 3 To illustrate the use of Figure 1 Diagram of the structure of the transport type cooling device of the cooling device. DETAILED DESCRIPTION
[0093] The acrylic rubber of the present invention is characterized in that it is composed of a binding unit from a (meth)acrylate, a binding unit from an ion-reactive group-containing monomer, and a binding unit from other monomers used as needed, the (meth)acrylate being selected from at least one of an alkyl (meth)acrylate and an alkoxyalkyl (meth)acrylate, and the weight average molecular weight (Mw) of the acrylic rubber is in the range of 1,000,000 to 3,500,000, the z average molecular weight (Mz) is in the range of 1,500,000 to 6,000,000, and the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is in the range of 3.7 to 6.5 based on the absolute molecular weight and absolute molecular weight distribution measured by the GPC-MALS method. Here, the "GPC-MALS method" refers to the following. The GPC (gel permeation chromatography) method is a liquid chromatography that separates based on the difference in molecular size. The "GPC-MALS method" is as follows: by installing a multi-angle laser scattering instrument (MALS) and a differential refractometer (RI) in the device, the light scattering intensity and refractive index difference of the molecular chain solution whose size has been differentiated by the GPC device are measured according to the dissolution time, and the molecular weight and content of the solute are calculated in turn, and finally the absolute molecular weight distribution and absolute average molecular weight value of the polymer substance are obtained.
[0094] <Monomer ingredients>
[0095] The acrylic rubber of the present invention is a polymer containing a bonding unit composed of at least one (meth)acrylate selected from alkyl (meth)acrylates and alkoxyalkyl (meth)acrylates, an ion reactive group-containing monomer, and other copolymerizable monomers used as required. In addition, in the present invention, "(meth)acrylate" is used as a term to collectively refer to esters of acrylic acid and / or methacrylic acid.
[0096] The alkyl (meth)acrylate is not particularly limited, but generally, an alkyl (meth)acrylate having an alkyl group having 1 to 12 carbon atoms is used, preferably an alkyl (meth)acrylate having an alkyl group having 1 to 8 carbon atoms is used, and more preferably an alkyl (meth)acrylate having an alkyl group having 2 to 6 carbon atoms is used.
[0097] Specific examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate. Among these, ethyl (meth)acrylate and n-butyl (meth)acrylate are preferred, and ethyl acrylate and n-butyl acrylate are more preferred.
[0098] The alkoxyalkyl (meth)acrylate is not particularly limited, but generally, an alkoxyalkyl (meth)acrylate having an alkoxyalkyl group having 2 to 12 carbon atoms is used, preferably an alkoxyalkyl (meth)acrylate having an alkoxyalkyl group having 2 to 8 carbon atoms is used, and more preferably an alkoxyalkyl (meth)acrylate having an alkoxyalkyl group having 2 to 6 carbon atoms is used.
[0099] Specific examples of the alkoxyalkyl (meth)acrylate include methoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, methoxypropyl (meth)acrylate, methoxybutyl (meth)acrylate, ethoxymethyl (meth)acrylate, ethoxyethyl (meth)acrylate, propoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, etc. Among these, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, etc. are preferred, and methoxyethyl acrylate and ethoxyethyl acrylate are more preferred.
[0100] At least one (meth)acrylate selected from these alkyl (meth)acrylates and alkoxyalkyl (meth)acrylates can be used alone or in combination of two or more. Their proportion in all monomer components is usually in the range of 50 to 99.99% by weight, preferably in the range of 62 to 99.95% by weight, more preferably in the range of 74 to 99.9% by weight, particularly preferably in the range of 80 to 99.5% by weight, and most preferably in the range of 87 to 99% by weight. In this case, the acrylic rubber has highly excellent weather resistance, heat resistance and oil resistance, so it is preferred.
[0101] The ion-reactive group-containing monomer is not particularly limited as long as it is a monomer having a functional group participating in an ion reaction, and can be appropriately selected according to the intended use. Generally, monomers having at least one functional group selected from a carboxyl group, an epoxy group, and a chlorine atom are mentioned. Preferred are monomers having a carboxyl group and an epoxy group, and more preferably a monomer having a carboxyl group. In this case, the short-term crosslinking property and the compression set resistance and water resistance of the crosslinked product can be highly improved, so it is preferred.
[0102] The monomer having a carboxyl group is not particularly limited, and preferably an ethylenically unsaturated carboxylic acid can be used. Examples of the ethylenically unsaturated carboxylic acid include ethylenically unsaturated monocarboxylic acids, ethylenically unsaturated dicarboxylic acids, and ethylenically unsaturated dicarboxylic acid monoesters. Among these, ethylenically unsaturated dicarboxylic acid monoesters are particularly preferred because they can further improve the compression set resistance when the acrylic rubber is made into a rubber cross-linked product.
[0103] The ethylenically unsaturated monocarboxylic acid is not particularly limited, but is preferably an ethylenically unsaturated monocarboxylic acid having 3 to 12 carbon atoms, and examples thereof include acrylic acid, methacrylic acid, α-ethylacrylic acid, crotonic acid, and cinnamic acid.
[0104] The ethylenically unsaturated dicarboxylic acid is not particularly limited, but preferably has 4 to 12 carbon atoms, and examples thereof include fumaric acid, maleic acid and other butenedioic acids, itaconic acid, citraconic acid, etc. The ethylenically unsaturated dicarboxylic acid also includes an ethylenically unsaturated dicarboxylic acid in the form of anhydride.
[0105] The above-mentioned ethylenically unsaturated dicarboxylic acid monoester is not particularly limited, and generally includes alkyl monoesters of ethylenically unsaturated dicarboxylic acids having 4 to 12 carbon atoms and having 1 to 12 carbon atoms, preferably alkyl monoesters of ethylenically unsaturated dicarboxylic acids having 4 to 6 carbon atoms and having 2 to 8 carbon atoms, and more preferably alkyl monoesters of butenedioic acid having 4 carbon atoms and having 2 to 6 carbon atoms.
[0106] Specific examples of ethylenically unsaturated dicarboxylic acid monoesters include: monoalkyl butenedioates such as monomethyl fumarate, monoethyl fumarate, monon-butyl fumarate, monomethyl maleate, monoethyl maleate, monon-butyl maleate, monocyclopentyl fumarate, monocyclohexyl fumarate, monocyclohexenyl fumarate, monocyclopentyl maleate, and monocyclohexyl maleate; and monoalkyl itaconates such as monomethyl itaconate, monoethyl itaconate, monon-butyl itaconate, and monocyclohexyl itaconate. Among these, monon-butyl fumarate and monon-butyl maleate are preferred, and monon-butyl fumarate is particularly preferred.
[0107] Examples of the monomer having an epoxy group include epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate; and epoxy group-containing vinyl ethers such as allyl glycidyl ether and vinyl glycidyl ether.
[0108] The monomer having a chlorine atom is not particularly limited, and examples thereof include unsaturated alcohol esters of chlorine-containing saturated carboxylic acids, chloroalkyl (meth)acrylates, chloroacyloxyalkyl (meth)acrylates, (chloroacetylcarbamoyloxy)alkyl (meth)acrylates, chlorine-containing unsaturated ethers, chlorine-containing unsaturated ketones, chlorine-containing methyl aromatic vinyl compounds, chlorine-containing unsaturated amides, chlorine-containing acetyl unsaturated monomers, and the like.
[0109] Specific examples of unsaturated alcohol esters of chlorine-containing saturated carboxylic acids include vinyl chloroacetate, vinyl 2-chloropropionate, and allyl chloroacetate. Specific examples of chloroalkyl (meth)acrylates include chloromethyl (meth)acrylate, 1-chloroethyl (meth)acrylate, 2-chloroethyl (meth)acrylate, 1,2-dichloroethyl (meth)acrylate, 2-chloropropyl (meth)acrylate, 3-chloropropyl (meth)acrylate, and 2,3-dichloropropyl (meth)acrylate. Specific examples of chloroacyloxyalkyl (meth)acrylates include 2-(chloroacetoxy)ethyl (meth)acrylate, 2-(chloroacetoxy)propyl (meth)acrylate, 3-(chloroacetoxy)propyl (meth)acrylate, and 3-(hydroxychloroacetoxy)propyl (meth)acrylate. Examples of (meth)acrylic acid (chloroacetylcarbamoyloxy)alkyl esters include 2-(chloroacetylcarbamoyloxy)ethyl (meth)acrylate and 3-(chloroacetylcarbamoyloxy)propyl (meth)acrylate. Specific examples of chlorine-containing unsaturated ethers include chloromethyl vinyl ether, 2-chloroethyl vinyl ether, 3-chloropropyl vinyl ether, 2-chloroethyl allyl ether, and 3-chloropropyl allyl ether. Specific examples of chlorine-containing unsaturated ketones include 2-chloroethyl vinyl ketone, 3-chloropropyl vinyl ketone, and 2-chloroethyl allyl ketone. Specific examples of chloromethyl-containing aromatic vinyl compounds include p-chloromethylstyrene, m-chloromethylstyrene, o-chloromethylstyrene, and p-chloromethyl-α-methylstyrene. Specific examples of chlorine-containing unsaturated amides include N-chloromethyl (meth)acrylamide. Specific examples of the chloroacetyl group-containing unsaturated monomer include 3-(hydroxychloroacetyloxy)propyl allyl ether and p-vinylbenzyl chloroacetate.
[0110] These ion-reactive group-containing monomers can be used alone or in combination of two or more, and their proportion in the total monomer components is usually in the range of 0.01 to 10% by weight, preferably in the range of 0.05 to 8% by weight, more preferably in the range of 0.1 to 6% by weight, particularly preferably in the range of 0.5 to 5% by weight, and most preferably in the range of 1 to 3% by weight.
[0111] Monomers other than the above monomers that can be used together with the above monomers as needed (referred to as "other monomers" in the present invention) are not particularly limited as long as they can be copolymerized with the above monomers, and examples thereof include aromatic vinyls such as styrene, α-methylstyrene, and divinylbenzene; ethylenically unsaturated nitriles such as acrylonitrile and methacrylonitrile; acrylamide-based monomers such as acrylamide and methacrylamide; olefin-based monomers such as ethylene, propylene, vinyl acetate, ethyl vinyl ether, and butyl vinyl ether, etc.
[0112] These other monomers can be used alone or in combination of two or more, and their proportion in the total monomer components is usually controlled in the range of 0 to 40% by weight, preferably in the range of 0 to 30% by weight, more preferably in the range of 0 to 20% by weight, particularly preferably in the range of 0 to 15% by weight, and most preferably in the range of 0 to 10% by weight.
[0113] <Acrylic rubber>
[0114] The acrylic rubber of the present invention is composed of a bonding unit derived from at least one (meth)acrylate selected from the above-mentioned alkyl (meth)acrylates and alkoxyalkyl (meth)acrylates, an ion reactive group-containing monomer, and other monomers contained as required, and the proportions of each of these monomers in the acrylic rubber are as follows: the bonding unit derived from at least one (meth)acrylate selected from the above-mentioned alkyl (meth)acrylates and alkoxyalkyl (meth)acrylates is usually in the range of 50 to 99.99% by weight, preferably in the range of 62 to 99.95% by weight, more preferably in the range of 74 to 99.9% by weight, and particularly preferably in the range of 8 The range of 0 to 99.5% by weight is preferred, and the range of 87 to 99% by weight is the most preferred. The binding unit derived from the monomer containing the ion reactive group is usually in the range of 0.01 to 10% by weight, preferably in the range of 0.05 to 8% by weight, more preferably in the range of 0.1 to 6% by weight, particularly preferably in the range of 0.5 to 5% by weight, and most preferably in the range of 1 to 3% by weight. The binding unit derived from other monomers is usually in the range of 0 to 40% by weight, preferably in the range of 0 to 30% by weight, more preferably in the range of 0 to 20% by weight, particularly preferably in the range of 0 to 15% by weight, and most preferably in the range of 0 to 10% by weight. When the monomer composition of the acrylic rubber is in this range, the characteristics such as short-term crosslinking, compression set resistance, weather resistance, heat resistance, and oil resistance are highly balanced, so it is preferred.
[0115] The content of the ionic reactive group of the acrylic rubber of the present invention is not particularly limited and can be appropriately selected according to the purpose of use. The weight ratio of the ionic reactive group itself is usually in the range of 0.001 to 5% by weight, preferably in the range of 0.01 to 3% by weight, more preferably in the range of 0.05 to 1% by weight, and particularly preferably in the range of 0.1 to 0.5% by weight. In this case, the processability, crosslinking, and the strength characteristics when the crosslinked product is made, the compression set resistance, oil resistance, cold resistance, and water resistance are highly balanced, so it is preferred. In addition, the ionic reactive group is preferably at least one functional group selected from a carboxyl group, an epoxy group, and a chlorine atom, more preferably an epoxy group or a carboxyl group, and particularly preferably a carboxyl group, as in the ionic reactive group of the above-mentioned ionic reactive group-containing monomer.
[0116] The measuring solvent of the GPC-MALS method for measuring the absolute molecular weight and absolute molecular weight distribution of the acrylic rubber of the present invention is not particularly limited as long as it is a solvent that can dissolve and measure the acrylic rubber of the present invention, and is preferably a dimethylformamide-based solvent. The dimethylformamide-based solvent used is not particularly limited as long as it is dimethylformamide as the main component, and can be 100% dimethylformamide or the proportion of dimethylformamide in the dimethylformamide-based solvent is 90% by weight, preferably 95% by weight, and more preferably 97% by weight or more. The compound added to dimethylformamide is not particularly limited, and in the present invention, it is particularly preferred to add lithium chloride at a concentration of 0.05 mol / L and a solution of 37% concentrated hydrochloric acid at a concentration of 0.01% to dimethylformamide.
[0117] The weight average molecular weight (Mw) of the acrylic rubber of the present invention is in the range of 1,000,000 to 3,500,000, preferably in the range of 1,200,000 to 3,000,000, more preferably in the range of 1,300,000 to 3,000,000, particularly preferably in the range of 1,500,000 to 2,500,000, and most preferably in the range of 1,900,000 to 2,100,000. In this case, the roll processability, strength characteristics, and compression set resistance of the acrylic rubber are highly balanced, so it is preferred. When the weight average molecular weight (Mw) of the acrylic rubber of the present invention is too small, the strength characteristics and compression set resistance are poor. On the contrary, when it is too large, the roll processability, Banbury processability, injection moldability, etc. are poor, which is not preferred.
[0118] The number average molecular weight (Mn) of the acrylic rubber of the present invention is not particularly limited and can be appropriately selected according to the purpose of use. In terms of absolute molecular weight measured by the GPC-MALS method, it is usually in the range of 100,000 to 500,000, preferably in the range of 200,000 to 480,000, more preferably in the range of 250,000 to 450,000, particularly preferably in the range of 300,000 to 400,000, and most preferably in the range of 350,000 to 400,000. In this case, the roll processability, strength characteristics and compression set resistance of the acrylic rubber are highly balanced, so it is preferred. When the number average molecular weight (Mn) of the acrylic rubber of the present invention is too small, the strength characteristics and compression set resistance are poor. On the contrary, when it is too large, the roll processability, Banbury processability, injection moldability, etc. are poor, which is not preferred.
[0119] The z-average molecular weight (Mz) of the acrylic rubber of the present invention is in the range of 1,500,000 to 6,000,000, preferably in the range of 2,000,000 to 5,000,000, more preferably in the range of 2,500,000 to 4,500,000, and particularly preferably in the range of 3,000,000 to 4,000,000, in which case the roll processability, strength characteristics, and compression set resistance of the acrylic rubber are highly balanced, which is preferred.
[0120] The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the acrylic rubber of the present invention is in the range of 3.7 to 6.5, preferably in the range of 3.8 to 6.2, more preferably in the range of 4 to 6, particularly preferably in the range of 4.5 to 5.7, and most preferably in the range of 4.7 to 5.5, in which case roll processability, strength characteristics during crosslinking, and compression set resistance are highly balanced, so it is preferred. When the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the acrylic rubber of the present invention is too small, roll processability is poor, and when it is too large, strength characteristics and compression set resistance are poor, and roll processability is also insufficient, both of which are not preferred.
[0121] The ratio (Mz / Mw) of the z-average molecular weight (Mz) to the weight-average molecular weight (Mw) of the acrylic rubber of the present invention is not particularly limited and may be appropriately selected depending on the intended use. In terms of absolute molecular weight distribution in the polymer region measured by the GPC-MALS method, the ratio is usually in the range of 1.3 to 3, preferably in the range of 1.4 to 2.7, more preferably in the range of 1.5 to 2.5, particularly preferably in the range of 1.8 to 2, and most preferably in the range of 1.8 to 1.95. In this case, the processability and strength characteristics of the acrylic rubber are highly balanced, and changes in physical properties during storage can be mitigated, which is preferred.
[0122] The ash content of the acrylic rubber of the present invention is not particularly limited and may be appropriately selected depending on the intended use. It is usually 0.5 wt % or less, preferably 0.3 wt % or less, more preferably 0.2 wt % or less, particularly preferably 0.15 wt % or less, and most preferably 0.13 wt % or less. When it is within this range, the water resistance, strength characteristics and processability of the acrylic rubber are highly balanced, so it is preferred.
[0123] The lower limit of the ash content of the acrylic rubber of the present invention is not particularly limited and may be appropriately selected depending on the intended use. It is usually 0.0001 wt % or more, preferably 0.0005 wt % or more, more preferably 0.001 wt % or more, particularly preferably 0.005 wt % or more, and most preferably 0.01 wt % or more. In this case, the metal adhesion of the rubber is reduced and the handleability is excellent, which is preferred.
[0124] The ash content when the water resistance, strength characteristics, processability and handling properties of the acrylic rubber of the present invention are highly balanced is usually in the range of 0.0001 to 0.5% by weight, preferably in the range of 0.0005 to 0.3% by weight, more preferably in the range of 0.001 to 0.2% by weight, particularly preferably in the range of 0.005 to 0.15% by weight, and most preferably in the range of 0.01 to 0.13% by weight.
[0125] The total amount of sodium, magnesium, calcium, phosphorus and sulfur in the ash of the acrylic rubber of the present invention is not particularly limited and can be appropriately selected according to the purpose of use. It is usually 50% by weight or more, preferably 60% by weight or more, more preferably 70% by weight or more, particularly preferably 80% by weight or more, and most preferably 90% by weight or more. In this case, the water resistance of the acrylic rubber can be highly improved, which is preferred. In addition, when the total amount of sodium, magnesium, calcium, phosphorus and sulfur in the ash of the acrylic rubber of the present invention is within this range, metal adhesion is reduced and the workability is excellent, which is preferred.
[0126] The total amount of magnesium and phosphorus in the ash of the acrylic rubber of the present invention is not particularly limited and can be appropriately selected according to the purpose of use. It is usually 30% by weight or more, preferably 50% by weight or more, more preferably 70% by weight or more, particularly preferably 80% by weight or more, and most preferably 90% by weight or more. In this case, the water resistance, strength characteristics and processability of the acrylic rubber are highly balanced, so it is preferred. In addition, when the total amount of magnesium and phosphorus in the ash of the acrylic rubber of the present invention is within this range, metal adhesion is reduced and the workability is excellent, so it is preferred.
[0127] The amount of magnesium in the ash of the acrylic rubber of the present invention is not particularly limited and can be appropriately selected according to the intended use. It is usually 10% by weight or more, preferably in the range of 15 to 60% by weight, more preferably in the range of 20 to 50% by weight, particularly preferably in the range of 25 to 45% by weight, and most preferably in the range of 30 to 40% by weight.
[0128] The phosphorus content in the ash of the acrylic rubber of the present invention is not particularly limited and can be appropriately selected depending on the intended use. It is usually 10% by weight or more, preferably in the range of 20 to 90% by weight, more preferably in the range of 30 to 80% by weight, particularly preferably in the range of 40 to 70% by weight, and most preferably in the range of 50 to 60% by weight.
[0129] The ratio of magnesium to phosphorus ([Mg] / [P]) in the ash of the acrylic rubber of the present invention is not particularly limited and may be appropriately selected depending on the intended use. In terms of weight ratio, it is usually in the range of 0.4 to 2.5, preferably in the range of 0.45 to 1.2, more preferably in the range of 0.45 to 1, particularly preferably in the range of 0.5 to 0.8, and most preferably in the range of 0.55 to 0.7. In this case, the water resistance, strength characteristics and processability of the acrylic rubber are highly balanced, which is preferred.
[0130] Here, the ash content in acrylic rubber mainly comes from the emulsifier used when emulsifying the monomer components for emulsion polymerization and the coagulant used when coagulating the emulsion polymerization solution. The total ash content, the magnesium and phosphorus contents in the ash, etc. vary not only depending on the conditions of the emulsion polymerization process and the coagulation process, but also depending on the various conditions of the subsequent processes.
[0131] When an anionic emulsifier, a cationic emulsifier or a nonionic emulsifier, preferably an anionic emulsifier, more preferably a phosphate ester salt or a sulfate ester salt is used as an emulsifier in the emulsion polymerization described later, the acrylic rubber of the present invention can highly improve the mold release and processability of the acrylic rubber in addition to the water resistance and strength characteristics, so it is preferred. The water resistance of the acrylic rubber is mainly related to the ash content in the acrylic rubber and the total amount of sodium, magnesium, calcium, phosphorus and sulfur in the ash, but the use of the above-mentioned emulsifier can make the water resistance, strength characteristics, mold release and processability of the acrylic rubber more highly balanced, so it is preferred.
[0132] When a metal salt, preferably an alkali metal salt or a metal salt of Group 2 of the periodic table, is used as a coagulant described later, the acrylic rubber of the present invention can highly improve the mold release and processability of the acrylic rubber in addition to the water resistance and strength characteristics, so it is preferred. The water resistance of the acrylic rubber is mainly related to the ash content in the acrylic rubber and the total amount of sodium, magnesium, calcium, phosphorus and sulfur in the ash, but the use of the above coagulant can make the water resistance, strength characteristics, mold release and processability of the acrylic rubber more highly balanced, so it is preferred.
[0133] The glass transition temperature (Tg) of the acrylic rubber of the present invention can be appropriately selected according to the purpose of use of the acrylic rubber, and is usually 20°C or less, preferably 10°C or less, and more preferably 0°C or less. In this case, processability and cold resistance are excellent, so it is preferred. The lower limit of the glass transition temperature (Tg) of the acrylic rubber is not particularly limited, but is usually -80°C or more, preferably -60°C or more, and more preferably -40°C or more. By making the glass transition temperature above the lower limit, oil resistance and heat resistance can be made more excellent, and by making it below the upper limit, processability, crosslinking and cold resistance can be made more excellent.
[0134] The complex viscosity ([η]60°C) of the acrylic rubber of the present invention at 60°C is not particularly limited and may be appropriately selected depending on the intended use. It is usually 15,000 [Pa·s] or less, preferably in the range of 1,000 to 10,000 [Pa·s], more preferably in the range of 2,000 to 5,000 [Pa·s], particularly preferably in the range of 2,500 to 4,000 [Pa·s], and most preferably in the range of 2,500 to 3,000 [Pa·s]. In this case, processability, oil resistance and shape retention are excellent, so it is preferred.
[0135] The complex viscosity ([η]100°C) of the acrylic rubber of the present invention at 100°C is not particularly limited and may be appropriately selected depending on the intended use. It is generally in the range of 1500 to 6000 [Pa·s], preferably in the range of 2000 to 5000 [Pa·s], more preferably in the range of 2300 to 4000 [Pa·s], particularly preferably in the range of 2500 to 3500 [Pa·s], and most preferably in the range of 2500 to 3000 [Pa·s]. In this case, processability, oil resistance and shape retention are excellent, so it is preferred.
[0136] The ratio of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) of the acrylic rubber of the present invention ([η]100°C / [η]60°C) is not particularly limited and may be appropriately selected depending on the intended use, and is generally 0.5 or more, preferably 0.6 or more, more preferably 0.7 or more, particularly preferably 0.8 or more, and most preferably 0.83 or more. In addition, the ratio of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) of the acrylic rubber of the present invention ([η]100°C / [η]60°C) is generally in the range of 0.5 to 0.99, preferably in the range of 0.6 to 0.98, more preferably in the range of 0.7 to 0.97, particularly preferably in the range of 0.8 to 0.96, and most preferably in the range of 0.85 to 0.95. In this case, processability, oil resistance, and shape retention are highly balanced, which is preferred.
[0137] The amount of the insoluble components in methyl ethyl ketone of the acrylic rubber of the present invention is not particularly limited and may be appropriately selected depending on the intended use. It is usually 50 wt % or less, preferably 30 wt % or less, more preferably 15 wt % or less, particularly preferably 10 wt % or less, and most preferably 5 wt % or less. In this case, the processability during Banbury kneading is highly improved, which is preferred.
[0138] The acrylic rubber of the present invention is preferably melt-kneaded and dried in a screw-type biaxial extruder dryer in a state where the water-containing pellets produced in the coagulation reaction are substantially free of water, because the Banbury processability and strength characteristics are well balanced.
[0139] The specific gravity of the acrylic rubber of the present invention is not particularly limited, and is usually 0.7 or more, preferably 0.8 or more, more preferably 0.9 or more, particularly preferably 0.95 or more, and most preferably 1 or more. In this case, there is almost no air inside, and the storage stability is excellent, so it is preferred. In addition, the specific gravity of the acrylic rubber of the present invention is usually in the range of 0.7 to 1.6, preferably in the range of 0.8 to 1.5, more preferably in the range of 0.9 to 1.4, particularly preferably in the range of 0.95 to 1.3, and most preferably in the range of 1.0 to 1.2. In this case, the productivity, storage stability, and stability of the crosslinking characteristics of the crosslinked product are highly balanced, so it is preferred. When the specific gravity of the acrylic rubber is too small, it means that there is a large amount of air in the acrylic rubber, which has a significant impact on the storage stability including oxidation degradation, so it is not preferred.
[0140] The specific gravity of the acrylic rubber of the present invention is obtained by dividing the mass by the volume including voids, that is, the mass measured in air by the buoyancy, and is usually measured according to Method A of JIS K6268 Crosslinked Rubber - Density Measurement.
[0141] The acrylic rubber of the present invention is preferably obtained by drying the water-containing pellets generated in the coagulation reaction under reduced pressure in a screw-type twin-screw extruder dryer, or by melt-kneading and drying under reduced pressure, because the storage stability, injection moldability and strength properties are particularly excellent and well-balanced.
[0142] The water content of the acrylic rubber of the present invention is not particularly limited and can be appropriately selected according to the intended use. It is usually less than 1 wt %, preferably 0.8 wt % or less, and more preferably 0.6 wt % or less. In this case, the vulcanization characteristics of the acrylic rubber are optimized, and the properties such as heat resistance and water resistance are highly improved, so it is preferred.
[0143] The pH of the acrylic rubber of the present invention is not particularly limited and may be appropriately selected depending on the intended use. It is usually 6 or less, preferably in the range of 2 to 6, more preferably in the range of 2.5 to 5.5, and most preferably in the range of 3 to 5. In this case, the storage stability of the acrylic rubber is highly improved, which is preferred.
[0144] The Mooney viscosity (ML1+4, 100°C) of the acrylic rubber of the present invention is not particularly limited and may be appropriately selected depending on the intended use. It is generally in the range of 10 to 150, preferably in the range of 20 to 100, and more preferably in the range of 25 to 70. In this case, the processability and strength characteristics of the acrylic rubber are highly balanced, so it is preferred.
[0145] The shape of the acrylic rubber of the present invention is not particularly limited and may be appropriately selected depending on the intended use. For example, the shape may be any of powder, pellet, strand, sheet, and bag.
[0146] <Method for producing acrylic rubber>
[0147] The method for producing the acrylic rubber is not particularly limited, and can be easily produced by, for example, a process comprising: a process of emulsifying a monomer component comprising a (meth)acrylate, an ion-reactive group-containing monomer, and other copolymerizable monomers used as required, with water and an emulsifier, wherein the (meth)acrylate is at least one selected from the group consisting of an alkyl (meth)acrylate and an alkoxyalkyl (meth)acrylate; a process of emulsion polymerization in the presence of a redox catalyst composed of an inorganic free radical generator and a reducing agent until the polymerization conversion rate reaches 90% by weight or more; and a process of post-adding a chain transfer agent in batches during the polymerization.
[0148] (Monomer component)
[0149] The monomer components used in the present invention are the same as the examples and preferred ranges of the monomer components described above. The amounts of the monomer components used are also as described above, and each monomer can be appropriately selected in the emulsion polymerization so as to achieve the above composition of the acrylic rubber of the present invention.
[0150] (Emulsifier)
[0151] The emulsifier used in the present invention is not particularly limited, and examples thereof include anionic emulsifiers, cationic emulsifiers, nonionic emulsifiers, and the like, and an anionic emulsifier is preferred.
[0152] There are no particular limitations on the anionic emulsifiers, and examples thereof include: salts of fatty acids such as myristic acid, palmitic acid, oleic acid, and linolenic acid; alkylbenzene sulfonates such as sodium dodecylbenzene sulfonate; sulfate esters such as sodium lauryl sulfate; phosphate esters such as polyoxyalkylene alkyl ether phosphate esters; alkyl sulfosuccinates, etc. Among these anionic emulsifiers, phosphate ester salts and sulfate ester salts are preferred, phosphate ester salts are particularly preferred, and divalent phosphate ester salts are most preferred. In this case, the water resistance, strength characteristics, metal mold release and processability of the obtained acrylic rubber can be highly balanced, so it is preferred. In addition, as these phosphate ester salts and sulfate ester salts, alkali metal salts of phosphate esters and sulfate esters are preferred, and sodium salts of phosphate esters and sulfate esters are more preferred. In this case, the water resistance, strength characteristics, metal mold release and processability of the obtained acrylic rubber can be highly balanced, so it is preferred.
[0153] The divalent phosphate salt is not particularly limited as long as it can be used as an emulsifier in the emulsion polymerization reaction, and examples thereof include alkoxy polyoxyalkylene phosphate salts, alkyl phenoxy polyoxyalkylene phosphate salts, etc. Among these, their metal salts are preferred, their alkali metal salts are more preferred, and their sodium salts are most preferred.
[0154] Examples of the alkoxy polyoxyalkylene phosphate salt include alkoxy polyoxyethylene phosphate salts and alkoxy polyoxypropylene phosphate salts. Among these, alkoxy polyoxyethylene phosphate salts are preferred.
[0155] Specific examples of the alkoxypolyoxyethylene phosphate salts include octyloxydioxyethylene phosphate, octyloxytrioxyethylene phosphate, octyloxytetraoxyethylene phosphate, decyloxytetraoxyethylene phosphate, dodecyloxytetraoxyethylene phosphate, tridecyloxytetraoxyethylene phosphate, tetradecyloxytetraoxyethylene phosphate, hexadecyloxytetraoxyethylene phosphate, octadecyloxytetraoxyethylene phosphate, octyloxypentaoxyethylene phosphate, decyloxypentaoxyethylene phosphate, dodecyloxypentaoxyethylene phosphate, tridecyloxypentaoxyethylene phosphate, tetradecyloxypentaoxyethylene phosphate, hexadecyloxypentaoxyethylene phosphate, octadecyloxypentaoxyethylene phosphate, Metal salts of pentylene phosphate, octyloxyhexaoxyethylene phosphate, decyloxyhexaoxyethylene phosphate, dodecyloxyhexaoxyethylene phosphate, tridecyloxyhexaoxyethylene phosphate, tetradecyloxyhexaoxyethylene phosphate, hexadecyloxyhexaoxyethylene phosphate, octadecyloxyhexaoxyethylene phosphate, octyloxyoctaoxyethylene phosphate, decyloxyoctaoxyethylene phosphate, dodecyloxyoctaoxyethylene phosphate, tridecyloxyoctaoxyethylene phosphate, tetradecyloxyoctaoxyethylene phosphate, hexadecyloxyoctaoxyethylene phosphate, octadecyloxyoctaoxyethylene phosphate, etc. Among these, alkali metal salts thereof are preferred, and sodium salts are particularly preferred.
[0156] Specific examples of the alkoxypolyoxypropylene phosphate salts include octyloxydipropylene phosphate, octyloxytripropylene phosphate, octyloxytetrapropylene phosphate, decyloxytetrapropylene phosphate, dodecyloxytetrapropylene phosphate, tridecyloxytetrapropylene phosphate, tetradecyloxytetrapropylene phosphate, hexadecyloxytetrapropylene phosphate, octadecyloxytetrapropylene phosphate, octyloxypentapropylene phosphate, decyloxypentapropylene phosphate, dodecyloxypentapropylene phosphate, tridecyloxypentapropylene phosphate, tetradecyloxypentapropylene phosphate, hexadecyloxypentapropylene phosphate, octadecyloxypentapropylene phosphate, Propylene phosphate, octyloxyhexaoxypropylene phosphate, decyloxyhexaoxypropylene phosphate, dodecyloxyhexaoxypropylene phosphate, tridecyloxyhexaoxypropylene phosphate, tetradecyloxyhexaoxypropylene phosphate, hexadecyloxyhexaoxypropylene phosphate, octadecyloxyhexaoxypropylene phosphate, octyloxyoctaoxypropylene phosphate, decyloxyoctaoxypropylene phosphate, dodecyloxyoctaoxypropylene phosphate, tridecyloxyoctaoxypropylene phosphate, tetradecyloxyoctaoxypropylene phosphate, hexadecyloxyoctaoxypropylene phosphate, octadecyloxyoctaoxypropylene phosphate, and metal salts thereof, etc. Among these, alkali metal salts thereof are preferred, and sodium salts are particularly preferred.
[0157] Specific examples of the alkylphenoxy polyoxyalkylene phosphate salt include alkylphenoxy polyoxyethylene phosphate salt and alkylphenoxy polyoxypropylene phosphate salt. Among these, alkylphenoxy polyoxyethylene phosphate salt is preferred.
[0158] Specific examples of the alkylphenoxy polyoxyethylene phosphate salts include methylphenoxy tetraoxyethylene phosphate, ethylphenoxy tetraoxyethylene phosphate, butylphenoxy tetraoxyethylene phosphate, hexylphenoxy tetraoxyethylene phosphate, nonylphenoxy tetraoxyethylene phosphate, dodecylphenoxy tetraoxyethylene phosphate, octadecylphenoxy tetraoxyethylene phosphate, methylphenoxy pentaoxyethylene phosphate, ethylphenoxy pentaoxyethylene phosphate, butylphenoxy pentaoxyethylene phosphate, hexylphenoxy pentaoxyethylene phosphate, nonylphenoxy pentaoxyethylene phosphate, dodecylphenoxy pentaoxyethylene phosphate, Metal salts of vinyl phosphate, methylphenoxy hexaoxyethylene phosphate, ethylphenoxy hexaoxyethylene phosphate, butylphenoxy hexaoxyethylene phosphate, hexylphenoxy hexaoxyethylene phosphate, nonylphenoxy hexaoxyethylene phosphate, dodecylphenoxy hexaoxyethylene phosphate, methylphenoxy hexaoxyethylene phosphate, ethylphenoxy octaoxyethylene phosphate, butylphenoxy octaoxyethylene phosphate, hexylphenoxy octaoxyethylene phosphate, nonylphenoxy octaoxyethylene phosphate, dodecylphenoxy octaoxyethylene phosphate, etc., among which alkali metal salts thereof are preferred, and sodium salts are particularly preferred.
[0159] Specific examples of the alkylphenoxy polyoxypropylene phosphate salts include methylphenoxy tetraoxypropylene phosphate, ethylphenoxy tetraoxypropylene phosphate, butylphenoxy tetraoxypropylene phosphate, hexylphenoxy tetraoxypropylene phosphate, nonylphenoxy tetraoxypropylene phosphate, dodecylphenoxy tetraoxypropylene phosphate, methylphenoxy pentaoxypropylene phosphate, ethylphenoxy pentaoxypropylene phosphate, butylphenoxy pentaoxypropylene phosphate, hexylphenoxy pentaoxypropylene phosphate, nonylphenoxy pentaoxypropylene phosphate, dodecylphenoxy pentaoxypropylene phosphate, methylphenoxy pentaoxypropylene phosphate, ethylphenoxy pentaoxypropylene phosphate, butylphenoxy pentaoxypropylene phosphate, hexylphenoxy pentaoxypropylene phosphate, nonylphenoxy pentaoxypropylene phosphate, dodecylphenoxy pentaoxypropylene phosphate, methylphenoxy polyoxypropylene phosphate Metal salts of phenoxy hexaoxypropylene phosphate, ethyl phenoxy hexaoxypropylene phosphate, butyl phenoxy hexaoxypropylene phosphate, hexyl phenoxy hexaoxypropylene phosphate, nonyl phenoxy hexaoxypropylene phosphate, dodecyl phenoxy hexaoxypropylene phosphate, methyl phenoxy octaoxypropylene phosphate, ethyl phenoxy octaoxypropylene phosphate, butyl phenoxy octaoxypropylene phosphate, hexyl phenoxy octaoxypropylene phosphate, nonyl phenoxy octaoxypropylene phosphate, dodecyl phenoxy octaoxypropylene phosphate, etc., among which alkali metal salts thereof are preferred, and sodium salts are particularly preferred.
[0160] As the phosphoric acid ester salt, a monovalent phosphoric acid ester salt such as a sodium di(alkoxypolyoxyalkylene)phosphate ester salt may be used alone or in combination with a divalent phosphoric acid ester salt.
[0161] Examples of the sulfuric acid ester salt include sodium lauryl sulfate, potassium lauryl sulfate, ammonium lauryl sulfate, sodium myristyl sulfate, sodium polyoxyethylene alkyl sulfate, sodium polyoxyethylene alkylaryl sulfate, and the like, and sodium lauryl sulfate is preferred.
[0162] Examples of the cationic emulsifier include alkyltrimethylammonium chloride, dialkylammonium chloride, and benzylammonium chloride.
[0163] Examples of the nonionic emulsifier include polyoxyalkylene fatty acid esters such as polyoxyethylene stearate; polyoxyalkylene alkyl ethers such as polyoxyethylene lauryl ether; polyoxyalkylene alkylphenol ethers such as polyoxyethylene nonylphenyl ether; polyoxyethylene sorbitan alkyl esters, etc., preferably polyoxyalkylene alkyl ethers and polyoxyalkylene alkylphenol ethers, more preferably polyoxyethylene alkyl ethers and polyoxyethylene alkylphenol ethers.
[0164] These emulsifiers can be used alone or in combination of two or more, and the amount used is usually in the range of 0.01 to 10 parts by weight, preferably 0.1 to 5 parts by weight, more preferably 1 to 3 parts by weight, based on 100 parts by weight of the monomer component.
[0165] The method for mixing the monomer components, water and the emulsifier (mixing method) may be a conventional method, for example, a method of stirring the monomer, emulsifier and water using a homogenizer, a disk turbine or other agitator, etc. The amount of water used is usually in the range of 1 to 1000 parts by weight, preferably in the range of 5 to 500 parts by weight, more preferably in the range of 4 to 300 parts by weight, particularly preferably in the range of 3 to 150 parts by weight, and most preferably in the range of 20 to 80 parts by weight, relative to 100 parts by weight of the monomer components.
[0166] (Inorganic free radical generator)
[0167] The polymerization catalyst used in the present invention is characterized in that a redox catalyst composed of an inorganic radical generator and a reducing agent is used. In particular, the use of an inorganic radical generator is preferred because the processability of a roller or the like of the acrylic rubber to be produced can be greatly improved.
[0168] The inorganic radical generator is not particularly limited as long as it is an inorganic radical generator commonly used in emulsion polymerization, and examples thereof include persulfates such as sodium persulfate, potassium persulfate, and ammonium persulfate, hydrogen peroxide, and the like. Among these, persulfates are preferred, potassium persulfate and ammonium persulfate are more preferred, and potassium persulfate is particularly preferred.
[0169] These inorganic free radical generating agents can be used alone or in combination of two or more, and their usage amount is usually in the range of 0.0001 to 5 parts by weight, preferably in the range of 0.0005 to 1 part by weight, more preferably in the range of 0.001 to 0.25 part by weight, particularly preferably in the range of 0.01 to 0.21 part by weight, and most preferably in the range of 0.1 to 0.2 part by weight, relative to 100 parts by weight of the monomer component.
[0170] (reducing agent)
[0171] The reducing agent used in the present invention is not particularly limited as long as it is a reducing agent commonly used in emulsion polymerization. It is preferred to use at least two reducing agents. Combining a metal ion compound in a reduced state with another reducing agent is preferred because it can further highly balance the Banbury processability, injection moldability and strength characteristics of the acrylic rubber.
[0172] The metal ion compound in a reduced state is not particularly limited, and examples thereof include ferrous sulfate, sodium iron hexamethylenediaminetetraacetate, cuprous cyclopentaneate, etc. Among these, ferrous sulfate is preferred. These metal ion compounds in a reduced state can be used alone or in combination of two or more, and their usage amount is usually in the range of 0.000001 to 0.01 parts by weight, preferably in the range of 0.00001 to 0.001 parts by weight, and more preferably in the range of 0.00005 to 0.0005 parts by weight relative to 100 parts by weight of the monomer component.
[0173] The reducing agent other than the metal ion compound in a reduced state used in the present invention is not particularly limited, and examples thereof include: ascorbic acid or salts thereof such as ascorbic acid, sodium ascorbate, and potassium ascorbate; isoascorbic acid or salts thereof such as isoascorbic acid, sodium isoascorbate, and potassium isoascorbate; sulfinates such as sodium hydroxymethanesulfinate; sulfites such as sodium sulfite, potassium sulfite, sodium hydrogen sulfite, sodium acetaldehyde hydrogen sulfite, and potassium hydrogen sulfite; pyrosulfites such as sodium pyrosulfite, potassium pyrosulfite, sodium hydrogen pyrosulfite, and potassium hydrogen pyrosulfite; thiosulfates such as sodium thiosulfate and potassium thiosulfate; phosphorous acid or salts thereof such as phosphorous acid, sodium phosphite, potassium phosphite, sodium hydrogen phosphite, and potassium hydrogen phosphite; pyrophosphoric acid or salts thereof such as pyrophosphorous acid, sodium pyrophosphite, potassium pyrophosphite, sodium hydrogen pyrophosphite, and potassium hydrogen pyrophosphite; sodium formaldehyde sulfoxylate, and the like. Among these, ascorbic acid or its salt, sodium formaldehyde sulfoxylate and the like are preferred, and ascorbic acid or its salt is particularly preferred.
[0174] These reducing agents other than the metal ion compound in a reduced state can be used alone or in combination of two or more, and their usage amount is usually in the range of 0.001 to 1 part by weight, preferably in the range of 0.005 to 0.5 part by weight, and more preferably in the range of 0.01 to 0.1 part by weight, relative to 100 parts by weight of the monomer component.
[0175] The preferred combination of the metal ion compound in a reduced state and the reducing agent other than this is a combination of ferrous sulfate and ascorbic acid or its salt and / or sodium formaldehyde sulfoxylate, and more preferably a combination of ferrous sulfate and ascorbic acid or its salt. At this time, the amount of ferrous sulfate used is usually in the range of 0.000001 to 0.01 part by weight relative to 100 parts by weight of the monomer component, preferably in the range of 0.00001 to 0.001 part by weight, and more preferably in the range of 0.00005 to 0.0005 part by weight, and the amount of ascorbic acid or its salt and / or sodium formaldehyde sulfoxylate used is usually in the range of 0.001 to 1 part by weight relative to 100 parts by weight of the monomer component, preferably in the range of 0.005 to 0.5 part by weight, and more preferably in the range of 0.01 to 0.1 part by weight.
[0176] The amount of water used in the emulsion polymerization reaction may be only the amount used when the monomer components are emulsified, and can be adjusted to generally be in the range of 10 to 1000 parts by weight, preferably in the range of 50 to 500 parts by weight, more preferably in the range of 80 to 400 parts by weight, and most preferably in the range of 100 to 300 parts by weight, relative to 100 parts by weight of the monomer components used for polymerization.
[0177] The emulsion polymerization reaction can be carried out in a conventional manner, and can be any of batch, semi-batch, and continuous methods. The polymerization temperature and polymerization time are not particularly limited and can be appropriately selected according to the type of polymerization initiator used. The polymerization time is usually 0.5 to 100 hours, preferably 1 to 10 hours.
[0178] Emulsion polymerization is an exothermic reaction. If it is not controlled, the temperature will rise, which can also shorten the polymerization reaction. However, in the present invention, the emulsion polymerization temperature is usually controlled to be below 35°C, preferably controlled to 0-35°C, more preferably controlled to 5-30°C, and particularly preferably controlled to 10-25°C. This can highly balance the strength characteristics of the manufactured acrylic rubber and the processability during Banbury mixing, so it is preferred.
[0179] (Post-addition of chain transfer agent)
[0180] The present invention is characterized in that a chain transfer agent is not added initially, but is added in batches during polymerization. This makes it possible to produce an acrylic rubber in which a high molecular weight component and a low molecular weight component are separated, and the strength characteristics of the produced acrylic rubber and the processability during kneading with a roll are highly balanced, which is preferred.
[0181] The chain transfer agent used is not particularly limited as long as it is a chain transfer agent generally used in emulsion polymerization, and for example, a thiol compound can be preferably used.
[0182] As the thiol compound, an alkylthiol compound having 2 to 20 carbon atoms can be generally used, an alkylthiol compound having 5 to 15 carbon atoms is preferably used, and an alkylthiol compound having 6 to 14 carbon atoms is more preferably used.
[0183] The alkyl mercaptan compound may be any of a normal alkyl mercaptan compound, a secondary alkyl mercaptan compound, and a tertiary alkyl mercaptan compound, preferably a normal alkyl mercaptan compound or a tertiary alkyl mercaptan compound, and more preferably a normal alkyl mercaptan compound. In this case, the effect of the chain transfer agent can be stably exerted, and the processability of the manufactured acrylic rubber on a roller, etc., is highly improved, so it is preferred.
[0184] Specific examples of the alkyl mercaptan compound include n-pentyl mercaptan, n-hexyl mercaptan, n-heptyl mercaptan, n-octyl mercaptan, n-decyl mercaptan, n-dodecyl mercaptan, n-tridecyl mercaptan, n-tetradecyl mercaptan, n-hexadecyl mercaptan, n-octadecyl mercaptan, sec-pentyl mercaptan, sec-hexyl mercaptan, sec-heptyl mercaptan, sec-octyl mercaptan, sec-decyl mercaptan, sec-dodecyl mercaptan, sec-tridecyl mercaptan, sec-tetradecyl mercaptan, sec-hexadecyl mercaptan, sec-octadecyl mercaptan, tert-pentyl mercaptan, tert-hexyl mercaptan, tert-heptyl mercaptan, tert-octyl mercaptan, tert-decyl mercaptan, tert-dodecyl mercaptan, tert-tridecyl mercaptan, tert-tetradecyl mercaptan, tert-hexadecyl mercaptan, tert-octadecyl mercaptan, and the like. Preferably, n-octyl mercaptan, n-dodecyl mercaptan, and tert-dodecyl mercaptan are used, and more preferably, n-octyl mercaptan and n-dodecyl mercaptan are used.
[0185] These chain transfer agents can be used alone or in combination of two or more. The amount of the chain transfer agent used is not particularly limited, and is generally in the range of 0.0001 to 1 part by weight, preferably in the range of 0.0005 to 0.5 part by weight, more preferably in the range of 0.001 to 0.5 part by weight, particularly preferably in the range of 0.005 to 0.1 part by weight, and most preferably in the range of 0.01 to 0.06 part by weight, in which case the strength characteristics of the manufactured acrylic rubber and the roll processability are highly balanced, so it is preferred.
[0186] The present invention is characterized in that the chain transfer agent is not added at the beginning of the polymerization but is added in batches during the polymerization. This is preferred because it is possible to produce high molecular weight components and low molecular weight components of the obtained acrylic rubber and to make the molecular weight distribution within a specific range, thereby achieving a high balance between strength characteristics and processability with rollers, etc.
[0187] The number of times the chain transfer agent is added in batches is not particularly limited and can be appropriately selected according to the intended use. It is usually 1 to 5 times, preferably 2 to 4 times, more preferably 2 to 3 times, and particularly preferably 2 times. In this case, the strength characteristics of the manufactured acrylic rubber and the processability on rollers, etc. can be highly balanced, so it is preferred.
[0188] The timing of starting the batchwise post-addition of the chain transfer agent is not particularly limited and can be appropriately selected according to the intended use. It is usually 20 minutes or more after the initiation of polymerization, preferably 30 minutes or more after the initiation of polymerization, more preferably 30 to 200 minutes after the initiation of polymerization, particularly preferably 35 to 150 minutes after the initiation of polymerization, and most preferably 40 to 120 minutes after the initiation of polymerization. At this time, the strength characteristics of the manufactured acrylic rubber and the processability on rollers, etc. can be highly balanced, so it is preferred.
[0189] The amount of the chain transfer agent added each time in the batchwise post-addition is not particularly limited and can be appropriately selected according to the intended use. It is usually in the range of 0.00005 to 0.5 parts by weight, preferably in the range of 0.0001 to 0.1 parts by weight, more preferably in the range of 0.0005 to 0.05 parts by weight, particularly preferably in the range of 0.001 to 0.03 parts by weight, and most preferably in the range of 0.002 to 0.02 parts by weight, relative to 100 parts by weight of the monomer component. In this case, the strength characteristics and roll processability of the manufactured acrylic rubber can be highly balanced, so it is preferred.
[0190] After the chain transfer agent is added, the polymerization reaction can be continued for no particular limitation, usually for 30 minutes or more, preferably 45 minutes or more, more preferably 1 hour or more, and then the polymerization reaction is terminated.
[0191] (Post-addition of reducing agent)
[0192] In the present invention, the reducing agent of the redox catalyst can be added post-polymerization, and this is preferred because the strength characteristics of the produced acrylic rubber and the processability on rolls can be well balanced.
[0193] The reducing agent to be added later during the polymerization is the same as the examples and preferred ranges of the reducing agent described above. In the present invention, as the reducing agent to be added later, ascorbic acid or a salt thereof is preferred.
[0194] The amount of the reducing agent added after the polymerization is not particularly limited and may be appropriately selected depending on the intended use. It is generally in the range of 0.0001 to 1 part by weight, preferably in the range of 0.0005 to 0.5 part by weight, more preferably in the range of 0.001 to 0.5 part by weight, particularly preferably in the range of 0.005 to 0.1 part by weight, and most preferably in the range of 0.01 to 0.05 part by weight, relative to 100 parts by weight of the monomer component. In this case, the productivity of the acrylic rubber production is excellent, and the strength characteristics and processability of the manufactured acrylic rubber can be highly balanced, so it is preferred.
[0195] The reducing agent added during polymerization may be added continuously or batchwise, preferably batchwise. The number of times the reducing agent is added batchwise during polymerization is not particularly limited, but is usually 1 to 5 times, preferably 1 to 3 times, and more preferably 1 to 2 times.
[0196] When the reducing agent added at the beginning of the polymerization and during the polymerization is ascorbic acid or a salt thereof, the ratio of the amount of the ascorbic acid or a salt thereof added initially to the amount of the ascorbic acid or a salt thereof added later is not particularly limited, and is generally in the range of 1 / 9 to 8 / 2, preferably in the range of 2 / 8 to 6 / 4, and more preferably in the range of 3 / 7 to 5 / 5, in which case the productivity of the acrylic rubber production is excellent, and the strength characteristics and processability of the manufactured acrylic rubber can be highly balanced, so it is preferred.
[0197] The timing of post-addition of the reducing agent is not particularly limited and can be appropriately selected according to the purpose of use. It is usually 1 hour after the initiation of polymerization, preferably 1 to 3 hours after the initiation of polymerization, and more preferably 1.5 to 2.5 hours after the initiation of polymerization. At this time, the productivity of the acrylic rubber production is excellent, and the strength characteristics of the manufactured acrylic rubber and the processability of rollers, etc. can be highly balanced, so it is preferred.
[0198] The amount of the reducing agent added each time in the batchwise post-addition is not particularly limited and can be appropriately selected according to the intended use. It is usually in the range of 0.00005 to 0.5 parts by weight, preferably in the range of 0.0001 to 0.1 parts by weight, more preferably in the range of 0.0005 to 0.05 parts by weight, and particularly preferably in the range of 0.001 to 0.03 parts by weight, relative to 100 parts by weight of the monomer component. In this case, the strength characteristics of the manufactured acrylic rubber and the processability of rollers, etc. can be highly balanced, so it is preferred.
[0199] The operation after adding the reducing agent is not particularly limited, and the polymerization reaction can be continued for usually 30 minutes or more, preferably 45 minutes or more, and more preferably 1 hour or more, and then the polymerization reaction is terminated.
[0200] The polymerization conversion rate of the emulsion polymerization reaction is 90% by weight or more, preferably 95% by weight or more, at which time, the strength characteristics of the manufactured acrylic rubber are excellent and the monomer has no odor, so it is preferred. When terminating the polymerization, a polymerization terminator can be used.
[0201] After the emulsion polymerization, the obtained emulsion polymerization liquid (emulsion) is coagulated and dried to separate the acrylic rubber.
[0202] (Solidification process)
[0203] In the coagulation step after the emulsion polymerization, the emulsion polymerization liquid obtained in the emulsion polymerization is brought into contact with a coagulation liquid to coagulate, thereby generating water-containing particles of the acrylic rubber.
[0204] The solid content concentration of the emulsion polymerization liquid used in the coagulation reaction is not particularly limited, but is usually adjusted to a range of 5 to 50% by weight, preferably 10 to 45% by weight, and more preferably 20 to 40% by weight.
[0205] The coagulant of the coagulation liquid used is not particularly limited, and metal salts are generally used. Examples of the metal salt include alkali metals, metal salts of Group 2 of the periodic table, and other metal salts, preferably alkali metal salts, metal salts of Group 2 of the periodic table, more preferably metal salts of Group 2 of the periodic table, and particularly preferably magnesium salts, which can balance the water resistance, strength characteristics, metal mold release properties, and processability of the obtained acrylic rubber, so it is preferred.
[0206] Examples of the alkali metal salt include sodium salts such as sodium chloride, sodium nitrate, and sodium sulfate; potassium salts such as potassium chloride, potassium nitrate, and potassium sulfate; and lithium salts such as lithium chloride, lithium nitrate, and lithium sulfate. Among these, sodium salts are preferred, and sodium chloride and sodium sulfate are particularly preferred.
[0207] Examples of the periodic table Group 2 metal salts include magnesium chloride, calcium chloride, magnesium nitrate, calcium nitrate, magnesium sulfate, and calcium sulfate, and calcium chloride and magnesium sulfate are preferred.
[0208] Examples of other metal salts include zinc chloride, titanium chloride, manganese chloride, iron chloride, cobalt chloride, nickel chloride, aluminum chloride, tin chloride, zinc nitrate, titanium nitrate, manganese nitrate, iron nitrate, cobalt nitrate, nickel nitrate, aluminum nitrate, tin nitrate, zinc sulfate, titanium sulfate, manganese sulfate, iron sulfate, cobalt sulfate, nickel sulfate, aluminum sulfate, and tin sulfate.
[0209] These coagulants can be used alone or in combination of two or more, and their usage is usually in the range of 0.01 to 100 parts by weight, preferably in the range of 0.1 to 50 parts by weight, and more preferably in the range of 1 to 30 parts by weight, relative to 100 parts by weight of the monomer component. When the coagulant is within this range, the acrylic rubber can be fully coagulated, and the compression set resistance and water resistance can be highly improved when the acrylic rubber is cross-linked, so it is preferred.
[0210] In the coagulation process of the present invention, in particular, by concentrating the particle size of the generated water-containing aggregates in a specific area, the cleaning efficiency and the ash removal efficiency during dehydration are significantly improved, so it is preferred. The proportion of the range of 710μm to 6.7mm (not passing 710μm, passing 6.7mm) of the generated water-containing aggregates is not particularly limited, and is usually 30% by weight or more, preferably 50% by weight or more, more preferably 60% by weight or more, particularly preferably 70% by weight or more, and most preferably 80% by weight or more relative to all the generated water-containing aggregates. At this time, the water resistance of acrylic rubber can be significantly improved, so it is preferred. In addition, the proportion of the range of 710μm to 4.75mm (not passing 710μm, passing 4.75mm) of the generated water-containing aggregates is not particularly limited, and is usually 30% by weight or more, preferably 50% by weight or more, more preferably 60% by weight or more, particularly preferably 70% by weight or more, and most preferably 80% by weight or more relative to all the generated water-containing aggregates. At this time, the water resistance of acrylic rubber can be significantly improved, so it is preferred. Furthermore, the proportion of the range of 710 μm to 3.35 mm (not passing 710 μm, passing 3.35 mm) of the generated water-containing particles is not particularly limited, but is usually 20 wt % or more, preferably 30 wt % or more, more preferably 40 wt % or more, particularly preferably 50 wt % or more, and most preferably 60 wt % or more, relative to all the generated water-containing particles. In this case, the water resistance of the acrylic rubber can be significantly improved, so it is preferred.
[0211] There is no particular limitation on the method for producing the particle size of the generated water-containing aggregates within the above range, and it can be carried out, for example, by: the method for bringing the emulsion polymerization liquid into contact with the above coagulant is to add the emulsion polymerization liquid to a stirred coagulant liquid (aqueous solution of the coagulant); or by specifying the coagulant concentration of the coagulant liquid, the stirring number of the stirred coagulant liquid, and the peripheral speed.
[0212] The coagulating liquid used is usually used in the form of an aqueous solution, and the concentration of the coagulant in the aqueous solution is usually in the range of 0.1 to 20% by weight, preferably in the range of 0.5 to 15% by weight, more preferably in the range of 1 to 10% by weight, and particularly preferably in the range of 1.5 to 5% by weight. In this case, the particle size of the generated water-containing granules can be uniformly concentrated in a specific area, so it is preferred.
[0213] The temperature of the coagulation liquid is not particularly limited, but is usually 40° C. or higher, preferably in the range of 40 to 90° C., and more preferably in the range of 50 to 80° C. In this case, uniform water-containing granules can be generated, which is preferred.
[0214] The method for bringing the emulsion polymerization liquid into contact with the coagulation liquid is not particularly limited, and may be any of a method including, for example, a method of adding the coagulation liquid to the emulsion polymerization liquid, a method of adding the coagulation liquid to the emulsion polymerization liquid being stirred, a method of adding the emulsion polymerization liquid to the coagulation liquid, and a method of adding the emulsion polymerization liquid to the coagulation liquid being stirred. As described above, the method of adding the emulsion polymerization liquid to the coagulation liquid being stirred is preferred because the washing efficiency and dehydration efficiency of the generated water-containing particles are excellent and the water resistance and storage stability of the obtained acrylic rubber can be significantly improved.
[0215] The stirring speed (number of revolutions) of the stirred coagulation liquid, i.e., the number of revolutions of the stirring blade of the stirring device, is not particularly limited, but is usually 100 rpm or more, preferably 200 rpm or more, more preferably in the range of 200 to 1000 rpm, particularly preferably in the range of 300 to 900 rpm, and most preferably in the range of 400 to 800 rpm.
[0216] When the rotation speed is a rotation speed for a certain degree of vigorous stirring, the particle size of the generated water-containing agglomerates can be small and uniform. Therefore, it is preferred that by being above the above lower limit, the particle size of the generated agglomerates can be suppressed from being too large or too small, and by being below the above upper limit, the coagulation reaction can be more easily controlled.
[0217] The peripheral speed of the coagulating liquid being stirred, i.e. the speed of the outer periphery of the stirring blade of the stirring device is not particularly limited, preferably violently stirred to a certain extent, because the particle size of the water-containing agglomerates generated can be small and uniform. Usually more than 0.5m / s, preferably more than 1m / s, more preferably more than 1.5m / s, particularly preferably more than 2m / s, most preferably more than 2.5m / s. On the other hand, the upper limit of the peripheral speed is not particularly limited, usually less than 50m / s, preferably less than 30m / s, more preferably less than 25m / s, most preferably less than 20m / s, at this time, it is easy to control the coagulation reaction, so it is preferred.
[0218] By setting the above-mentioned conditions of the coagulation reaction (contact method, solid content concentration of the emulsion polymerization solution, concentration and temperature of the coagulation solution, number of revolutions and peripheral speed of the coagulation solution during stirring, etc.) within a specific range, the shape and particle size of the generated water-containing aggregates can be made uniform and centralized, and the removal efficiency of the emulsifier and coagulant during washing and dehydration can be significantly improved. As a result, the water resistance and storage stability of the manufactured acrylic rubber can be highly improved, so it is preferred.
[0219] (Cleaning process)
[0220] The water-containing particles generated in the above coagulation reaction are preferably washed before drying.
[0221] The washing method is not particularly limited, and the washing can be performed, for example, by mixing the produced water-containing pellets with a large amount of water.
[0222] The amount of water added for washing is not particularly limited. The amount of water added for each washing is usually 50 parts by weight or more relative to 100 parts by weight of the monomer component, preferably in the range of 50 to 15,000 parts by weight, more preferably in the range of 100 to 10,000 parts by weight, and further preferably in the range of 500 to 5,000 parts by weight. In this case, the ash content in the acrylic rubber can be effectively reduced, so it is preferred.
[0223] The temperature of the water used is not particularly limited, but hot water is preferably used, usually 40°C or higher, preferably 40 to 100°C, more preferably 50 to 90°C, and most preferably 60 to 80°C, because the cleaning efficiency can be significantly improved. By setting the temperature of the water used to be above the lower limit, the emulsifier and the coagulant are released from the water-containing particles, and the cleaning efficiency is further improved.
[0224] The washing time is not particularly limited, but is usually in the range of 1 to 120 minutes, preferably in the range of 2 to 60 minutes, and more preferably in the range of 3 to 30 minutes.
[0225] The number of washing (water washing) is not particularly limited, but is usually 1 to 10 times, preferably 1 to 5 times, and more preferably 2 to 3 times. In addition, from the viewpoint of reducing the residual amount of the coagulant in the acrylic rubber finally obtained, it is preferred that the number of water washings is large, but the number of water washings can be significantly reduced by making the shape of the water-containing pellets and the particle size of the water-containing pellets within the specific ranges and / or making the washing temperature within the above ranges as described above.
[0226] (Drying process)
[0227] The method for drying the above-mentioned water-containing pellets, preferably the water-containing pellets after washing, is not particularly limited, and a direct drying method such as hot air drying of the water-containing pellets after washing can be used, and it can be preferably carried out using a screw-type twin-shaft extrusion dryer. As the screw-type twin-shaft extrusion dryer used, it is not particularly limited as long as it is an extrusion dryer with two screws. In the present invention, the water-containing pellets are dried under high shear conditions using a screw-type twin-shaft extrusion dryer with two screws, which can make the roll processability, Banbury processability and strength characteristics of the obtained acrylic rubber highly balanced, so it is preferred.
[0228] In the present invention, the acrylic rubber can be obtained by melting the water-containing pellets in a screw-type twin-shaft extrusion dryer and extruding and drying. The drying temperature (set temperature) of the screw-type twin-shaft extrusion dryer can be appropriately selected, usually in the range of 100 to 250° C., preferably in the range of 110 to 200° C., and more preferably in the range of 120 to 180° C. At this time, the acrylic rubber will not be burned or deteriorated, and can be dried efficiently, so it is preferred.
[0229] In the present invention, it is preferred that the water-containing pellets are melted and extruded and dried under reduced pressure in a screw-type twin-shaft extrusion dryer, because the storage stability of the acrylic rubber can be highly improved without impairing roll processability and strength characteristics. In this stage, the vacuum degree in the screw-type twin-shaft extrusion dryer, which is preferred for removing air present in the acrylic rubber and improving storage stability, can be appropriately selected, and is usually in the range of 1 to 50 kPa, preferably in the range of 2 to 30 kPa, and more preferably in the range of 3 to 20 kPa.
[0230] In addition, in the present invention, when the water-containing pellets are melt-kneaded and dried in a screw-type twin-shaft extrusion dryer in a state where water is almost removed, the Banbury processability of the acrylic rubber can be highly improved without damaging the roll processability and strength characteristics, so it is preferred. As a state where water is almost removed that can highly improve the Banbury processability, it can be appropriately selected, and the water content of the acrylic rubber is usually less than 1% by weight, preferably less than 0.8% by weight, and more preferably less than 0.6% by weight. In addition, "melt-kneading" or "melt-kneading and drying" in the present invention refers to kneading (mixing) the acrylic rubber in a molten state in a screw-type twin-shaft extrusion dryer or extruding it in a molten state and drying it at this stage, or kneading, extruding, and drying the acrylic rubber in a molten (plasticized) state by a screw-type twin-shaft extrusion dryer.
[0231] The maximum torque of the screw-type twin-shaft extrusion dryer used in the present invention is not particularly limited, and is generally 30 N·m or more, preferably 35 N·m or more, and more preferably 40 N·m or more. In addition, the maximum torque of the screw-type twin-shaft extrusion dryer used in the present invention is generally in the range of 30 to 100 N·m, preferably in the range of 35 to 75 N·m, and more preferably in the range of 40 to 60 N·m. In this case, the roll processability, Banbury processability, and strength characteristics of the manufactured acrylic rubber can be highly balanced, so it is preferred.
[0232] The specific energy consumption of the screw-type twin-shaft extruder dryer used in the present invention is not particularly limited, but is generally in the range of 0.1 to 0.25 [kw·h / kg], preferably in the range of 0.13 to 0.23 [kw·h / kg], and more preferably in the range of 0.15 to 0.2 [kw·h / kg]. In this case, the roll processability, Banbury processability and strength characteristics of the obtained acrylic rubber are highly balanced, so it is preferred.
[0233] The specific power of the screw-type twin-shaft extruder dryer used in the present invention is not particularly limited, but is generally in the range of 0.2 to 0.6 [A·h / kg], preferably in the range of 0.25 to 0.55 [A·h / kg], and more preferably in the range of 0.35 to 0.5 [A·h / kg]. In this case, the roll processability, Banbury processability and strength characteristics of the obtained acrylic rubber are highly balanced, so it is preferred.
[0234] The shear rate of the screw-type twin-screw extruder dryer used in the present invention is not particularly limited, but is generally in the range of 40 to 150 [1 / s], preferably 45 to 125 [1 / s], and more preferably 50 to 100 [1 / s]. In this case, the storage stability, roll processability, Banbury processability, and strength characteristics of the obtained acrylic rubber are highly balanced, so it is preferred.
[0235] The shear viscosity of the acrylic rubber in the screw-type twin-screw extruder dryer used in the present invention is not particularly limited, but is generally in the range of 4000 to 8000 [Pa·s], preferably in the range of 4500 to 7500 [Pa·s], and more preferably in the range of 5000 to 7000 [Pa·s]. In this case, the storage stability, roll processability, Banbury processability and strength characteristics of the obtained acrylic rubber are highly balanced, which is preferred.
[0236] The acrylic rubber of the present invention obtained in this way is preferred because it is excellent in storage stability, roll processability, Banbury processability, strength characteristics, water resistance, and compression set resistance.
[0237] The acrylic rubber of the present invention is cooled after melt kneading and drying. The cooling rate is not particularly limited, but is usually 40°C / hour or more, preferably 50°C / hour or more, more preferably 100°C / hour or more, and particularly preferably 150°C / hour or more. In this case, the storage stability, roll processability, Banbury processability, strength characteristics, water resistance and compression set resistance are excellent, and the scorch stability is particularly excellent, so it is preferred.
[0238] <Acrylic rubber molded products>
[0239] The acrylic rubber molded article of the present invention is obtained by molding the above-mentioned acrylic rubber, and is usually obtained by coagulating an acrylic rubber emulsion obtained by emulsion polymerization and directly drying the granular acrylic rubber obtained by molding into a predetermined shape, and the characteristic values (physical property values) of the acrylic rubber itself can be maintained even when it is made into an acrylic rubber molded article. The acrylic rubber molded article of the present invention obtained in this way is usually not cross-linked.
[0240] The shape of the acrylic rubber molded product of the present invention is not particularly limited and may be appropriately selected according to the mode of use. Examples thereof include strands, sheets, and bags. Sheet-shaped acrylic rubber sheets or bag-shaped acrylic rubber bags are preferred because they are excellent in handling and storage stability.
[0241] The specific gravity of the acrylic rubber molded article of the present invention is not particularly limited, but is usually 0.7 or more, preferably 0.8 or more, more preferably 0.9 or more, particularly preferably 0.95 or more, and most preferably 1 or more. In this case, there is almost no air inside, and the storage stability is excellent, which is preferred. In addition, the specific gravity of the acrylic rubber molded article of the present invention is usually in the range of 0.7 to 1.6, preferably in the range of 0.8 to 1.5, more preferably in the range of 0.9 to 1.4, particularly preferably in the range of 0.95 to 1.3, and most preferably in the range of 1.0 to 1.2. In this case, productivity, storage stability, and crosslinking characteristics and stability of the crosslinked product are highly balanced, which is preferred.
[0242] The acrylic rubber molded product of the present invention is preferably obtained by drying the acrylic rubber under reduced pressure using a screw-type twin-screw extruder dryer, or by melt-kneading and drying the acrylic rubber under reduced pressure, because the properties such as storage stability, roll processability and strength properties are particularly excellent and well-balanced.
[0243] The acrylic rubber molded article of the present invention is preferably obtained by melt-kneading and drying the acrylic rubber in a screw-type biaxial extruder dryer in a state where water is substantially removed, since the Banbury processability and strength characteristics are well balanced.
[0244] The ash content, ash content (total amount of sodium, magnesium, calcium, phosphorus and sulfur, total amount of magnesium and phosphorus, magnesium amount, or phosphorus amount), ash composition ratio, complex viscosity at 60°C ([η]60°C), complex viscosity at 100°C ([η]100°C), ratio of the complex viscosity at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) ([η]100°C / [η]60°C), methyl ethyl ketone insoluble content, water content, pH and Mooney viscosity (ML1+4,100°C) of the acrylic rubber molded product of the present invention are the same as the examples and preferred ranges of the above-mentioned acrylic rubber.
[0245] The thickness of the acrylic rubber sheet of the present invention is not particularly limited, and can be appropriately selected according to the purpose of use. It is usually in the range of 1 to 40 mm, preferably in the range of 2 to 35 mm, more preferably in the range of 3 to 30 mm, and most preferably in the range of 5 to 25 mm. In this case, the handleability, storage stability and productivity are highly balanced, so it is preferred. The width of the acrylic rubber sheet of the present invention can be appropriately selected according to the purpose of use. It is usually in the range of 300 to 1200 mm, preferably in the range of 400 to 1000 mm, and more preferably in the range of 500 to 800 mm. In this case, the handleability is particularly excellent, so it is preferred. The length of the acrylic rubber sheet of the present invention is not particularly limited, and is usually in the range of 300 to 1200 mm, preferably in the range of 400 to 1000 mm, and more preferably in the range of 500 to 800 mm. In this case, the handleability is particularly excellent, so it is preferred.
[0246] The size of the acrylic rubber bag of the present invention is not particularly limited and can be appropriately selected according to the purpose of use. The width is usually in the range of 100 to 800 mm, preferably in the range of 200 to 500 mm, and more preferably in the range of 250 to 450 mm. The length is usually in the range of 300 to 1200 mm, preferably in the range of 400 to 1000 mm, and more preferably in the range of 500 to 800 mm. The height (thickness) is usually in the range of 50 to 500 mm, preferably in the range of 100 to 300 mm, and more preferably in the range of 150 to 250 mm. The above ranges are appropriate ranges. In addition, the shape of the acrylic rubber bag of the present invention is also not limited and can be appropriately selected according to the purpose of use of the acrylic rubber bag. In most cases, a rectangular parallelepiped is preferred.
[0247] The acrylic rubber content of the acrylic rubber molded product of the present invention may be appropriately selected depending on the intended use, and is usually 90 wt % or more, preferably 95 wt % or more, and more preferably 97 wt % or more. In this case, the strength characteristics and the processability with rollers etc. are well balanced, which is preferred.
[0248] The acrylic rubber molded article of the present invention is excellent in handling properties, storage stability, roll processability, Banbury processability, strength characteristics, and compression set resistance, and can be used as it is or after being cut.
[0249] <Method for producing acrylic rubber molded article>
[0250] The method for producing the acrylic rubber molded product is not particularly limited as long as it is a method for molding the acrylic rubber, and the molding process can be preferably performed subsequently to the method for producing the acrylic rubber.
[0251] As a specific method for producing an acrylic rubber molded body, there can be mentioned, for example, a method for producing an acrylic rubber sheet comprising the following steps: an emulsion polymerization step, in which a monomer component comprising a (meth)acrylate, an ion reactive group-containing monomer, and other copolymerizable monomers used as required is emulsified with water and an emulsifier, and then a polymerization reaction is initiated in the presence of a redox catalyst consisting of an inorganic free radical generator and a reducing agent, a chain transfer agent is added in batches during the polymerization, and then emulsion polymerization is carried out until the polymerization conversion rate is 90% by weight or more to obtain an emulsion polymerization solution; and a coagulation step, in which the obtained An emulsion polymerization liquid is contacted with a coagulation liquid to generate water-containing pellets; a washing step of washing the generated water-containing pellets; and a dehydration-drying-molding step, using a dehydrating barrel having a dehydration slit, a drying barrel under reduced pressure, and a screw-type twin-shaft extrusion dryer having a die head at the top end, dehydrating the washed water-containing pellets with the dehydrating barrel to a water content of 1 to 40% by weight, and then drying with the drying barrel to a water content of less than 1% by weight, and extruding a sheet-like dry rubber from the die head. In addition, a method for producing an acrylic rubber bag further includes a bag-forming step of laminating and bagging the extruded sheet-like dry rubber.
[0252] (Emulsion polymerization process, coagulation process and cleaning process)
[0253] The emulsion polymerization step, coagulation step, and washing step in the method for producing the acrylic rubber molded article are the same as those described in the method for producing the acrylic rubber.
[0254] (Dehydration-Drying-Forming Process)
[0255] The dehydration-drying-molding step in the method for producing an acrylic rubber molded body preferably uses a dehydrating barrel having a dehydration slit, a drying barrel under reduced pressure, and a screw-type twin-shaft extruder dryer having a die head at the top end, and the above-mentioned washed water-containing pellets are dehydrated to a water content of 1 to 40% by weight by the dehydrating barrel, and then dried to a water content of less than 1% by weight by the drying barrel, and a sheet-like dried rubber is extruded from the die head.
[0256] Although the specific embodiment thereof is shown below, the scope of the present invention is not limited thereto.
[0257] In the present invention, the water-containing pellets supplied to the screw-type twin-screw extruder dryer are preferably water-containing pellets from which free water has been removed (dehydrated) after washing.
[0258] (Water removal process)
[0259] In the method for producing an acrylic rubber molded body of the present invention, it is preferred to provide a dehydration step for separating free water from the washed water-containing pellets using a dehydrator after the water washing step and before the dehydration-drying-molding step, because this can improve the dehydration efficiency.
[0260] As the dewatering machine, a known dewatering machine can be used without particular limitation, and examples thereof include a metal mesh, a screen, and an electric sieving machine, and a metal mesh and a screen are preferred.
[0261] The mesh size of the dewatering machine is not particularly limited, but is usually in the range of 0.01 to 5 mm, preferably in the range of 0.1 to 1 mm, and more preferably in the range of 0.2 to 0.6 mm. In this case, the loss of water-containing particles is small and water can be removed efficiently, which is preferred.
[0262] The water content of the hydrous granules after water removal, that is, the water content of the hydrous granules subjected to the dehydration-drying step is not particularly limited, but is usually in the range of 50 to 80 wt %, preferably in the range of 50 to 70 wt %, and more preferably in the range of 50 to 60 wt %.
[0263] The temperature of the water-containing pellets after dehydration, that is, the temperature of the water-containing pellets put into the dehydration-drying step is not particularly limited, but is usually in the range of 40°C or above, preferably in the range of 40 to 100°C, more preferably in the range of 50 to 90°C, particularly preferably in the range of 55 to 85°C, and most preferably in the range of 60 to 80°C. In this case, a screw-type twin-shaft extrusion dryer can be used to efficiently dehydrate and dry water-containing pellets that are difficult to increase in temperature and have a high specific heat of 1.5 to 2.5 kJ / kg·K, such as the acrylic rubber of the present invention, so it is preferred.
[0264] (Dehydration of water-containing pellets in the dehydrator barrel)
[0265] The dehydration of the water-containing pellets is carried out in a dehydrating barrel in a screw-type twin-shaft extruder dryer having a dehydration slit. The mesh size of the dehydration slit can be appropriately selected according to the use conditions, and is usually in the range of 0.01 to 5 mm, preferably in the range of 0.1 to 1 mm, and more preferably in the range of 0.2 to 0.6 mm. In this case, the loss of the water-containing pellets is small and the water-containing pellets can be dehydrated efficiently, so it is preferred.
[0266] The number of dehydrating barrels in the screw-type twin-screw extruder dryer is not particularly limited, but is usually plural, preferably 2 to 10, and more preferably 3 to 6. Within this range, the adhesive acrylic rubber can be efficiently dehydrated, which is preferred.
[0267] There are two ways to remove water from the water-containing pellets in the dehydration barrel: removing water in a liquid state (drainage) from the dehydration slits and removing water in a vapor state (steam exhaust). In the present invention, drainage is defined as dehydration and steam exhaust is defined as pre-drying.
[0268] In the dehydration of the water-containing pellets, the water discharged from the dehydration slit may be in any state of liquid (drainage) or vapor (exhaust steam). When a screw-type twin-shaft extrusion dryer having a plurality of dehydration barrels is used for dehydration, the adhesive acrylic rubber can be dehydrated efficiently by combining drainage and steam exhaust, so it is preferred. In a screw-type twin-shaft extrusion dryer having three or more dehydration barrels, each dehydration barrel may be a drainage type dehydration barrel or a steam exhaust type dehydration barrel, which may be appropriately selected according to the purpose of use. Generally, when reducing the ash content in the manufactured acrylic rubber molded body, the drainage type barrel is increased, and when reducing the water content, the steam exhaust type barrel is increased.
[0269] The set temperature of the dehydrating barrel can be appropriately selected according to the monomer composition, ash content, water content, and operating conditions of the acrylic rubber, and is usually in the range of 60 to 150° C., preferably in the range of 70 to 140° C., and more preferably in the range of 80 to 130° C. The set temperature of the dehydrating barrel for dehydrating in a drained state is usually 60 to 120° C., preferably 70 to 110° C., and more preferably 80 to 100° C. The set temperature of the dehydrating barrel for dehydrating in a steamed state is usually in the range of 100 to 150° C., preferably in the range of 105 to 140° C., and more preferably in the range of 110 to 130° C.
[0270] The water content after dehydration in the drainage type dehydration for squeezing water from the water-containing pellets is not particularly limited, but is 1 to 40% by weight, preferably 5 to 40% by weight, more preferably 5 to 35% by weight, and particularly preferably 10 to 35% by weight. At this time, the productivity and ash removal efficiency are highly balanced, so it is preferred.
[0271] Regarding the dehydration of adhesive acrylic rubber having reactive groups, when dehydration is performed using a centrifuge or the like, the acrylic rubber adheres to the dehydration slit and can hardly be dehydrated (to a water content of about 45 to 55% by weight). However, in the present invention, a screw-type twin-shaft extrusion dryer having a dehydration slit and capable of forced extrusion by a screw is used, so that the water content can be reduced to the above range.
[0272] In the case of dehydrating the water-containing pellets with a drainage type dehydrator barrel and a steam exhaust type dehydrator barrel, the water content after drainage in the drainage type dehydrator barrel portion is usually 5 to 40% by weight, preferably 10 to 40% by weight, and more preferably 15 to 35% by weight, and the water content after pre-drying in the steam exhaust type dehydrator barrel portion is usually 1 to 30% by weight, preferably 3 to 20% by weight, and more preferably 5 to 15% by weight.
[0273] By setting the water content after dehydration to be not less than the above lower limit, the dehydration time can be shortened and deterioration of the acrylic rubber can be suppressed, while by setting the water content to be not more than the above upper limit, the ash content can be sufficiently reduced.
[0274] (Drying of water-containing pellets in the dryer barrel)
[0275] The drying of the water-containing granules after the above dehydration is preferably carried out using a screw-type twin-shaft extrusion dryer with a dryer barrel, and the drying is carried out in the dryer barrel under reduced pressure. By drying the acrylic rubber in the dryer barrel under reduced pressure, the drying efficiency of the acrylic rubber is high, and the air present in the acrylic rubber can be removed, so that acrylic rubber or acrylic rubber molded products with excellent storage stability can be manufactured, so it is preferred. In addition, in the present invention, by melting the acrylic rubber and extruding and drying it under reduced pressure, the storage stability of the acrylic rubber molded product can be highly improved. The storage stability of the acrylic rubber molded product is mainly related to the specific gravity of the acrylic rubber molded product and can be controlled by the specific gravity. However, when the storage stability of the acrylic rubber molded product with a large specific gravity is controlled at a high level, the storage stability of the acrylic rubber molded product can be controlled by the vacuum degree of the extrusion dryer, etc.
[0276] The vacuum degree of the drying barrel can be appropriately selected, and is usually 1 to 50 kPa, preferably 2 to 30 kPa, and more preferably 3 to 20 kPa. At this time, the water-containing particles can be dried efficiently, and acrylic rubber or acrylic rubber molded products with high specific gravity (no air inside) and excellent storage stability can be produced, so it is preferred.
[0277] The setting temperature of the drying barrel can be appropriately selected, and is usually in the range of 100 to 250° C., preferably in the range of 110 to 200° C., and more preferably in the range of 120 to 180° C. At this time, the acrylic rubber will not be burned or deteriorated, and can be dried efficiently, and the amount of methyl ethyl ketone insoluble components in the acrylic rubber or acrylic rubber molded body can be reduced, so it is preferred.
[0278] The number of drying barrels in the screw-type twin-shaft extrusion dryer is not particularly limited, and is usually multiple, preferably 2 to 10, and more preferably 3 to 8. The vacuum degree in the case of multiple drying barrels can be set to an approximate vacuum degree for all drying barrels, or each barrel can be changed. The set temperature in the case of multiple drying barrels can be set to an approximate temperature for all drying barrels, or each barrel can be changed. Preferably, the temperature of the discharge portion (the side close to the die head) is higher than the temperature of the introduction portion (the side close to the dehydration barrel), because this can improve the drying efficiency.
[0279] The water content of the dried rubber after drying is usually less than 1% by weight, preferably less than 0.8% by weight, and more preferably less than 0.6% by weight. In the present invention, it is particularly preferred to melt-extrude the dried rubber in a screw-type twin-shaft extrusion dryer so that the water content of the dried rubber is this value (a state in which water is almost removed), because this can reduce the amount of methyl ethyl ketone insoluble components of the acrylic rubber or acrylic rubber molded body. In the present invention, the acrylic rubber molded body melt-mixed or melt-mixed and dried using a screw-type twin-shaft extrusion dryer has a high balance of strength characteristics and Banbury processability, so it is preferred. In addition, "melt mixing" or "melt mixing and drying" in the present invention refers to that the acrylic rubber is mixed (mixed) in a molten state in a screw-type twin-shaft extrusion dryer or extruded in a molten state and dried at this stage, or the acrylic rubber is mixed, extruded, and dried in a molten (plasticized) state using a screw-type twin-shaft extrusion dryer.
[0280] In the present invention, the shear rate applied in the drying barrel of the screw-type twin-screw extruder dryer in a state where the acrylic rubber does not substantially contain water is not particularly limited, but is usually in the range of 10 [1 / s] or more, preferably in the range of 10 to 400 [1 / s], and more preferably in the range of 50 to 250 [1 / s]. In this case, the storage stability, roll processability, Banbury processability, strength characteristics and compression set resistance of the obtained acrylic rubber or acrylic rubber molded product are highly balanced, which is preferred.
[0281] The shear viscosity of the acrylic rubber in the screw-type twin-shaft extrusion dryer used in the present invention, especially in the drying barrel, is not particularly limited, but is usually 12000 [Pa·s] or less, preferably in the range of 1000 to 12000 [Pa·s], more preferably in the range of 2000 to 10000 [Pa·s], particularly preferably in the range of 3000 to 7000 [Pa·s], and most preferably in the range of 4000 to 6000 [Pa·s]. In this case, the storage stability, roll processability, Banbury processability and strength characteristics of the obtained acrylic rubber or acrylic rubber molded product are highly balanced, so it is preferred.
[0282] (Extrusion of dry rubber from the die head)
[0283] The dried rubber dehydrated and dried in the screw parts of the dehydrating barrel and the drying barrel is sent to a screw-free calibrated die head and extruded from the die head into a desired shape. A porous plate or a metal mesh may or may not be provided between the screw part and the die head.
[0284] It is preferred that the extruded dry rubber is extruded into a sheet shape by making the die shape substantially rectangular, because this allows the obtained dry rubber to have less air entrainment, a high specific gravity, and excellent storage stability.
[0285] The resin pressure at the die head is not particularly limited, but is usually in the range of 0.1 to 10 MPa, preferably in the range of 0.5 to 5 MPa, and more preferably in the range of 1 to 3 MPa. In this case, the acrylic rubber molded body has less air entrained (higher specific gravity) and excellent productivity, so it is preferred.
[0286] (Screw type twin-shaft extrusion dryer and operating conditions)
[0287] The screw length (L) of the screw-type twin-screw extruder dryer used may be appropriately selected depending on the intended use, and is usually in the range of 3000 to 15000 mm, preferably in the range of 4000 to 10000 mm, and more preferably in the range of 4500 to 8000 mm.
[0288] The screw diameter (D) of the screw-type twin-screw extruder dryer used may be appropriately selected depending on the intended use, and is usually in the range of 50 to 250 mm, preferably in the range of 100 to 200 mm, and more preferably in the range of 120 to 160 mm.
[0289] The ratio (L / D) of the screw length (L) to the screw diameter (D) of the screw-type twin-shaft extrusion dryer used is not particularly limited, but is generally in the range of 10 to 100, preferably in the range of 20 to 80, and more preferably in the range of 30 to 60. In this case, the molecular weight of the dried rubber will not be reduced or burned, and the water content can be made less than 1% by weight, so it is preferred.
[0290] The number of revolutions (N) of the screw-type twin-shaft extrusion dryer used can be appropriately selected according to various conditions, and is generally 10 to 1000 rpm, preferably 50 to 750 rpm, more preferably 100 to 500 rpm, and most preferably 120 to 300 rpm. At this time, the water content and the amount of methyl ethyl ketone insoluble components of the acrylic rubber or acrylic rubber molded product can be efficiently reduced, so it is preferred.
[0291] The extrusion rate (Q) of the screw-type twin-shaft extruder dryer used is not particularly limited, but is usually in the range of 100 to 1500 kg / hour, preferably in the range of 300 to 1200 kg / hour, more preferably in the range of 400 to 1000 kg / hour, and most preferably in the range of 500 to 800 kg / hour.
[0292] The ratio (Q / N) of the extrusion rate (Q) to the number of revolutions (N) of the screw-type twin-screw extruder dryer used is not particularly limited, but is usually in the range of 2-10, preferably in the range of 3-8, and more preferably in the range of 4-6.
[0293] The maximum torque of the screw-type twin-shaft extrusion dryer used is not particularly limited, but is usually 30 N·m or more, preferably 35 N·m or more, and more preferably 40 N·m or more. In addition, the maximum torque of the screw-type twin-shaft extrusion dryer used in the present invention is usually in the range of 30 to 100 N·m, preferably in the range of 35 to 75 N·m, and more preferably in the range of 40 to 60 N·m. In this case, the roll processability, Banbury processability, and strength characteristics of the manufactured acrylic rubber can be highly balanced, so it is preferred.
[0294] The specific energy consumption of the screw-type twin-shaft extruder dryer used is not particularly limited, but is generally in the range of 0.1 to 0.25 [kw·h / kg], preferably in the range of 0.13 to 0.23 [kw·h / kg], and more preferably in the range of 0.15 to 0.2 [kw·h / kg]. In this case, the roll processability, Banbury processability and strength characteristics of the obtained acrylic rubber are highly balanced, so it is preferred.
[0295] The specific power of the screw-type twin-shaft extruder dryer used is not particularly limited, but is generally in the range of 0.2 to 0.6 [A·h / kg], preferably in the range of 0.25 to 0.55 [A·h / kg], and more preferably in the range of 0.35 to 0.5 [A·h / kg]. In this case, the roll processability, Banbury processability and strength characteristics of the obtained acrylic rubber are highly balanced, so it is preferred.
[0296] The shear rate of the screw-type twin-screw extruder dryer used is not particularly limited, but is generally in the range of 40 to 150 [1 / s], preferably 45 to 125 [1 / s], and more preferably 50 to 100 [1 / s]. In this case, the storage stability, roll processability, Banbury processability, and strength characteristics of the obtained acrylic rubber are highly balanced, so it is preferred.
[0297] The shear viscosity of the acrylic rubber in the screw-type twin-screw extruder dryer used is not particularly limited, but is generally in the range of 4000 to 8000 [Pa·s], preferably in the range of 4500 to 7500 [Pa·s], and more preferably in the range of 5000 to 7000 [Pa·s]. In this case, the storage stability, roll processability, Banbury processability and strength characteristics of the obtained acrylic rubber are highly balanced, so it is preferred.
[0298] As described above, in the present invention, it is preferable to use an extrusion dryer having a twin-shaft screw because dehydration, drying, and molding can be performed under high shear conditions.
[0299] (Flake dry rubber)
[0300] The shape of the dried rubber extruded from the screw-type twin-shaft extrusion dryer is preferably a sheet because air is not entrained, the specific gravity can be increased, and the storage stability can be highly improved. The sheet-shaped dried rubber extruded from the screw-type twin-shaft extrusion dryer is usually cut after cooling and used as an acrylic rubber sheet.
[0301] The thickness of the sheet-like dry rubber extruded from the screw-type twin-shaft extruder dryer is not particularly limited, but is generally in the range of 1 to 40 mm, preferably in the range of 2 to 35 mm, more preferably in the range of 3 to 30 mm, and most preferably in the range of 5 to 25 mm, which is preferred because of excellent operability and productivity. In particular, since the thermal conductivity of the sheet-like dry rubber is as low as 0.15 to 0.35 W / mK, the thickness of the sheet-like dry rubber in the case of improving the cooling efficiency and significantly improving the productivity is generally in the range of 1 to 30 mm, preferably in the range of 2 to 25 mm, more preferably in the range of 3 to 15 mm, and particularly preferably in the range of 4 to 12 mm.
[0302] The width of the sheet-like dry rubber extruded from the screw-type biaxial extruder dryer can be appropriately selected depending on the intended use, and is usually in the range of 300 to 1200 mm, preferably in the range of 400 to 1000 mm, and more preferably in the range of 500 to 800 mm.
[0303] The temperature of the dried rubber extruded from the screw-type twin-screw extruder dryer is not particularly limited, but is usually in the range of 100 to 200°C, preferably in the range of 110 to 180°C, and more preferably in the range of 120 to 160°C.
[0304] The water content of the dried rubber extruded from the screw-type twin-screw extruder dryer is not particularly limited, but is usually less than 1% by weight, preferably 0.8% by weight or less, and more preferably 0.6% by weight or less.
[0305] The complex viscosity ([η]100°C) of the sheet-like dry rubber extruded from the screw-type twin-shaft extruder dryer at 100°C is not particularly limited, but is generally in the range of 1500 to 6000 [Pa·s], preferably in the range of 2000 to 5000 [Pa·s], more preferably in the range of 2500 to 4000 [Pa·s], and most preferably in the range of 2500 to 3500 [Pa·s]. In this case, the extrudability and shape retention of the sheet are highly balanced, so it is preferred. That is, by being equal to or greater than the lower limit, the extrudability can be made more excellent, and by being equal to or less than the upper limit, the shape collapse and breakage of the sheet-like dry rubber can be suppressed.
[0306] The sheet-like dried rubber extruded from the screw-type twin-screw extruder dryer can be folded and used directly, and can usually be cut and used.
[0307] The method for cutting the sheet-like dry rubber is not particularly limited. Since the acrylic rubber of the acrylic rubber molded product of the present invention has strong adhesiveness, it is preferred to cut the sheet-like dry rubber after cooling it in order to cut it continuously without entraining air.
[0308] The cutting temperature of the sheet-like dry rubber is not particularly limited, but is usually 60° C. or lower, preferably 55° C. or lower, and more preferably 50° C. or lower. In this case, the cutting property and productivity are well balanced, which is preferred.
[0309] The complex viscosity of the sheet-like dry rubber at 60°C ([η]60°C) is not particularly limited, but is usually 15,000 [Pa·s] or less, preferably in the range of 2,000 to 10,000 [Pa·s], more preferably in the range of 2,500 to 7,000 [Pa·s], and most preferably in the range of 2,700 to 5,500 [Pa·s]. In this case, it is preferred because continuous cutting can be achieved without entraining air.
[0310] The ratio of the complex viscosity of the sheet-like dry rubber at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) ([η]100°C / [η]60°C) is not particularly limited and may be appropriately selected depending on the intended use. It is usually 0.5 or more, preferably 0.6 or more, more preferably 0.7 or more, particularly preferably 0.8 or more, and most preferably 0.85 or more. The upper limit is usually 0.98 or less, preferably 0.97 or less, more preferably 0.96 or less, particularly preferably 0.95 or less, and most preferably 0.93 or less. In this case, air entrainment is low and the cutting property and productivity are well balanced, which is preferred.
[0311] The method for cooling the dried rubber sheet is not particularly limited, and the dried rubber sheet may be left at room temperature. Since the thermal conductivity of the dried rubber sheet is 0.15 to 0.35 W / mK, which is very low, forced cooling such as air cooling with blowing air or cooling air, watering with spraying water, or immersion in water is preferred in order to improve productivity. Air cooling with blowing air or cooling air is particularly preferred.
[0312] In the air cooling method of the sheet-like dried rubber, for example, the sheet-like dried rubber can be extruded from a screw-type twin-shaft extrusion dryer onto a conveyor such as a conveyor belt, and conveyed and cooled while blowing cold air. The temperature of the cold air is not particularly limited, but is usually in the range of 0 to 25° C., preferably in the range of 5 to 25° C., and more preferably in the range of 10 to 20° C. The cooling length is not particularly limited, but is usually in the range of 5 to 500 m, preferably in the range of 10 to 200 m, and more preferably in the range of 20 to 100 m.
[0313] The cooling rate of the sheet-like dried rubber is not particularly limited, but is usually 40°C / hour or more, preferably 50°C / hour or more, more preferably 100°C / hour or more, and particularly preferably 150°C / hour or more. In this case, it is easy to cut, air is not caught in the molded body, and the storage stability can be improved, which is preferred. In addition, in the present invention, the cooling rate of the sheet-like dried rubber is usually 40°C / hour or more, preferably 50°C / hour or more, more preferably 100°C / hour or more, and particularly preferably 150°C / hour or more. In this case, the scorch stability of the acrylic rubber composition is excellent, which is preferred.
[0314] The cut length of the sheet-like dry rubber is not particularly limited and can be appropriately selected depending on the intended use, but is usually in the range of 100 to 800 mm, preferably in the range of 200 to 500 mm, and more preferably in the range of 250 to 450 mm.
[0315] The acrylic rubber sheet obtained in this way has excellent handling properties compared to pelletized acrylic rubber, and is excellent in roll processability, crosslinking properties, strength characteristics, and compression set resistance. It is also excellent in storage stability, Banbury processability, and water resistance, and can be used directly or in a laminated and rubber-wrapped form.
[0316] (Lamination process)
[0317] The method for producing the acrylic rubber package of the present invention is not particularly limited, but it is preferred that an acrylic rubber package having less air entrainment and excellent storage stability be obtained by laminating the above-mentioned acrylic rubber sheets.
[0318] The lamination temperature of the acrylic rubber sheets is not particularly limited, but is usually 30°C or higher, preferably 35°C or higher, and more preferably 40°C or higher. At this time, air drawn in during lamination can escape, which is preferred. The number of sheets to be laminated can be appropriately selected according to the size or weight of the acrylic rubber package. The acrylic rubber package of the present invention is integrated by the weight of the laminated acrylic rubber sheets.
[0319] The acrylic rubber package of the present invention thus obtained is superior in handling properties, roll processability, crosslinking properties, strength characteristics, and compression set resistance, as compared to pelletized acrylic rubber, and is also superior in storage stability, Banbury processability, and water resistance. The acrylic rubber package can be used as it is, or cut into a desired amount and put into a mixer such as a Banbury or roll mixer for use.
[0320] <Rubber composition>
[0321] The rubber composition of the present invention is characterized by comprising a rubber component containing the acrylic rubber or the acrylic rubber molded product, a filler, and a crosslinking agent.
[0322] The rubber component as the main component of the rubber composition of the present invention may be the acrylic rubber of the present invention alone, or may be used in combination with other rubber components as required. The content of the acrylic rubber of the present invention or the acrylic rubber molded product in the rubber component may be appropriately selected according to the purpose of use, and is usually 30% by weight or more, preferably 50% by weight or more, and more preferably 70% by weight or more.
[0323] The other rubber components to be combined with the acrylic rubber of the present invention are not particularly limited, and examples thereof include natural rubber, polybutadiene rubber, polyisoprene rubber, styrene-butadiene rubber, acrylonitrile-butadiene rubber, silicone rubber, fluororubber, olefin elastomers, styrene elastomers, vinyl chloride elastomers, polyester elastomers, polyamide elastomers, polyurethane elastomers, and polysiloxane elastomers.
[0324] These other rubber components can be used alone or in combination of two or more. The shapes of these other rubber components can be any of pellets, strands, rubber bags, sheets, powders, etc. The content of other rubber components in the rubber component as a whole can be appropriately selected within the range that does not impair the effect of the present invention, for example, usually 70% by weight or less, preferably 50% by weight or less, and more preferably 30% by weight or less.
[0325] The filler contained in the rubber composition is not particularly limited, and examples thereof include reinforcing fillers and non-reinforcing fillers. A reinforcing filler is preferred. In this case, the rubber composition has excellent Banbury processability and short-time crosslinking properties, and the strength characteristics and compression set resistance of the crosslinked product are highly excellent, and water resistance is also excellent, so it is preferred.
[0326] Examples of reinforcing fillers include carbon blacks such as furnace black, acetylene black, thermal black, channel black, and graphite; silicon dioxides such as wet silica, dry silica, and colloidal silica, etc. Examples of non-reinforcing fillers include quartz powder, diatomaceous earth, zinc oxide, basic magnesium carbonate, activated calcium carbonate, magnesium silicate, aluminum silicate, titanium dioxide, talc, aluminum sulfate, calcium sulfate, and barium sulfate.
[0327] These fillers can be used alone or in combination of two or more, and their blending amount can be appropriately selected within the range that does not impair the effects of the present invention. It is usually in the range of 1 to 200 parts by weight, preferably in the range of 10 to 150 parts by weight, and more preferably in the range of 20 to 100 parts by weight, relative to 100 parts by weight of the rubber component.
[0328] As the crosslinking agent used for the rubber composition, there is no particular limitation, and a known crosslinking agent can be selected according to the purpose of use, and inorganic crosslinking agents such as sulfur compounds, organic crosslinking agents, etc. can be cited, preferably organic crosslinking agents. In addition, as a crosslinking agent, it can be any of a polynary compound or a mononary compound, preferably a polynary compound with more than two reactive groups. Furthermore, as a crosslinking agent, it can be any of an ionic crosslinking compound or a free radical crosslinking compound, preferably an ionic crosslinking compound.
[0329] As an organic crosslinking agent, there is no particular limitation, and an ion crosslinking organic compound is preferred, and a polyionic organic compound is particularly preferred. When the crosslinking agent is a polyionic organic compound (polyionic crosslinking compound), the Banbury processability and short-time crosslinking of the rubber composition are excellent, and the strength characteristics and compression set resistance of the crosslinked product are highly excellent, and the water resistance is also excellent, so it is particularly preferred. As the "ion" of ion crosslinking or polyionic, it is an ion reactive ion, for example, as long as it is an ion that undergoes an ion reaction with the ion reactive group of the ion reactive group-containing monomer of the above-mentioned acrylic rubber, there is no particular limitation, and preferably ion crosslinking organic compounds having ion reactive groups such as amino groups, epoxy groups, carboxyl groups, and thiol groups can be cited.
[0330] Specific examples of the polyvalent ionic organic compound include polyvalent amine compounds, polyvalent epoxy compounds, polyvalent carboxylic acid compounds, polyvalent thiol compounds, and the like. Polyvalent amine compounds and polyvalent thiol compounds are preferred, and polyvalent amine compounds are more preferred.
[0331] Examples of the polyamine compound include aliphatic polyamine compounds such as hexamethylenediamine, hexamethylenediamine carbamate, and N,N-biscinnamaldehyde-1,6-hexanediamine; aromatic polyamine compounds such as 4,4'-methylenedianiline, p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-(m-phenylenediisopropylidene)diphenylamine, 4,4'-(p-phenylenediisopropylidene)diphenylamine, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminobenzanilide, 4,4'-bis(4-aminophenoxy)biphenyl, m-phenylenediamine, p-phenylenediamine, and 1,3,5-phenyltriamine. Among these, hexamethylenedianiline carbamate and 2,2'-bis[4-(4-aminophenoxy)phenyl]propane are preferred. In addition, as the polyamine compound, the carbonates of these can be preferably used. These polyamine compounds are particularly preferably used in combination with a carboxyl group-containing acrylic rubber or acrylic rubber molded product, or an epoxy group-containing acrylic rubber or acrylic rubber molded product.
[0332] As the polythiol compound, a triazinethiol compound is preferably used, and examples thereof include 6-trimercapto-s-triazine, 2-anilino-4,6-dimercapto-s-triazine, 1-dibutylamino-3,5-dimercaptotriazine, 2-dibutylamino-4,6-dimercapto-s-triazine, 1-phenylamino-3,5-dimercaptotriazine, 2,4,6-trimercapto-1,3,5-triazine, 1-hexylamino-3,5-dimercaptotriazine, etc. These triazinethiol compounds are particularly preferably used in combination with a chlorine-containing acrylic rubber or an acrylic rubber molded product.
[0333] Examples of other polyvalent organic compounds include polyvalent carboxylic acid compounds such as tetradecanedioic acid, and metal dithiocarbamates such as zinc dimethyldithiocarbamate, etc. These other polyvalent organic compounds are particularly preferably used in combination with the epoxy-containing acrylic rubber or acrylic rubber molded product.
[0334] These crosslinking agents can be used alone or in combination of two or more, and the amount thereof is usually 0.001 to 20 parts by weight, preferably 0.1 to 10 parts by weight, and more preferably 0.1 to 5 parts by weight relative to 100 parts by weight of the rubber component. The amount of the crosslinking agent in this range is preferred because it can provide sufficient rubber elasticity and excellent mechanical strength as a crosslinked rubber.
[0335] The rubber composition of the present invention may be blended with an antioxidant as required. The type of antioxidant is not particularly limited, and examples thereof include 2,6-di-tert-butyl-4-methylphenol, 2,6-di-tert-butylphenol, butylhydroxyanisole, 2,6-di-tert-butyl-α-dimethylamino-p-cresol, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, styrenated phenol, 2,2'-methylenebis(6-α-methylbenzyl-p-cresol), 4,4'-methylenebis(2,6-di-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,4-bis[(octylthio)methyl]-6-methylphenol, 2,2'-thiobis(4-methyl-6-tert-butylphenol), 4,4'-thiobis(6-tert-butyl-o-cresol), 2,6-di-tert-butyl-4-[4,6 -bis(octylthio)-1,3,5-triazine-2-ylamino]phenol and other phenol antioxidants; tri(nonylphenyl)phosphite, diphenylisodecylphosphite, tetraphenyldipropylene glycol·diphosphite and other phosphite antioxidants; dilaurylthiodipropionate and other thioester antioxidants; phenyl-α-naphthylamine, phenyl-β-naphthylamine, p-(p-toluenesulfonamide)-diphenylamine, 4,4'-(α,α-dimethylbenzyl)diphenylamine, N,N-diphenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, butyraldehyde-aniline condensate and other amine antioxidants; 2-mercaptobenzimidazole and other imidazole antioxidants; 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline and other quinoline antioxidants; 2,5-di(tert-amyl)hydroquinone and other hydroquinone antioxidants, etc. Among these, amine antioxidants are particularly preferred.
[0336] These antioxidants can be used alone or in combination of two or more, and the amount thereof is in the range of 0.01 to 15 parts by weight, preferably 0.1 to 10 parts by weight, and more preferably 1 to 5 parts by weight, based on 100 parts by weight of the rubber component.
[0337] The rubber composition of the present invention comprises the rubber component of the acrylic rubber of the present invention and / or the acrylic rubber molded body of the present invention, a filler and a crosslinking agent as essential components, and contains an antioxidant as required, and further, can be arbitrarily combined with other additives commonly used in the technical field as required, such as: a crosslinking aid, a crosslinking accelerator, a crosslinking retarder, a silane coupling agent, a plasticizer, a processing aid, a lubricant, a pigment, a colorant, an antistatic agent, a foaming agent, etc. These other compounding agents can be used alone or in combination of two or more, and their compounding amounts can be appropriately selected within the range that does not impair the effects of the present invention.
[0338] As a method for producing the rubber composition of the present invention, there can be cited a method of mixing a rubber component containing the acrylic rubber and / or acrylic rubber molded body of the present invention, a filler, a crosslinking agent, and an antioxidant and other compounding ingredients that may be contained as needed. The mixing can be performed by any method available in the existing rubber processing field, such as an open roll, a Banbury mixer, various kneading machines, etc. The mixing order of the components can be carried out according to the usual order in the rubber processing field. For example, it is preferred that the components that are not easy to react and decompose when heated are fully mixed, and then the crosslinking agent, which is a component that is easy to react and decompose when heated, is mixed in a short time at a temperature where no reaction or decomposition occurs.
[0339] <Rubber cross-linked products>
[0340] The cross-linked rubber of the present invention is obtained by cross-linking the above-mentioned rubber composition.
[0341] The rubber cross-linked product of the present invention can be manufactured as follows: using the rubber composition of the present invention, it is molded using a molding machine corresponding to the desired shape, such as an extruder, an injection molding machine, a compressor or a roller, and a cross-linking reaction is carried out by heating to fix the shape to form a rubber cross-linked product. In this case, cross-linking can be carried out after pre-molding, or it can be cross-linked simultaneously with molding. The molding temperature is generally 10 to 200°C, preferably 25 to 150°C. The cross-linking temperature is generally 100 to 250°C, preferably 130 to 220°C, and more preferably 150 to 200°C. The cross-linking time is generally 0.1 minutes to 10 hours, preferably 1 minute to 5 hours. As a heating method, a method used in rubber cross-linking such as press heating, steam heating, oven heating, and hot air heating can be appropriately selected.
[0342] The cross-linked rubber of the present invention may be further heated for secondary cross-linking depending on the shape and size of the cross-linked rubber. The secondary cross-linking varies depending on the heating method, cross-linking temperature, shape, etc., and is preferably performed for 1 to 48 hours. The heating method and heating temperature may be appropriately selected.
[0343] The cross-linked rubber of the present invention maintains the basic properties of rubber such as tensile strength, elongation, hardness, etc., and also has excellent compression set resistance and water resistance.
[0344] The rubber cross-linked product of the present invention can be preferably used as, for example, sealing materials such as O-rings, packaging materials, diaphragms, oil seals, shaft seals, bearing seals, mechanical seals, wellhead seals, seals for electrical and electronic equipment, and seals for air compressors; various gaskets such as a rocker cover gasket installed at the connection between a cylinder block and a cylinder head, an oil pan gasket installed at the connection between an oil pan and a cylinder head or a transmission case, a gasket for a fuel cell spacer installed between a pair of casings sandwiching a unit cell having a positive electrode, an electrolyte plate, and a negative electrode, and a gasket for a top cover of a hard disk drive; a cushioning material, a vibration-proof material; a wire coating material; an industrial belt; a tube / hoses; a sheet, and the like.
[0345] The rubber cross-linked product of the present invention is preferably used as an extrusion molded product and a die cross-linked product used in automobile applications, for example, in fuel hoses such as fuel hoses, fuel filler nozzle hoses, exhaust hoses, paper hoses, oil hoses and other fuel tank fuel hoses; air hoses such as turbocharger air hoses and transmission control hoses; and various hoses such as radiator hoses, heater hoses, brake hoses, and air conditioning hoses.
[0346] <Structure of apparatus for producing acrylic rubber and acrylic rubber molded product>
[0347] Next, the structure of an apparatus for producing the acrylic rubber and the acrylic rubber molded product according to one embodiment of the present invention will be described. Figure 1 The figure schematically shows an example of an acrylic rubber manufacturing system having an apparatus structure for manufacturing an acrylic rubber and an acrylic rubber molded body according to an embodiment of the present invention. In the manufacture of the acrylic rubber of the present invention, for example, Figure 1 An acrylic rubber manufacturing system 1 is shown.
[0348] Figure 1 The acrylic rubber production system 1 shown is composed of an emulsion polymerization reactor (not shown), a coagulation device 3, a cleaning device 4, a dehydrator 43, and a screw-type twin-screw extruder dryer.
[0349] The emulsion polymerization reactor is configured to carry out the treatment in the above-mentioned emulsion polymerization step. Figure 1Although not shown in the figure, the emulsion polymerization reactor has, for example, a polymerization reaction tank, a temperature control unit for controlling the reaction temperature, and a stirring device having a motor and a stirring blade. In the emulsion polymerization reactor, water and an emulsifier are mixed in the monomer components for forming the acrylic rubber, and emulsification is performed while appropriately stirring with a stirrer, and an emulsion polymerization reaction is initiated in the presence of a redox catalyst composed of an inorganic free radical generator and a reducing agent, and a chain transfer agent is added batchwise during the polymerization, thereby obtaining an emulsion polymerization liquid. The emulsion polymerization reactor can be any of a batch type, a semi-batch type, and a continuous type, and can be any of a tank type reactor and a tubular type reactor.
[0350] Figure 1 The solidification device 3 shown is constructed in such a way as to carry out the above-mentioned solidification process. Figure 1 As schematically shown, the coagulation device 3 includes, for example, a stirring tank 30, a heating unit 31 for heating the inside of the stirring tank 30, a temperature control unit (not shown) for controlling the temperature in the stirring tank 30, a stirring device 34 including a motor 32 and a stirring blade 33, and a drive control unit (not shown) for controlling the number of revolutions and the rotation speed of the stirring blade 33. In the coagulation device 3, the emulsion polymerization liquid obtained in the emulsion polymerization reactor is brought into contact with the coagulation liquid and coagulated, thereby generating water-containing particles.
[0351] In the coagulation device 3, for example, the emulsion polymerization liquid and the coagulation liquid can be brought into contact by a method of adding the emulsion polymerization liquid to the coagulation liquid being stirred. That is, the stirring tank 30 of the coagulation device 3 is pre-filled with the coagulation liquid, and the emulsion polymerization liquid is added to the coagulation liquid and brought into contact with the coagulation liquid to coagulate the emulsion polymerization liquid, thereby generating water-containing particles.
[0352] The heating unit 31 of the coagulation device 3 is configured to heat the coagulation liquid filled in the stirring tank 30. In addition, the temperature control unit of the coagulation device 3 is configured as follows: while monitoring the temperature in the stirring tank 30 measured by a thermometer, the heating operation of the heating unit 31 is controlled, thereby controlling the temperature in the stirring tank 30. The temperature of the coagulation liquid in the stirring tank 30 is controlled by the temperature control unit to be generally in the range of 40° C. or more, preferably in the range of 40 to 90° C., and more preferably in the range of 50 to 80° C.
[0353] The stirring device 34 of the coagulation device 3 is configured to stir the coagulation liquid filled in the stirring tank 30. Specifically, the stirring device 34 has a motor 32 that generates a rotational power and a stirring blade 33 that extends in a direction perpendicular to the rotation axis of the motor 32. The stirring blade 33 can rotate around the rotation axis in the coagulation liquid filled in the stirring tank 30 by the rotational power of the motor 32, thereby causing the coagulation liquid to flow. The shape, size, number of settings, etc. of the stirring blade 33 are not particularly limited.
[0354] The drive control unit of the solidification device 3 controls the rotation drive of the motor 32 of the stirring device 34, and sets the number of revolutions and the speed of the stirring blade 33 of the stirring device 34 to a predetermined value. The driving control unit controls the rotation of the stirring blade 33, so that the stirring number of the solidification liquid is, for example, usually in the range of 100 rpm or more, preferably in the range of 200 to 1000 rpm, more preferably in the range of 300 to 900 rpm, and particularly preferably in the range of 400 to 800 rpm. The driving control unit controls the rotation of the stirring blade 33, so that the circumferential speed of the solidification liquid is usually 0.5 m / s or more, preferably 1 m / s or more, more preferably 1.5 m / s or more, particularly preferably 2 m / s or more, and most preferably 2.5 m / s or more. Furthermore, the driving control unit controls the rotation of the stirring blade 33, so that the upper limit of the circumferential speed of the solidification liquid is usually 50 m / s or less, preferably 30 m / s or less, more preferably 25 m / s or less, and most preferably 20 m / s or less.
[0355] Figure 1 The cleaning device 4 shown is constructed in such a way as to carry out the above-mentioned cleaning process. Figure 1 As schematically shown, the cleaning device 4 includes, for example, a cleaning tank 40, a heating unit 41 for heating the inside of the cleaning tank 40, and a temperature control unit (not shown) for controlling the temperature in the cleaning tank 40. In the cleaning device 4, the water-containing pellets generated in the coagulation device 3 are mixed with a large amount of water for cleaning, so that the ash content in the finally obtained acrylic rubber can be efficiently reduced.
[0356] The heating unit 41 of the cleaning device 4 is configured to heat the inside of the cleaning tank 40. The temperature control unit of the cleaning device 4 is configured to control the heating operation of the heating unit 41 while monitoring the temperature inside the cleaning tank 40 measured by a thermometer, thereby controlling the temperature inside the cleaning tank 40. As described above, the temperature of the cleaning water in the cleaning tank 40 is usually controlled to be in the range of 40° C. or higher, preferably in the range of 40 to 100° C., more preferably in the range of 50 to 90° C., and most preferably in the range of 60 to 80° C.
[0357] The water-containing pellets washed in the washing device 4 are supplied to the screw-type twin-screw extrusion dryer 5 for performing a dehydration process and a drying process. At this time, the washed water-containing pellets are preferably supplied to the screw-type twin-screw extrusion dryer 5 after passing through a dehydrator 43 capable of separating free water. For example, a metal mesh, a screen, an electric sieving machine, etc. can be used for the dehydrator 43.
[0358] In addition, when the washed water pellets are supplied to the screw-type twin-shaft extrusion dryer 5, the temperature of the water pellets is 40°C or higher, and more preferably 60°C or higher. For example, by setting the temperature of the water used for washing in the washing device 4 to 60°C or higher (for example, 70°C), the temperature of the water pellets supplied to the screw-type twin-shaft extrusion dryer 5 can be maintained at 60°C or higher, and the temperature of the water pellets can be heated to 40°C or higher, preferably 60°C or higher when conveyed from the washing device 4 to the screw-type twin-shaft extrusion dryer 5. As a result, the dehydration process and the drying process of the subsequent process can be efficiently performed, and the water content of the finally obtained dried rubber can be greatly reduced.
[0359] Figure 1 The screw-type twin-shaft extrusion drying machine 5 shown is constructed in such a way as to perform the above-mentioned dehydration process and drying process. Figure 1 A screw-type twin-shaft extrusion dryer 5 is illustrated as a preferred example, but a centrifuge, a press, etc. may be used as a dehydrator for the dehydration process, and a hot air dryer, a reduced pressure dryer, an expansion dryer, a kneading machine type dryer, etc. may be used as a dryer for the drying process.
[0360] The screw-type twin-shaft extrusion dryer 5 is configured to mold the dried rubber obtained through the dehydration process and the drying process into a predetermined shape and discharge it. Specifically, the screw-type twin-shaft extrusion dryer 5 is configured as follows: it has a dehydrator barrel 53, which has a function as a dehydrator to dehydrate the water-containing pellets cleaned by the cleaning device 4; a drying barrel 54, which has a function as a dryer to dry the water-containing pellets; and a die head 59, which has a molding function and molds the water-containing pellets on the downstream side of the screw-type twin-shaft extrusion dryer 5.
[0361] Below, while referring to Figure 2 , while explaining the structure of the screw type twin-shaft extrusion dryer 5. Figure 2 Shown as Figure 1 The structure of a preferred specific example of the screw-type twin-screw extrusion dryer 5 is shown. By this screw-type twin-screw extrusion dryer 5, the above-mentioned dehydration-drying step can be preferably performed.
[0362] Figure 2 The screw-type twin-shaft extrusion dryer 5 shown is a twin-shaft screw-type extrusion dryer having a pair of screws (not shown) in a barrel unit 51. The screw-type twin-shaft extrusion dryer 5 has a drive unit 50 for rotating and driving the pair of screws in the barrel unit 51. This structure is preferred because it is possible to apply high shear to the acrylic rubber for drying. The drive unit 50 is installed at the upstream end ( Figure 2In addition, the screw-type twin-shaft extruder dryer 5 has a lower end ( Figure 2 The right end of the die 59 is provided.
[0363] The barrel unit 51 is from the upstream side to the downstream side ( Figure 2 From the left side to the right side in the figure, there is a supply barrel section 52, a dehydrator barrel section 53, and a drying barrel section 54.
[0364] The supply cylinder portion 52 is composed of two supply cylinders, that is, a first supply cylinder 52 a and a second supply cylinder 52 b .
[0365] Furthermore, the dehydrating barrel section 53 is composed of three dehydrating barrels, namely, a first dehydrating barrel 53a, a second dehydrating barrel 53b, and a third dehydrating barrel 53c.
[0366] The dryer cylinder portion 54 includes eight dryer cylinders, namely, a first dryer cylinder 54a, a second dryer cylinder 54b, a third dryer cylinder 54c, a fourth dryer cylinder 54d, a fifth dryer cylinder 54e, a sixth dryer cylinder 54f, a seventh dryer cylinder 54g, and an eighth dryer cylinder 54h.
[0367] In this way, the barrel unit 51 is composed of 13 divided barrels 52a to 52b, 53a to 53c, and 54a to 54h connected from the upstream side to the downstream side.
[0368] In addition, the screw-type twin-shaft extrusion dryer 5 has a heating unit (not shown) that heats each of the above-mentioned barrels 52a to 52b, 53a to 53c, and 54a to 54h individually and heats the water-containing pellets in each barrel 52a to 52b, 53a to 53c, and 54a to 54h to a predetermined temperature. The heating unit has a number corresponding to each barrel 52a to 52b, 53a to 53c, and 54a to 54h. As such a heating unit, for example, a structure in which high-temperature steam is supplied from a steam supply unit to a steam flow isolation cover formed in each barrel 52a to 52b, 53a to 53c, and 54a to 54h can be adopted, but it is not limited to this. In addition, the screw-type twin-shaft extrusion dryer 5 has a temperature control unit (not shown) for controlling the set temperature of each heating unit corresponding to each barrel 52a to 52b, 53a to 53c, and 54a to 54h.
[0369] The number of supply barrels, dehydration barrels, and drying barrels constituting the barrel sections 52, 53, and 54 in the barrel unit 51 is not limited to Figure 2 In the manner shown, the amount can be set to correspond to the water content of the water-containing pellets of the acrylic rubber to be dried.
[0370] For example, the number of supply cylinders of the supply cylinder section 52 is, for example, 1 to 3. In addition, the number of dehydrating cylinders of the dehydrating cylinder section 53 is, for example, preferably 2 to 10, and when it is 3 to 6, it is more preferable because the water-containing pellets of the adhesive acrylic rubber can be dehydrated efficiently. In addition, the number of drying cylinders of the drying cylinder section 54 is, for example, preferably 2 to 10, and more preferably 3 to 8.
[0371] The pair of screws in the barrel unit 51 are driven to rotate by a drive unit such as a motor housed in the drive unit 50. The pair of screws extend from the upstream side to the downstream side in the barrel unit 51, and by being driven to rotate, the water-containing pellets supplied to the supply barrel portion 52 can be mixed and transported to the downstream side. As a pair of screws, it is preferred that the screw ridge portion and the screw groove portion are in a state of meshing with each other, thereby improving the dehydration efficiency and drying efficiency of the water-containing pellets.
[0372] In addition, the rotation direction of a pair of screws can be the same direction or different directions. From the performance aspect of self-cleaning, it is preferred to rotate in the same direction. The screw shape of a pair of screws is not particularly limited, as long as it is the shape required by each barrel portion 52, 53, 54, and is not particularly limited.
[0373] The supply barrel section 52 is a region for supplying water-containing particles into the barrel unit 51. The first supply barrel 52a of the supply barrel section 52 has a feed port 55 for supplying water-containing particles into the barrel unit 51.
[0374] The dehydrator cylinder 53 is a region where liquid (slurry) containing a coagulant and the like is separated from the water-containing particles and discharged.
[0375] The first to third dehydrating cylinders 53a to 53c constituting the dehydrating cylinder portion 53 respectively have dehydrating slits 56a, 56b, 56c for discharging water of the water-containing aggregates to the outside. A plurality of dehydrating slits 56a, 56b, 56c are formed in each of the dehydrating cylinders 53a to 53c.
[0376] The slit width, i.e., mesh size, of each dehydration slit 56a, 56b, 56c may be appropriately selected according to the use conditions and is usually 0.01 to 5 mm. From the viewpoint of minimizing the loss of water-containing aggregates and being able to efficiently dehydrate the water-containing aggregates, it is preferably 0.1 to 1 mm, and more preferably 0.2 to 0.6 mm.
[0377] There are two situations in which water is removed from the water-containing pellets in each dehydrating barrel 53a to 53c of the dehydrating barrel section 53: the situation in which water is removed from each dehydrating slit 56a, 56b, 56c in a liquid state and the situation in which water is removed in a vapor state. In the dehydrating barrel section 53 of the present embodiment, the situation in which water is removed in a liquid state is defined as drainage, and the situation in which water is removed in a vapor state is defined as steam discharge, so as to distinguish them.
[0378] In the dehydrator barrel section 53, the combination of draining water and exhausting steam can effectively reduce the moisture content of the adhesive acrylic rubber, so it is preferred. In the dehydrator barrel section 53, which dehydrator barrel performs draining water or exhausting steam among the first to third dehydrator barrels 53a to 53c can be appropriately set according to the purpose of use. Generally, in the case of reducing the ash content in the manufactured acrylic rubber, the dehydrator barrel that performs draining water is increased. In this case, for example, Figure 2 As shown, the first and second dehydrating barrels 53a and 53b on the upstream side are drained, and the third dehydrating barrel 53c on the downstream side is discharged steam. In addition, when the dehydrating barrel section 53 has four dehydrating barrels, for example, it is possible to consider a method in which, for example, three dehydrating barrels on the upstream side are drained and one dehydrating barrel on the downstream side is discharged steam. On the other hand, in the case of reducing the water content, it is sufficient to increase the dehydrating barrel that discharges steam.
[0379] The set temperature of the dehydrator barrel 53 is usually in the range of 60 to 150°C, preferably in the range of 70 to 140°C, and more preferably in the range of 80 to 130°C, as described in the above-mentioned dehydration-drying process. The set temperature of the dehydrator barrel for dehydration in a drained state is usually in the range of 60 to 120°C, preferably in the range of 70 to 110°C, and more preferably in the range of 80 to 100°C. The set temperature of the dehydrator barrel for dehydration in a steam-exhausted state is usually in the range of 100 to 150°C, preferably in the range of 105 to 140°C, and more preferably in the range of 110 to 130°C.
[0380] The dryer cylinder 54 is a region where the dehydrated water-containing aggregates are dried under reduced pressure. Among the first to eighth dryer cylinders 54a to 54h constituting the dryer cylinder 54, the second dryer cylinder 54b, the fourth dryer cylinder 54d, the sixth dryer cylinder 54f, and the eighth dryer cylinder 54h respectively have exhaust ports 58a, 58b, 58c, and 58d for degassing. Each exhaust port 58a, 58b, 58c, and 58d is connected to an exhaust pipe (not shown).
[0381] The ends of the exhaust pipes are connected to vacuum pumps (not shown), and the operation of these vacuum pumps reduces the pressure in the dryer barrel 54 to a predetermined pressure. The screw-type twin-shaft extruder dryer 5 has a pressure control unit (not shown) for controlling the operation of these vacuum pumps and controlling the vacuum degree in the dryer barrel 54.
[0382] The degree of vacuum in the dryer cylinder 54 may be appropriately selected, and is usually set to 1 to 50 kPa, preferably 2 to 30 kPa, and more preferably 3 to 20 kPa, as described above.
[0383] The set temperature in the dryer cylinder 54 may be appropriately selected, and is usually set to 100 to 250°C, preferably 110 to 200°C, and more preferably 120 to 180°C, as described above.
[0384] In each of the dryer barrels 54a to 54h constituting the dryer barrel portion 54, the set temperatures in all of the dryer barrels 54a to 54h can be approximately the same value, or they can be different. When the temperature on the downstream side (die head 59 side) is set higher than the temperature on the upstream side (dehydrator barrel portion 53 side), it is preferred because the drying efficiency can be improved.
[0385] The die head 59 is a metal mold disposed at the downstream end of the barrel unit 51, and has a discharge port of a predetermined nozzle shape. The acrylic rubber dried in the dryer barrel 54 is extruded through the discharge port of the die head 59 into a shape corresponding to the predetermined nozzle shape. The acrylic rubber passing through the die head 59 can be formed into various shapes such as granules, columns, round rods, sheets, etc. according to the nozzle shape of the die head 59, and is formed into a sheet in the present invention. A porous plate or a metal mesh may be provided between the screw and the die head 59, or may not be provided.
[0386] The water-containing pellets of acrylic rubber obtained through the washing process are supplied to the supply barrel section 52 from the feed port 55. The water-containing pellets supplied to the supply barrel section 52 are conveyed from the supply barrel section 52 to the dehydrating barrel section 53 by the rotation of a pair of screws in the barrel unit 51. In the dehydrating barrel section 53, as described above, water contained in the water-containing pellets is drained and steam is discharged from the dehydrating slits 56a, 56b, and 56c respectively provided in the first to third dehydrating barrels 53a to 53c, and the water-containing pellets are dehydrated.
[0387] The water-containing pellets dehydrated in the dehydrator barrel 53 are sent to the dryer barrel 54 by the rotation of a pair of screws in the barrel unit 51. The water-containing pellets sent to the dryer barrel 54 are plasticized and mixed to become a melt, and are transported to the downstream side while releasing heat and raising the temperature. Then, the water contained in the melt of the acrylic rubber is vaporized, and the water (steam) is discharged to the outside through the exhaust pipes (not shown) connected to the exhaust ports 58a, 58b, 58c, and 58d, respectively.
[0388] As described above, the water-containing pellets are dried by the drying barrel 54 to become a melt of acrylic rubber, and the acrylic rubber is supplied to the die 59 by the rotation of the pair of screws in the barrel unit 51 and extruded from the die 59 .
[0389] Here, an example of the operating conditions of the screw-type twin-screw extrusion dryer 5 according to the present embodiment will be described.
[0390] The number of revolutions (N) of the pair of screws in the barrel unit 51 can be appropriately selected according to various conditions, and is generally 10 to 1000 rpm. From the perspective of being able to efficiently reduce the water content of the acrylic rubber and the amount of methyl ethyl ketone insoluble components, it is preferably 50 to 750 rpm, more preferably 100 to 500 rpm, and most preferably 120 to 300 rpm.
[0391] The extrusion rate (Q) of the acrylic rubber is not particularly limited, but is usually 100 to 1500 kg / hour, preferably 300 to 1200 kg / hour, more preferably 400 to 1000 kg / hour, and most preferably 500 to 800 kg / hour.
[0392] The ratio (Q / N) of the acrylic rubber extrusion amount (Q) to the screw rotation number (N) is not particularly limited, but is usually 1-20, preferably 2-10, more preferably 3-8, and particularly preferably 4-6.
[0393] The maximum torque in the barrel unit 51 is not particularly limited, but is usually in the range of 30 to 100 N·m, preferably in the range of 35 to 75 N·m, and more preferably in the range of 40 to 60 N·m.
[0394] The specific energy consumption in the barrel unit 51 is not particularly limited, but is usually in the range of 0.1 to 0.25 [kw·h / kg], preferably 0.13 to 0.23 [kw·h / kg], and more preferably 0.15 to 0.2 [kw·h / kg].
[0395] The specific power in the barrel unit 51 is not particularly limited, but is usually in the range of 0.2 to 0.6 [A·h / kg], preferably 0.25 to 0.55 [A·h / kg], and more preferably 0.35 to 0.5 [A·h / kg].
[0396] The shear rate in the barrel unit 51 is not particularly limited, but is usually in the range of 40 to 150 [1 / s], preferably 45 to 125 [1 / s], and more preferably 50 to 100 [1 / s].
[0397] The shear viscosity of the acrylic rubber in the barrel unit 51 is not particularly limited, but is usually in the range of 4000 to 8000 [Pa·s], preferably 4500 to 7500 [Pa·s], and more preferably 5000 to 7000 [Pa·s].
[0398] Figure 1 The cooling device 6 shown is configured to cool the dried rubber obtained through the dehydration process using the dehydrator and the drying process using the dryer. As the cooling method using the cooling device 6, various methods including air cooling under blowing or cold air, watering by spraying water, immersion in water, etc. can be adopted. In addition, the dried rubber can also be cooled by leaving it at room temperature.
[0399] As described above, the dried rubber discharged from the screw-type twin-shaft extruder drier 5 is extruded and molded into various shapes such as granules, columns, round rods, and sheets, depending on the nozzle shape of the die head 59. In the present application, the dried rubber is molded into a sheet shape. Figure 3 , a conveyor type cooling device 60 for cooling the sheet-shaped dry rubber 10 formed into a sheet shape will be described as an example of the cooling device 6 .
[0400] Figure 3 Shown as Figure 1 The cooling device 6 shown is a preferred structure of a transport cooling device 60. Figure 3 The conveyor type cooling device 60 shown is configured to cool the sheet-shaped dried rubber 10 discharged from the discharge port of the die head 59 of the screw type twin-screw extrusion dryer 5 by air cooling while conveying it. By using this conveyor type cooling device 60, the sheet-shaped dried rubber discharged from the screw type twin-screw extrusion dryer 5 can be preferably cooled.
[0401] Figure 3 The transportable cooling device 60 shown is similar to, for example, Figure 2 The die head 59 of the screw type twin-screw extrusion dryer 5 shown is directly connected or installed near the die head 59 for use.
[0402] The transportable cooling device 60 has a Figure 3 The conveyor 61 for conveying the sheet-like dried rubber 10 discharged from the die head 59 of the screw-type biaxial extrusion dryer 5 in the direction of the middle arrow A and the cooling unit 65 for blowing cold air to the sheet-like dried rubber 10 on the conveyor 61 .
[0403] The conveyor 61 has rollers 62 and 63, and a conveyor belt 64 which is tightly wound around these rollers 62 and 63 and on which the sheet-like dried rubber 10 is placed. The conveyor 61 continuously conveys the sheet-like dried rubber 10 discharged from the die head 59 of the screw-type twin-shaft extrusion dryer 5 to the downstream side ( Figure 3 The method is as follows:
[0404] The cooling unit 65 is not particularly limited, and examples thereof include a cooling unit having a structure capable of blowing cooling air sent from a cooling air generating unit (not shown) onto the surface of the sheet-like dry rubber 10 on the conveyor 64 .
[0405] The length L1 of the conveyor 61 and the cooling unit 65 of the conveyor type cooling device 60 (the length of the portion capable of blowing cooling air) is not particularly limited, and is, for example, 10 to 100 m, preferably 20 to 50 m. In addition, the conveying speed of the sheet-like dried rubber 10 in the conveyor type cooling device 60 can be appropriately adjusted according to the length L1 of the conveyor 61 and the cooling unit 65, the discharge speed of the sheet-like dried rubber 10 discharged from the die head 59 of the screw-type twin-shaft extrusion dryer 5, the target cooling speed, the cooling time, etc., and is, for example, 10 to 100 m / hour, and more preferably 15 to 70 m / hour.
[0406] according to Figure 3 The conveyor cooling device 60 shown cools the dried rubber sheet 10 by blowing cooling air from a cooling unit 65 to the dried rubber sheet 10 while conveying the dried rubber sheet 10 discharged from the die head 59 of the screw-type twin-screw extruder drier 5 by a conveyor 61 .
[0407] In addition, the transport type cooling device 60 is not particularly limited to Figure 3 The structure having one conveyor 61 and one cooling unit 65 shown in the figure may be a structure having two or more conveyors 61 and two or more corresponding cooling units 65. In this case, the combined length of each of the two or more conveyors 61 and the cooling unit 65 may be set within the above range.
[0408] Figure 1 The bagging device 7 shown is configured to process the dried rubber extruded from the screw-type twin-shaft extrusion dryer 5 and cooled by the cooling device 6 to produce a whole bag. As described above, the screw-type twin-shaft extrusion dryer 5 can extrude the dried rubber into various shapes such as granules, columns, round rods, and sheets, and the bagging device 7 is configured to bag the dried rubber formed into various shapes. The weight and shape of the acrylic rubber bag produced by the bagging device 7 are not particularly limited, and for example, a substantially rectangular acrylic rubber bag of about 20 kg can be produced.
[0409] The bagging device 7 includes, for example, a baler, and the dried rubber after cooling can be compressed by the baler to produce an acrylic rubber bag.
[0410] In addition, when the sheet-shaped dry rubber 10 is produced by the screw-type twin-screw extruder drier 5, an acrylic rubber package on which the sheet-shaped dry rubber 10 is laminated can be produced. Figure 3 The bagging device 7 on the downstream side of the conveyor cooling device 60 shown in the figure is provided with a cutting mechanism for cutting the sheet-like dry rubber 10. Specifically, the cutting mechanism of the bagging device 7 is configured, for example, in such a manner that the cooled sheet-like dry rubber 10 is continuously cut at predetermined intervals to form slice-like dry rubber 16 of a predetermined size. A plurality of slice-like dry rubber 16 cut into a predetermined size by the cutting mechanism are stacked, thereby manufacturing an acrylic rubber bag formed by stacking the slice-like dry rubber 16.
[0411] When manufacturing an acrylic rubber package formed by laminating sliced dry rubber 16, it is preferable to laminate sliced dry rubber 16 at, for example, 40° C. or higher. Laminating sliced dry rubber 16 at 40° C. or higher allows air to be discharged well by further cooling and compression by its own weight.
[0412] Example
[0413] The present invention is described in more detail below with reference to Examples and Comparative Examples. Unless otherwise specified, the "parts", "%" and "ratios" in each example are by weight. In addition, various physical properties were evaluated according to the following methods.
[0414] [Monomer composition]
[0415] Regarding the monomer composition of acrylic rubber, 1 H-NMR confirms the monomer structure of each monomer unit in the acrylic rubber, and the residual activity of the reactive group in the acrylic rubber and the content of each reactive group are confirmed by the following method. In addition, the content ratio of each monomer unit in the acrylic rubber is calculated based on the usage amount of each monomer for the polymerization reaction and the polymerization conversion rate. Specifically, since the polymerization reaction is an emulsion polymerization reaction and its polymerization conversion rate is approximately 100% that the unreacted monomers cannot be confirmed, the content ratio of each monomer unit in the rubber is the same as the usage amount of each monomer.
[0416] [Reactive group content]
[0417] The content of reactive groups in the acrylic rubber or the acrylic rubber molded product is measured by the following method.
[0418] (1) The amount of carboxyl groups is calculated as follows: A sample (acrylic rubber or acrylic rubber molded product) is dissolved in acetone and potentiometric titration is performed using a potassium hydroxide solution.
[0419] (2) The amount of epoxy groups is calculated as follows: a sample is dissolved in methyl ethyl ketone, a prescribed amount of hydrochloric acid is added thereto to react with the epoxy groups, and the amount of residual hydrochloric acid is titrated with potassium hydroxide.
[0420] (3) The amount of chlorine is calculated by completely burning the sample in a combustion flask, absorbing the generated chlorine with water, and titrating with silver nitrate.
[0421] [Ash content]
[0422] The ash content (%) contained in the acrylic rubber or the acrylic rubber molded product is measured in accordance with JIS K6228 A method.
[0423] [Ash content]
[0424] The amount (ppm) of each component in the ash of the acrylic rubber or acrylic rubber molded article was measured by XRF using ZSX Primus (manufactured by Rigaku Corporation) by pressing the ash collected in the above ash content measurement onto a 20 mm diameter titration filter paper.
[0425] [Molecular weight and molecular weight distribution]
[0426] The molecular weight (Mw, Mn, Mz) and molecular weight distribution (Mw / Mn and Mz / Mw) of acrylic rubber are absolute molecular weight and absolute molecular weight distribution measured by the GPC-MALS method. In the GPC-MALS method, a solution prepared by adding lithium chloride at a concentration of 0.05 mol / L and 37% concentrated hydrochloric acid at a concentration of 0.01% to dimethylformamide was used as a solvent.
[0427] The main device, a gel permeation chromatography multi-angle light scattering photometer, was composed of a pump (LC-20ADOpt manufactured by Shimadzu Corporation), a differential refractometer (Optilab rEX manufactured by Wyatt Technologies) and a multi-angle light scattering detector (DAWN HELEOS manufactured by Wyatt Technologies) as a detector.
[0428] Specifically, a multi-angle laser scatterer (MALS) and a differential refractive index detector (RI) are installed in a GPC (Gel Permeation Chromatography) device, and the light scattering intensity and refractive index difference of the molecular chain solution whose size has been distinguished by the GPC device are measured according to the dissolution time, thereby successively calculating the molecular weight and content of the solute. The measurement conditions and measurement methods using the GPC device are as follows.
[0429] Column: TSKgelα-M 2 pieces (Ф7.8mm×30cm, manufactured by Tosoh Corporation)
[0430] Column temperature: 40°C
[0431] Flow rate: 0.8ml / mm
[0432] Sample preparation: 5 ml of a solvent was added to 10 mg of a sample (acrylic rubber or acrylic rubber molded product), and the mixture was slowly stirred at room temperature (dissolution was visually confirmed), and then filtered using a 0.5 μm filter.
[0433] [Glass transition temperature (Tg)]
[0434] The glass transition temperature (Tg) of the acrylic rubber is measured using a differential scanning calorimeter (DSC, product name "X-DSC7000", manufactured by Hitachi High-Tech Sciences, Ltd.).
[0435] [Amount of methyl ethyl ketone insoluble components]
[0436] The methyl ethyl ketone insoluble content (%) of the acrylic rubber or the acrylic rubber molded product is the amount of the insoluble content in methyl ethyl ketone, and is determined by the following method.
[0437] About 0.2 g (Xg) of acrylic rubber or acrylic rubber molded body is weighed and immersed in 100 ml of methyl ethyl ketone. After standing at room temperature for 24 hours, components insoluble in methyl ethyl ketone are filtered out using an 80-mesh wire mesh to obtain a filtrate in which only rubber components soluble in methyl ethyl ketone are dissolved. The filtrate is evaporated and dried to solidify, and the dry solid content (Yg) is weighed and calculated by the following formula.
[0438] Amount of insoluble components in methyl ethyl ketone (%) = 100 × (XY) / X
[0439] [proportion]
[0440] The specific gravity of the acrylic rubber or the acrylic rubber molded product is measured in accordance with Method A of JIS K6268 Cross-linked rubber-Determination of density.
[0441] The measured value obtained by the following measurement method is the density, but the density of water is set to 1Mg / m 3 To obtain the specific gravity. Specifically, the specific gravity of the rubber sample obtained according to JIS K6268 Cross-linked Rubber - Density Measurement Method A is a value obtained by dividing the mass by the volume of the voids containing the rubber sample, and is a value obtained by dividing the density of the rubber sample measured according to JIS K6268 Cross-linked Rubber - Density Measurement Method A by the density of water (when the density of the rubber sample is divided by the density of water, the values are the same and the unit disappears). In detail, the specific gravity of the rubber sample can be obtained according to the following steps.
[0442] (1) Cut a 2.5 g test piece from a rubber sample that has been left to stand at a standard temperature (23°C ± 2°C) for at least 3 hours. Use a thin nylon thread with a mass of less than 0.010 g to hang the test piece from a hook on a chemical balance with an accuracy of 1 mg in such a way that the bottom edge of the test piece is at least 25 mm away from the chemical balance tray. Measure the mass (m1) of the test piece twice in the atmosphere until mg is obtained.
[0443] (2) Next, place the 250 cm 3 Fill a beaker of sufficient capacity with distilled water that has been boiled and then cooled to the standard temperature, immerse the test piece in it, remove the bubbles attached to the surface of the test piece, observe the swing of the balance pointer for a few seconds, confirm that the pointer does not swing slowly due to convection, and measure the mass of the test piece in the water twice in mg (m2).
[0444] (3) In addition, the density of the test piece is less than 1Mg / m 3 When the test piece is floating in water, add a weight to the test piece and measure the mass of the weight in water (m3) and the mass of the test piece and the weight (m4) twice in mg.
[0445] (4) Using the average values of m1, m2, m3, and m4 measured above, the density (Mg / m) was calculated based on the following formula: 3 ), divide the calculated density by the density of water (1.00Mg / m 3 ), calculate the specific gravity of the rubber sample.
[0446] (Density of rubber sample without weight)
[0447] Density = m1 / (m1-m2)
[0448] (Density of rubber sample when using a weight)
[0449] Density = m1 / (m1+m3-m4)
[0450] [Water content]
[0451] The water content (%) was measured in accordance with JIS K6238-1: Oven A (volatile component measurement) method.
[0452] [pH]
[0453] The pH was measured by dissolving 6 g (±0.05 g) of acrylic rubber or acrylic rubber molded product in 100 g of tetrahydrofuran, adding 2.0 ml of distilled water, and confirming that the mixture was completely dissolved. The pH was then measured using a pH electrode.
[0454] [Complex viscosity]
[0455] Regarding the complex viscosity η, a dynamic viscoelasticity measuring device "Rubber Processing Analyzer RPA-2000" (manufactured by Alpha Technology Co., Ltd.) was used to measure the temperature dispersion (40 to 120°C) at a strain of 473% and 1 Hz, and the complex viscosity η at each temperature was obtained. Here, the dynamic viscoelasticity at 60°C in the above-mentioned dynamic viscoelasticity is taken as the complex viscosity η(60°C), and the dynamic viscoelasticity at 100°C is taken as the complex viscosity η(100°C), and the value of the ratio η(100°C) / η(60°C) is calculated.
[0456] [Mooney viscosity (ML1+4, 100℃)]
[0457] The Mooney viscosity (ML1+4, 100°C) was measured in accordance with the physical testing method for uncrosslinked rubber of JIS K6300.
[0458] [Crosslinking]
[0459] The crosslinking property of the rubber sample was determined by calculating the change rate between the breaking strength of the rubber cross-linked product after secondary crosslinking for 2 hours and the breaking strength of the rubber cross-linked product after secondary crosslinking for 4 hours ((breaking strength of the rubber cross-linked product after 4 hours / breaking strength of the rubber cross-linked product after 2 hours)×100) and judging according to the following criteria.
[0460] ◎: Change rate of breaking strength is less than 10%
[0461] ×: The breaking strength change rate is 10% or more.
[0462] [Roller processability]
[0463] The roll processability of the rubber sample was evaluated based on the following criteria by observing the roll winding property and the state of the rubber when the rubber sample was rolled.
[0464] ◎: Easy to knead, easy to wind around the roller, no detachment from the roller was observed, and the surface of the rubber composition after kneading was smooth
[0465] ○: Easy to mix and roll around, no detachment from the roll was observed, and slight irregularities were observed on the surface of a portion of the rubber composition after mixing.
[0466] □: Easy to mix, excellent rollability, and the surface of the rubber composition after mixing is slightly uneven
[0467] △: Easy to mix, slightly poor rollability, rough surface of the rubber composition after mixing
[0468] ×: There is a load on kneading and the roll windability is also poor
[0469] [Banbury processability]
[0470] Regarding the Banbury processability of the rubber sample, the rubber sample was put into a Banbury mixer heated to 50°C and plasticized for 1 minute, and then the compounding agent A of the rubber mixture formula described in Table 1 was put into it. The time until the first stage of rubber mixture integration and the maximum torque value were shown, i.e., BIT (Black Incorporation Time) was measured, and the evaluation was performed using an index with Comparative Example 2 as 100 (the smaller the index, the better the processability).
[0471] [Storage stability evaluation]
[0472] The storage stability of the rubber sample was evaluated by placing the rubber sample in a constant temperature and humidity chamber (SH-222 manufactured by ESPEC Corporation) at 45°C x 80% RH, and calculating the change rate of the water content before and after 7 days of the test. The index was used with Comparative Example 2 being 100 (the smaller the index, the better the storage stability).
[0473] [Water resistance evaluation]
[0474] The water resistance of the rubber sample was evaluated by immersing the cross-linked rubber sample in distilled water at a temperature of 85° C. for 100 hours in accordance with JIS K6258. The volume change rate before and after immersion was calculated according to the following formula and evaluated using an index with Comparative Example 2 being 100 (the smaller the index, the better the water resistance).
[0475] Volume change rate before and after immersion (%) = ((volume of test piece after immersion - volume of test piece before immersion) / volume of test piece before immersion) × 100
[0476] [Compression set resistance]
[0477] The compression set resistance of the rubber sample was evaluated according to JIS K6262 by measuring the compression set rate after leaving the cross-linked rubber sample at 175° C. for 90 hours in a state where the cross-linked rubber sample was compressed by 25%.
[0478] ◎: Compression set rate is less than 15%
[0479] ×: Compression set rate is 15% or more
[0480] [Normal physical property evaluation]
[0481] Normal physical properties of rubber samples The breaking strength, 100% tensile stress and breaking elongation of the rubber cross-linked product of the rubber sample were measured in accordance with JIS K6251 and evaluated according to the following criteria.
[0482] (1) For the breaking strength, 10 MPa or more was evaluated as ◎, and less than 10 MPa was evaluated as ×.
[0483] (2) For 100% tensile stress, 5 MPa or more was evaluated as ◎, and less than 5 MPa was evaluated as ×.
[0484] (3) Regarding the elongation at break, 150% or more was evaluated as ◎, and less than 150% was evaluated as ×.
[0485] [Evaluation of the variation of the amount of insoluble components in methyl ethyl ketone]
[0486] Evaluation of the variation in the amount of methyl ethyl ketone insoluble components of the rubber sample was performed by measuring the amount of methyl ethyl ketone insoluble components at 20 points randomly selected from 20 parts (20 kg) of the rubber sample and evaluating the results according to the following criteria.
[0487] ◎: The average value of the insoluble content of methyl ethyl ketone at 20 locations was calculated, and all 20 locations were within the range of ±3 of the average value.
[0488] 0: The average value of the amount of the insoluble component of methyl ethyl ketone at the 20 measured points was calculated, and all the 20 measured points were within the range of the average value ± 5 (one of the 20 measured points was outside the range of the average value ± 3, but all 20 points were within the range of the average value ± 5)
[0489] ×: The average value of the amount of methyl ethyl ketone insoluble components at 20 locations was calculated, and one of the 20 locations was outside the range of ±5 of the average value.
[0490] [Evaluation of processing stability based on Mooney scorch suppression]
[0491] The Mooney scorch stability of the acrylic rubber composition was evaluated with respect to the cooling rate of the sheet-shaped acrylic rubber extruded from the screw-type twin-screw extrusion dryer described in Japanese Patent No. 6683189.
[0492] [Example 1]
[0493] In a mixing container with a homogenizer, as shown in Table 2-1, 46 parts of pure water, 4.5 parts of ethyl acrylate, 64.5 parts of n-butyl acrylate, 29.5 parts of methoxyethyl acrylate and 1.5 parts of mono-n-butyl fumarate as monomer components, and 1.8 parts of sodium salt of octyloxydioxyethylene phosphate as an emulsifier were added and stirred to obtain a monomer emulsion.
[0494] In a polymerization reaction tank equipped with a thermometer and a stirring device, 170 parts of pure water and 3 parts of the monomer emulsion obtained above were added, cooled to 12° C. under a nitrogen stream, and then 0.00033 parts of ferrous sulfate, 0.02 parts of sodium ascorbate, and 0.2 parts of potassium persulfate as an inorganic free radical generator were added to initiate a polymerization reaction. The temperature in the polymerization reaction tank was maintained at 23° C., and the remaining part of the monomer emulsion was continuously added dropwise over 3 hours. 0.0072 parts of n-dodecyl mercaptan were added 50 minutes after the reaction was initiated, 0.0036 parts of n-dodecyl mercaptan were added 100 minutes later, and 0.4 parts of sodium L-ascorbate were added 120 minutes later. The polymerization reaction was continued. When the polymerization conversion rate reached approximately 100%, a polymerization terminator hydroquinone was added to terminate the polymerization reaction to obtain an emulsion polymer solution.
[0495] Next, in a coagulation tank equipped with a thermometer and a stirring device, the emulsion polymerized liquid obtained above was heated to 80°C and continuously added to 350 parts of a 2% magnesium sulfate aqueous solution (coagulation liquid using magnesium sulfate as a coagulating agent) heated to 80°C and vigorously stirred at 600 revolutions (circumferential speed 3.1 m / s) of the stirring blade of the stirring device, so that the polymer was coagulated to obtain a coagulation slurry containing pellets of acrylic rubber as a coagulated product and water. The pellets were filtered out from the obtained slurry, and water was discharged from the coagulation layer to obtain water-containing pellets.
[0496] 194 parts of hot water (70°C) were added to the coagulation tank where the filtered water pellets remained, and stirred for 15 minutes. After washing the water pellets, the water was drained, and 194 parts of hot water (70°C) were added again, and stirred for 15 minutes to wash the water pellets (the total number of washing times was 2 times). The washed water pellets (water pellet temperature 65°C) were supplied to the screw-type twin-shaft extrusion dryer 5, dehydrated and dried, and a sheet-shaped dry rubber with a width of 300 mm and a thickness of 10 mm was extruded. Next, a conveyor-type cooling device directly connected to the screw-type twin-shaft extrusion dryer 5 was used to cool the sheet-shaped dry rubber at a cooling rate of 200°C / hour.
[0497] The screw-type twin-shaft extrusion dryer used in Example 1 is composed of one supply barrel, three dehydration barrels (the first to third dehydration barrels), and five drying barrels (the first to fifth drying barrels). The first dehydration barrel is used for drainage, and the second and third dehydration barrels are used for steam discharge. The operating conditions of the screw-type twin-shaft extrusion dryer are as follows.
[0498] Water content:
[0499] · Moisture content of the water-containing pellets after drainage in the first dehydrator barrel: 20%
[0500] · Moisture content of the pellets after steam is exhausted from the 3rd dehydrator barrel: 10%
[0501] · Moisture content of the hydrated pellets after drying in the 5th drying barrel: 0.4%
[0502] Rubber temperature:
[0503] Temperature of the water-containing pellets supplied to the supply barrel: 65°C
[0504] · Temperature of rubber discharged from screw type twin-screw extruder dryer: 140°C
[0505] Set temperature of each barrel:
[0506] ·1st dehydration barrel: 100℃
[0507] · Second dehydration barrel: 120℃
[0508] ·3rd dehydration barrel: 120℃
[0509] ·1st drying barrel: 120℃
[0510] · Second drying barrel: 130℃
[0511] ·3rd drying barrel: 140℃
[0512] ·4th drying barrel: 160℃
[0513] ·5th drying barrel: 180℃
[0514] Operating conditions:
[0515] Screw diameter (D): 132mm
[0516] · Overall length of screw (L): 4620mm
[0517] L / D: 35
[0518] Screw speed: 135rpm
[0519] Vacuum degree of drying barrel: 10kPa
[0520] ·Amount of rubber extruded from the die: 700kg / hour
[0521] Resin pressure of die head: 2MPa
[0522] Maximum torque in screw type twin-shaft extruder dryer: 15N·m
[0523] The extruded sheet-like dried rubber was cooled to 50°C and cut with a cutter, and then stacked into 20 portions (20 kg) before the temperature dropped below 40°C to obtain acrylic rubber (A) (acrylic rubber bag). The reactive group content, ash content, ash content, methyl ethyl ketone insoluble component content, pH, specific gravity, glass transition temperature (Tg), water content, molecular weight, molecular weight distribution, and complex viscosity at 100°C and 60°C of the obtained acrylic rubber (A) were measured and shown in Table 2-2. In addition, a storage stability test of the acrylic rubber (A) was conducted to determine the water content change rate, and the results are shown in Table 2-2.
[0524] Next, 100 parts of acrylic rubber (A) and compounding agent A of "Formulation 1" shown in Table 1 were added using a Banbury mixer and mixed at 50°C for 5 minutes (first stage mixing). The BIT at this time was measured and the Banbury processability of the acrylic rubber was evaluated. The results are shown in Table 2-2.
[0525] Next, the obtained mixture was transferred to a roll at 50°C, and compounding ingredient B of "Formulation 1" was added and mixed (second-stage mixing) to obtain a rubber composition. The roll processability at this time was evaluated, and the results are shown in Table 2-2.
[0526] [Table 1]
[0527]
[0528] ※1: SEAST3 (HAF) in the table is carbon black (produced by Tokai Tanso Co., Ltd.).
[0529] ※2: NOCRAC CD in the table is 4,4′-bis(α,α-dimethylbenzyl)diphenylamine (manufactured by Ouchi Shinko Co., Ltd.).
[0530] ※3: Rhenogran XLA-60 in the table is a vulcanization accelerator (manufactured by LANXESS).
[0531] The obtained rubber composition was placed in a metal mold of 15 cm in length, 15 cm in width and 0.2 cm in depth, and pressed at 180°C for 10 minutes while being pressed at 10 MPa, thereby performing a primary crosslinking. The obtained primary crosslinked product was further heated at 180°C for 2 hours in a Gill oven to perform a secondary crosslinking, thereby obtaining a sheet-like rubber crosslinked product. Then, a 3 cm × 2 cm × 0.2 cm test piece was cut from the obtained sheet-like rubber crosslinked product to evaluate water resistance, compression set resistance and normal physical properties. In addition, the normal physical properties of the sheet-like rubber crosslinked product that was further secondary crosslinked for 2 hours were measured to evaluate the crosslinking property. These results are shown in Table 2-2.
[0532] [Example 2]
[0533] The same procedure as in Example 1 was carried out except that the emulsifier was changed to 1.8 parts of sodium salt of nonylphenoxy hexaoxyethylene phosphate, the amount of potassium persulfate as an inorganic radical generator was changed to 0.21 parts, and the post-addition of n-dodecyl mercaptan as a chain transfer agent was changed to 0.017 parts after 50 minutes, 0.017 parts after 100 minutes, and 0.017 parts after 120 minutes, to obtain acrylic rubber (B), and the various properties were evaluated. These results are shown in Table 2-2.
[0534] [Example 3]
[0535] The monomer components were changed to 48.25 parts of ethyl acrylate, 50 parts of n-butyl acrylate and 1.75 parts of mono-n-butyl fumarate, the emulsifier was changed to 1.8 parts of sodium tridecyloxyhexaoxyethylene phosphate, and the washed water-containing pellets were dried to a water content of 0.4% using a hot air dryer at 160°C to obtain pelletized acrylic rubber, which was then filled into a baler of 300×650×300 mm and compacted at a pressure of 3 MPa for 25 seconds to obtain a bag-shaped acrylic rubber. Acrylic rubber (C) was obtained in the same manner as in Example 1. The various properties of acrylic rubber (C) were evaluated (the compounding ingredients were changed to "Formulation 2"), and the results are shown in Table 2-2.
[0536] [Example 4]
[0537] The same procedure as in Example 3 was followed except that the monomer components were changed to 28 parts of ethyl acrylate, 38 parts of n-butyl acrylate, 27 parts of methoxyethyl acrylate, 5 parts of acrylonitrile and 2 parts of allyl glycidyl ether to obtain acrylic rubber (D), and the various properties were evaluated (the compounding ingredients were changed to "Formulation 3"). The results are shown in Table 2-2.
[0538] [Example 5]
[0539] The same procedure as in Example 3 was followed except that the monomer components were changed to 42.2 parts of ethyl acrylate, 35 parts of n-butyl acrylate, 20 parts of methoxyethyl acrylate, 1.5 parts of acrylonitrile and 1.3 parts of vinyl chloroacetate to obtain acrylic rubber (E), and the various properties were evaluated (the compounding ingredients were changed to "Formulation 4"). The results are shown in Table 2-2.
[0540] [Example 6]
[0541] The monomer components were changed to 48.25 parts of ethyl acrylate, 50 parts of n-butyl acrylate and 1.75 parts of mono-n-butyl fumarate, the emulsifier was changed to 1.8 parts of sodium tridecyloxyhexaoxyethylene phosphate, and the washed water-containing pellets were dried to a water content of 0.4% using a hot air dryer at 160°C to obtain a pelletized acrylic rubber, which was then filled into a baler of 300×650×300 mm and compacted at a pressure of 3 MPa for 25 seconds to obtain a bagged acrylic rubber. Acrylic rubber (F) was obtained in the same manner as in Example 2 except that the above. The various properties of acrylic rubber (F) were evaluated (the compounding ingredients were changed to "Formulation 2"), and the results are shown in Table 2-2.
[0542] [Example 7]
[0543] Except that the monomer components were changed to 28 parts of ethyl acrylate, 38 parts of n-butyl acrylate, 27 parts of methoxyethyl acrylate, 5 parts of acrylonitrile and 2 parts of allyl glycidyl ether, the same procedure as in Example 6 was carried out to obtain acrylic rubber (G), and various properties were evaluated (the compounding ingredients were changed to "Formulation 3"). The results are shown in Table 2-2.
[0544] [Example 8]
[0545] The same procedure as in Example 6 was followed except that the monomer components were changed to 42.2 parts of ethyl acrylate, 35 parts of n-butyl acrylate, 20 parts of methoxyethyl acrylate, 1.5 parts of acrylonitrile and 1.3 parts of vinyl chloroacetate to obtain acrylic rubber (H), and the various properties were evaluated (the compounding ingredients were changed to "Formulation 4"). The results are shown in Table 2-2.
[0546] [Reference Example 1]
[0547] Acrylic rubber (I) was obtained in the same manner as in Example 8 except that the amount of potassium persulfate as an inorganic radical generator was changed to 0.22 parts, no chain transfer agent was added, and no baler was used for baling to obtain a pelletized acrylic rubber. The results are shown in Table 2-2.
[0548] [Comparative Example 1]
[0549] Acrylic rubber (J) was obtained in the same manner as in Reference Example 1 except that a 0.7% magnesium sulfate aqueous solution was added to the stirred emulsion polymerization solution (stirring speed 100 rpm, peripheral speed 0.5 m / s) after the emulsion polymerization to carry out a coagulation reaction, and various properties were evaluated. The results are shown in Table 2-2.
[0550] [Comparative Example 2]
[0551] The emulsifier was changed to 0.709 parts of sodium lauryl sulfate and 1.82 parts of polyoxyethylene lauryl ether, the coagulation liquid was changed to 0.7% sodium sulfate aqueous solution, and the washing method was changed to: 194 parts of industrial water was added to 100 parts of the water-containing pellets after the coagulation reaction, and the water-containing pellets were washed from the coagulation tank after stirring at 25°C for 5 minutes, and then 194 parts of sulfuric acid aqueous solution of pH 3 was added, stirred at 25°C for 5 minutes, and then the water was drained from the coagulation tank, and acid washing was performed once, and then 194 parts of pure water was added and pure water washing was performed once. The same method as Comparative Example 1 was used to obtain acrylic rubber (K), and various properties were evaluated. These results are shown in Table 2-2.
[0552] [Comparative Example 3]
[0553] The same procedure as in Comparative Example 2 was followed except that 0.025 parts of n-dodecyl mercaptan as a chain transfer agent was continuously added to the monomer emulsion, and that the washing of the water-containing pellets was performed by adding 194 parts of industrial water only twice, stirring in a coagulation tank at 25° C. for 5 minutes, and then draining the water from the coagulation tank. Acrylic rubber (L) was obtained and various properties were evaluated. The results are shown in Table 2-2.
[0554] [Table 2-1]
[0555]
[0556] [Table 2-2]
[0557]
[0558] As can be seen from Tables 2-1 and 2-2, the acrylic rubbers (A) to (H) of the present invention are composed of a bonding unit derived from at least one (meth)acrylate selected from alkyl (meth)acrylates and alkoxyalkyl (meth)acrylates, a bonding unit derived from an ion reactive group-containing monomer, and a bonding unit derived from other monomers used as needed, and the weight average molecular weight (Mw) based on the absolute molecular weight and absolute molecular weight distribution measured by the GPC-MALS method is in the range of 1,000,000 to 3,500,000, the z average molecular weight (Mz) is in the range of 1,500,000 to 6,000,000, and the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is in the range of 3.7 to 6.5. They are excellent in crosslinking property, roll processability, compression set resistance, and normal physical properties including strength characteristics, and are also particularly excellent in Banbury processability, storage stability, and water resistance (Examples 1 to 8).
[0559] In addition, as can be seen from Table 2-2, the acrylic rubbers (A) to (L) produced under the conditions of the examples, reference examples and comparative examples of the present application have any ion reactive groups such as carboxyl groups, epoxy groups and chlorine atoms, and the weight average molecular weight (Mw) of the absolute molecular weight measured by the GPC-MALS method exceeds 1 million, and the z average molecular weight (Mz) exceeds 1.5 million, which are large values, so the short-term crosslinking, compression set resistance and normal physical properties including strength characteristics are excellent (Examples 1 to 8, Reference Example 1 and Comparative Examples 1 to 3). However, although the acrylic rubbers (J) to (L) of Comparative Examples 1 to 3 are excellent in crosslinking, compression set resistance and strength characteristics, they are poor in roll processability, Banbury processability, storage stability and water resistance (Comparative Examples 1 to 2), and also poor in roll processability, storage stability and water resistance (Comparative Example 3).
[0560] As can be seen from Table 2-2, regarding roll processability, the larger the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn), the better. In particular, by increasing the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) to 3.7 or more and increasing the weight average molecular weight (Mw) and the z-average molecular weight (Mz) to a specific range, roll processability can be significantly improved without impairing strength properties (comparison of Examples 1 to 8 with Comparative Examples 1 to 3).
[0561] In addition, it can be seen from Table 2-1 and Table 2-2 that the acrylic rubber with wide Mw / Mn, large Mw and Mz, excellent strength characteristics and roll processability can be achieved by reducing the inorganic free radical generator, extending one polymer chain, and adding the chain transfer agent (n-dodecyl mercaptan) batch by batch (Examples 1 to 8). In addition, it can be seen that in order to efficiently expand Mw / Mn, the number of batch post-additions is more important than the difference in the amount of chain transfer agent added in batches. The Mw / Mn of the batch post-addition number of 2 times is wider than that of 3 times (comparison of Examples 3 to 5 and Examples 6 to 8). When the chain transfer agent is added continuously, the expansion of Mw / Mn is small and the improvement of roll processability is limited (Comparative Example 3). This is presumably because, although it is not a complete double peak on the graph of the GPC-MALS method, by adding the chain transfer agent in batches, a high molecular weight component and a low molecular weight component appear, Mw / Mn is expanded, and roll processability is greatly improved. In addition, although not shown in Table 2-1, in the examples of the present application, sodium ascorbate is added as a reducing agent 120 minutes after the polymerization is initiated, thereby easily generating high molecular weight components of acrylic rubber and increasing the effect of widening Mw / Mn by adding the chain transfer agent later.
[0562] As shown in Table 2-2, the acrylic rubbers (A) to (H) of the present invention are excellent in crosslinking, roll processability, compression set resistance and strength characteristics, and are also excellent in Banbury processability, and are also excellent in both roll processability and Banbury processability (Examples 1 to 8). In addition, it can be seen that the Banbury processability of the acrylic rubber is related to the amount of methyl ethyl ketone insoluble components, and the Banbury processability of the acrylic rubber with less methyl ethyl ketone insoluble components is excellent (comparison of Examples 1 to 2, Examples 3 to 8 & Reference Example 1, and Comparative Examples 1 to 3). It can also be seen that the amount of methyl ethyl ketone insoluble components of the acrylic rubber can be reduced by emulsion polymerization in the presence of a chain transfer agent (Examples 3 to 8 and Comparative Example 3), and in particular, when the polymerization conversion rate is increased in order to improve the strength characteristics, the amount of methyl ethyl ketone insoluble components increases sharply, so in Examples 3 to 8 where the chain transfer agent is added in the second half of the polymerization, the generation of methyl ethyl ketone insoluble components can be suppressed. Furthermore, by using a screw-type twin-shaft extrusion dryer to dry the water-containing pellets, the amount of methyl ethyl ketone insoluble components of the acrylic rubber can be significantly reduced, and the Banbury processability of the manufactured acrylic rubber can be greatly improved (comparison between Examples 1 to 2 and Examples 3 to 8). In the present invention, although not shown in this example, it can be confirmed that the amount of methyl ethyl ketone insoluble components that increases sharply during emulsion polymerization without adding a chain transfer agent (Comparative Examples 1 to 2) disappears by melt-kneading in a screw-type twin-shaft extrusion dryer in a state that does not substantially contain water (water content is less than 1% by weight), and the Banbury processability can be greatly improved without impairing the strength characteristics.
[0563] In addition, as shown in Table 2-2, the acrylic rubbers (A) to (H) of the present invention are excellent in crosslinking, roll processability, compression set resistance and strength characteristics, and are also particularly excellent in storage stability (Examples 1 to 8). It is also known that the storage stability of acrylic rubber is closely related to the specific gravity of acrylic rubber. When the specific gravity is high, the acrylic rubber does not contain air and has excellent storage stability (comparison between Examples 1 to 2, Examples 3 to 8 and Comparative Examples 1 to 3). Acrylic rubber with a high specific gravity can be obtained by compressing a pelletized acrylic rubber with a baler to form a bale (Examples 3 to 8), and more preferably by extruding it into a sheet without containing air with a screw-type twin-shaft extrusion dryer, cutting it at a specific temperature, and laminating it to form a bale (Examples 1 to 2). In addition, it is known that in the present invention, in particular, the acrylic rubber bale obtained by laminating acrylic rubber sheets that have been melt-kneaded and dried under reduced pressure can significantly improve the storage stability without impairing the short-time crosslinking, roll processability, compression set resistance, normal physical properties including strength characteristics, and water resistance (Examples 1 to 2). It was also found that, with regard to the storage stability of acrylic rubber, the smaller the ash content and the lower the pH, the more preferable it is (Examples 1 to 8).
[0564] In addition, as shown in Table 2-2, the acrylic rubber (A) to (H) of the present invention has excellent crosslinking properties, roll processability, compression set resistance and strength characteristics, and is also particularly excellent in water resistance (Examples 1 to 8). It can also be seen that the water resistance of acrylic rubber is greatly affected by the ash content, and the ash content in acrylic rubber is greatly affected by the manufacturing conditions, and can be greatly reduced by the following methods: preparing a coagulant-concentrated aqueous solution (coagulation liquid), and vigorously stirring, adding an emulsion polymerization liquid that has been subjected to emulsion polymerization to the coagulation liquid to perform a coagulation reaction; washing with hot water; and drying after dehydrating the water-containing pellets (Comparison of Examples 1 to 2, Examples 3 to 8 and Comparative Example 1). In addition, by increasing the content of phosphorus and magnesium in the ash content and making the ratio of phosphorus to magnesium within a specific range, the water resistance of acrylic rubber can be greatly improved (Comparison of Examples 1 to 8 and Comparative Examples 1 to 3). In addition, regarding the effect of the number of washing times on the ash content in the acrylic rubber, in the case of washing with water at room temperature, the ash content can be reliably reduced up to the third time, but there is almost no difference between the third and fourth times, and the ash content reduction effect is almost not observed after the fourth time. On the other hand, in the case of washing with hot water, the ash content in the acrylic rubber is reduced up to the second time, and the washing effect after the third time is almost not observed.
[0565] Furthermore, for each rubber sample, the variation of the amount of methyl ethyl ketone insoluble components was evaluated by the above-mentioned method. That is, the variation of the amount of methyl ethyl ketone insoluble components of the rubber sample was evaluated by measuring the amount of methyl ethyl ketone insoluble components at 20 points randomly selected from 20 parts (20 kg) of the rubber sample and evaluating it based on the above-mentioned criteria.
[0566] When the acrylic rubbers (A) to (H) obtained in Examples 1 to 8 and the acrylic rubber (J) obtained in Comparative Example 1 as rubber samples were evaluated for the deviation in the amount of the methyl ethyl ketone insoluble component, the results of the acrylic rubbers (A) to (H) were all "◎", and the result of the acrylic rubber (J) was "×".
[0567] This is presumably because the acrylic rubbers (A) to (H) are melt-kneaded and dried in a substantially water-free state (water content of less than 1 wt%) by using a screw-type twin-shaft extruder dryer, and the amount of methyl ethyl ketone-insoluble components is almost eliminated and there is almost no deviation in the amount of methyl ethyl ketone-insoluble components, thereby significantly improving the Banbury processability without impairing the crosslinking property, roll processability, compression set resistance, and normal physical properties including strength characteristics.
[0568] On the other hand, it can be seen that the water-containing pellets produced after emulsion polymerization and coagulation washing under the conditions for producing acrylic rubber (J) in Comparative Example 1 were fed into a screw-type twin-screw extruder dryer under the same conditions as in Example 1 and extrusion dried to obtain an acrylic rubber. The methyl ethyl ketone-insoluble component amount and the methyl ethyl ketone-insoluble component amount deviation measured for the obtained acrylic rubber were substantially the same as those of the acrylic rubber (A), and the Banbury processability was also improved, but the roll processability was still evaluated as "×".
[0569] [Regarding the particle size of the generated water-containing aggregates]
[0570] Regarding the water-containing aggregates generated in the coagulation step of Examples 1 to 8, Reference Example 1 and Comparative Example 1, the ratio of the amount of water-containing aggregates in the range of (1) 710 μm to 6.7 mm (not passing 710 μm, passing 6.7 mm), (2) 710 μm to 4.75 mm (not passing 710 μm, passing 4.75 mm), and (3) 710 μm to 3.35 mm (not passing 710 μm, passing 3.35 mm) to the total amount of water-containing aggregates was measured using a JIS sieve. The results are shown below.
[0571] Example 1: (1) 90 wt%, (2) 90 wt%, (3) 87 wt%
[0572] Example 2: (1) 92 wt%, (2) 91 wt%, (3) 89 wt%
[0573] Example 3: (1) 89 wt%, (2) 87 wt%, (3) 83 wt%
[0574] Example 4: (1) 91 wt%, (2) 90 wt%, (3) 83 wt%
[0575] Example 5: (1) 93 wt%, (2) 91 wt%, (3) 89 wt%
[0576] Example 6: (1) 95 wt%, (2) 89 wt%, (3) 80 wt%
[0577] Example 7: (1) 92 wt%, (2) 92 wt%, (3) 88 wt%
[0578] Example 8: (1) 94 wt%, (2) 93 wt%, (3) 87 wt%
[0579] Reference Example 1: (1) 90 wt%, (2) 89 wt%, (3) 88 wt%
[0580] Comparative Example 1: (1) 15 wt%, (2) 1 wt%, (3) 0 wt%
[0581] From these results, it can be seen that even if the same cleaning is performed, the amount of ash remaining in the acrylic rubber or acrylic rubber bag varies depending on the size of the water-containing particles generated in the coagulation step, and the one with a larger specific ratio of (1) to (3) has a high cleaning efficiency, a reduced ash content, and excellent water resistance (comparison between Examples 3 to 8 and Reference Example 1 and Comparative Example 1 in Table 2-2). In addition, it can be further seen that the water-containing particles with a larger specific ratio of (1) to (3) also have a high ash removal rate when dehydrated by 20% by weight, and can further reduce the ash content and significantly improve the water resistance of the acrylic rubber (comparison between Examples 1 to 2 and Examples 3 to 8). In addition, compared with Reference Example 1, Example 8 shows that the particle size of the water-containing particles generated in the coagulation step is not related to the presence or absence of a chain transfer agent.
[0582] In addition, for reference, in the coagulation process, the emulsion polymerization liquid was added to the coagulation liquid, and the same method as Comparative Example 1 was used (Reference Example 2). In addition, the emulsion polymerization liquid was added to the coagulation liquid, and the coagulant concentration of the coagulation liquid was changed from 0.7 wt % to 2 wt %, and the same method as Comparative Example 1 was used (Reference Example 3), and the particle size ratio of the generated water-containing aggregates and the ash content in the acrylic rubber were measured. Their results are shown below. In addition, when the stirring number of the coagulation liquid of Reference Example 3 was changed from 100 rpm to 600 rpm, the circumferential speed was increased from 0.5 m / s to 3.1 m / s, and the conditions were changed to violent rotation conditions, the same conditions as Reference Example 1 were obtained.
[0583] Reference Example 2: (1) 90 wt%, (2) 55 wt%, (3) 22 wt%, ash content 0.55 wt%
[0584] Reference Example 3: (1) 91 wt%, (2) 70 wt%, (3) 40 wt%, ash content 0.41 wt%
[0585] From these results, it can be seen that the acrylic rubbers (A) to (H) of the present invention can significantly improve water resistance while maintaining excellent properties such as crosslinking properties, roll processability, compression set resistance, and normal physical properties including strength properties by setting the particle size of the water-containing particles generated in the coagulation step to a specific range (Examples 1 to 8).
[0586] [Example 9]
[0587] As shown in Table 3-1, the monomer components were changed to 74.5 parts of ethyl acrylate, 17 parts of n-butyl acrylate, 7 parts of methoxyethyl acrylate, 1.5 parts of mono-n-butyl fumarate, and the emulsifier was changed to 1.8 parts of tridecyloxy hexaoxyethylene phosphate sodium salt. The same method as in Example 2 was used to obtain acrylic rubber (M), and various properties were evaluated. The results are shown in Table 3-2. In addition, Table 3-1 shows the water content after dehydration (drainage), maximum torque, specific power, specific energy consumption, shear rate and shear viscosity of the screw-type twin-shaft extrusion dryer.
[0588] [Example 10]
[0589] The same method as in Example 1 was followed except that the monomer components were changed to 74.5 parts of ethyl acrylate, 17 parts of n-butyl acrylate, 7 parts of methoxyethyl acrylate and 1.5 parts of mono-n-butyl fumarate, and the emulsifier was changed to 1.8 parts of sodium tridecyloxyhexaoxyethylene phosphate, to obtain acrylic rubber (N), and the various properties were evaluated. The results are shown in Table 3-2. In addition, Table 3-1 shows the water content after dehydration (drainage), maximum torque, specific power, specific energy consumption, shear rate and shear viscosity of the screw-type twin-shaft extrusion dryer.
[0590] [Example 11]
[0591] The same method as in Example 9 was followed except that the monomer components were changed to 28 parts of ethyl acrylate, 38 parts of n-butyl acrylate, 27 parts of methoxyethyl acrylate, 5 parts of acrylonitrile and 2 parts of allyl glycidyl ether, and the operating conditions of the screw-type twin-shaft extrusion dryer were changed to high shear (maximum torque 45 N·m), to obtain acrylic rubber (O), and the various properties were evaluated (the compounding ingredients were changed to "Formulation 3"). The results are shown in Table 3-2. In addition, Table 3-1 shows the water content after dehydration (drainage), maximum torque, specific power, specific energy consumption, shear rate and shear viscosity of the screw-type twin-shaft extrusion dryer.
[0592] [Example 12]
[0593] The same procedure as in Example 11 was followed except that the monomer components were changed to 48.5 parts of ethyl acrylate, 50 parts of n-butyl acrylate, and 1.5 parts of mono-n-butyl fumarate to obtain acrylic rubber (P), and the various properties were evaluated (the compounding ingredients were changed to "Formulation 1"). The results are shown in Table 3-2. In addition, Table 3-1 shows the water content after dehydration (drainage), the maximum torque, the specific power, the specific energy consumption, the shear rate, and the shear viscosity of the screw-type twin-shaft extrusion dryer.
[0594] [Example 13]
[0595] The same procedure as in Example 11 was followed except that the monomer components were changed to 48.25 parts of ethyl acrylate, 50 parts of n-butyl acrylate, and 1.75 parts of mono-n-butyl fumarate to obtain acrylic rubber (Q), and the various properties were evaluated (the compounding ingredients were changed to "Formulation 2"). The results are shown in Table 3-2. In addition, Table 3-1 shows the water content after dehydration (drainage), the maximum torque, the specific power, the specific energy consumption, the shear rate, and the shear viscosity of the screw-type twin-shaft extrusion dryer.
[0596] [Example 14]
[0597] The same method as in Example 10 was followed except that the monomer components were changed to 28 parts of ethyl acrylate, 38 parts of n-butyl acrylate, 27 parts of methoxyethyl acrylate, 5 parts of acrylonitrile and 2 parts of allyl glycidyl ether, and the operating conditions of the screw-type twin-shaft extrusion dryer were changed to high shear (maximum torque 45 N·m), to obtain acrylic rubber (R), and the various properties were evaluated (the compounding ingredients were changed to "Formulation 3"), and the results are shown in Table 3-2. In addition, Table 3-1 shows the water content after dehydration (drainage), maximum torque, specific power, specific energy consumption, shear rate and shear viscosity of the screw-type twin-shaft extrusion dryer.
[0598] [Example 15]
[0599] The same procedure as in Example 14 was followed except that the monomer components were changed to 48.5 parts of ethyl acrylate, 50 parts of n-butyl acrylate, and 1.5 parts of mono-n-butyl fumarate to obtain acrylic rubber (S), and the various properties were evaluated (the compounding ingredients were changed to "Formulation 1"). The results are shown in Table 3-2. In addition, Table 3-1 shows the water content after dehydration (drainage), maximum torque, specific power, specific energy consumption, shear rate, and shear viscosity of the screw-type twin-shaft extrusion dryer.
[0600] [Example 16]
[0601] The same procedure as in Example 14 was followed except that the monomer components were changed to 48.25 parts of ethyl acrylate, 50 parts of n-butyl acrylate, and 1.75 parts of mono-n-butyl fumarate to obtain acrylic rubber (T), and the various properties were evaluated (the compounding ingredients were changed to "Formulation 2"). The results are shown in Table 3-2. In addition, Table 3-1 shows the water content after dehydration (drainage), the maximum torque, the specific power, the specific energy consumption, the shear rate, and the shear viscosity of the screw-type twin-shaft extrusion dryer.
[0602] [Table 3-1]
[0603]
[0604] [Table 3-2]
[0605]
[0606] As shown in Table 3-1 and Table 3-2, by increasing the maximum torque of the screw-type twin-shaft extrusion dryer to a specific region (set to high shear) and dehydrating and drying the water-containing pellets, the crosslinking property, compression set resistance and strength characteristics of the acrylic rubber of the present invention can be not impaired, and the roll processability can be further significantly improved (comparison of Examples 11 to 16 with Examples 9 to 10). It can be seen that by using a screw-type twin-shaft extrusion dryer, the acrylic rubber composed of high molecular weight components and low molecular weight components, which is emulsion polymerized by adding a chain transfer agent later, is dried at high shear to obtain an acrylic rubber with a balanced molecular weight and molecular weight distribution, thereby significantly improving the roll processability. On the other hand, although not shown in Table 3-1, when the chain transfer agent is excessively added and the molecular weight distribution (Mw / Mn) is excessively broadened, for example, to 10 or more, the low molecular weight components of the acrylic rubber become excessive, and the strength characteristics and compression set resistance deteriorate, which is not preferred.
[0607] The acrylic rubber compositions containing the acrylic rubbers (M) to (S) of Examples 9 to 16 were evaluated for Mooney scorch storage stability by measuring the Mooney scorch time t5 (minutes) at a temperature of 125° C. using the above-mentioned method for evaluating processing stability based on Mooney scorch suppression in accordance with JIS K 6300. The Mooney scorch storage stability was evaluated according to the following criteria. The results were all “◎”, i.e., good results.
[0608] ◎: Mooney scorch time t5 exceeds 2.0 minutes
[0609] ○: Mooney scorch time t5 is 1.5 to 2.0 minutes
[0610] ×: Mooney scorch time t5 is less than 1.5 minutes
[0611] In addition, regarding these acrylic rubbers (M) to (S), the cooling rate of the sheet-shaped dried rubber extruded from the screw-type biaxial extruder dryer was as fast as in Example 1, which was approximately 200° C. / hour, and was 40° C. / hour or more.
[0612] [Release from metal mold]
[0613] The rubber compositions of the acrylic rubbers (M) to (S) obtained in Examples 9 to 16 were pressed into a 10 mm Ø × 200 mm metal mold, and cross-linked at a metal mold temperature of 165°C for 2 minutes. The cross-linked rubber was taken out and the metal mold release properties were evaluated according to the following criteria. At this time, the acrylic rubbers (M) to (S) were all rated "◎", i.e., good.
[0614] ◎: Can be easily released from the metal mold without mold residue
[0615] ○: Can be easily released from the metal mold, but a very small amount of mold residue can be confirmed
[0616] △: Can be easily released from the metal mold, but there is a small amount of mold residue
[0617] ×: Difficult to peel off from the metal mold
[0618] Description of Reference Numerals
[0619] 1: Acrylic rubber manufacturing system
[0620] 3: Solidification device
[0621] 4: Cleaning device
[0622] 5: Screw type twin-shaft extrusion dryer
[0623] 6: Cooling device
[0624] 7: Rubber packaging device
Claims
1. An acrylic rubber comprising a bonding unit derived from a (meth)acrylate, a bonding unit derived from an ion reactive group-containing monomer, and a bonding unit derived from other monomers used as required, The monomer composition of the acrylic rubber is composed of 50 to 99.99% by weight of a bonding unit derived from a (meth)acrylate, 0.01 to 10% by weight of a bonding unit derived from an ion reactive group-containing monomer, and 0 to 40% by weight of a bonding unit derived from other monomers. The (meth)acrylate is selected from at least one of an alkyl (meth)acrylate and an alkoxyalkyl (meth)acrylate. The ion reactive group is at least one functional group selected from a carboxyl group, an epoxy group and a chlorine atom, Based on the absolute molecular weight and absolute molecular weight distribution measured by GPC-MALS method, the weight average molecular weight (Mw) of the acrylic rubber is in the range of 1,500,000 to 2,100,000, the z average molecular weight (Mz) is in the range of 3,000,000 to 4,000,000, and the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is in the range of 4.5 to 6.
5. The acrylic rubber is prepared by emulsion polymerization using a phosphate ester salt or a sulfate ester salt as an emulsifier.
2. The acrylic rubber according to claim 1, in, The measurement solvent of the GPC-MALS method is a dimethylformamide-based solvent.
3. The acrylic rubber according to claim 1 or 2, in, The ion reactive group content is in the range of 0.001 to 5% by weight.
4. The acrylic rubber according to claim 1 or 2, in, The ion-reactive group is a carboxyl group or an epoxy group.
5. The acrylic rubber according to claim 1 or 2, in, The ratio (Mz / Mw) of the z-average molecular weight (Mz) to the weight-average molecular weight (Mw) of the acrylic rubber is in the range of 1.3 to 3.
6. The acrylic rubber according to claim 1 or 2, in, The acrylic rubber has an amount of methyl ethyl ketone-insoluble components of 15% by weight or less.
7. The acrylic rubber according to claim 1 or 2, in, The acrylic rubber has an ash content of 0.5 wt % or less.
8. The acrylic rubber according to claim 1 or 2, in, The total amount of sodium, magnesium, calcium, phosphorus and sulfur in the ash is 50% by weight or more.
9. The acrylic rubber according to claim 1 or 2, in, The acrylic rubber has a complex viscosity at 60° C. ([η]60° C.) of 15,000 [Pa·s] or less.
10. The acrylic rubber according to claim 1 or 2, in, The acrylic rubber has a complex viscosity at 100° C. ([η]100° C.) of 2000 [Pa·s] or more.
11. The acrylic rubber according to claim 1 or 2, in, The ratio of the complex viscosity of the acrylic rubber at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) ([η]100°C / [η]60°C) is 0.5 or more.
12. The acrylic rubber according to claim 1 or 2, in, The ratio ([η]100°C / [η]60°C) of the complex viscosity of the acrylic rubber at 100°C ([η]100°C) to the complex viscosity at 60°C ([η]60°C) is 0.8 or more.
13. The acrylic rubber according to claim 1 or 2, in, The water content of the acrylic rubber is less than 1% by weight.
14. The acrylic rubber according to claim 1 or 2, in, The pH of the acrylic rubber is 6 or less.
15. The acrylic rubber according to claim 1 or 2, in, The acrylic rubber is obtained by coagulating and drying a polymer solution obtained by emulsion polymerization using an alkali metal salt or a metal salt of Group 2 of the periodic table as a coagulant.
16. The acrylic rubber according to claim 1 or 2, in, The acrylic rubber is prepared by melt-kneading and drying after solidification.
17. The acrylic rubber according to claim 16, in, The melt kneading and drying are performed in a state where there is substantially no water.
18. The acrylic rubber according to claim 16, in, The melt-kneading and drying are performed under reduced pressure.
19. The acrylic rubber according to claim 16, in, After the melt-kneading and drying, cooling is performed at a cooling rate of 40° C. / hour or more.
20. A method for producing acrylic rubber, comprising the following steps: A step of emulsifying a monomer component comprising a (meth)acrylate, an ion reactive group-containing monomer, and other copolymerizable monomers used as required, with water and an emulsifier, wherein the (meth)acrylate is at least one selected from the group consisting of an alkyl (meth)acrylate and an alkoxyalkyl (meth)acrylate; A step of performing emulsion polymerization in the presence of a redox catalyst composed of an inorganic free radical generator and a reducing agent until the polymerization conversion rate reaches 90% by weight or more; and The process of adding the chain transfer agent in batches during the polymerization. The method for producing an acrylic rubber produces the acrylic rubber according to any one of claims 1 to 19.
21. The method for producing acrylic rubber according to claim 20, in, The chain transfer agent is added batchwise in the range of 1 to 5 times.
22. The method for producing acrylic rubber according to claim 20 or 21, in, The batchwise post-addition of the chain transfer agent was started after 30 minutes from the initiation of the polymerization.
23. The method for producing acrylic rubber according to claim 20 or 21, in, The amount of the chain transfer agent added in batches at one time is in the range of 0.00005 to 0.5 parts by weight relative to 100 parts by weight of the monomer component.
24. The method for producing acrylic rubber according to claim 20 or 21, in, The chain transfer agent is a thiol compound.
25. The method for producing acrylic rubber according to claim 24, in, The chain transfer agent is an alkyl mercaptan compound having 2 to 20 carbon atoms.
26. The method for producing acrylic rubber according to claim 24, in, The chain transfer agent is an n-alkyl mercaptan compound.
27. The method for producing acrylic rubber according to claim 20 or 21, in, The reducing agent is composed of a combination of at least two reducing agents.
28. The method for producing acrylic rubber according to claim 20 or 21, in, The reducing agent comprises ferrous sulfate.
29. The method for producing acrylic rubber according to claim 20 or 21, in, The reducing agent is ascorbic acid or a salt thereof.
30. The method for producing acrylic rubber according to claim 20 or 21, in, During the polymerization, the reducing agent is added later.
31. The method for producing acrylic rubber according to claim 30, in, The post-addition of the reducing agent was carried out batchwise.
32. The method for producing acrylic rubber according to claim 30, in, The reducing agent added later is ascorbic acid or a salt thereof.
33. The method for producing acrylic rubber according to claim 32, in, The ratio of the amount of ascorbic acid or its salt initially added to the amount of ascorbic acid or its salt subsequently added is in the range of 1 / 9 to 8 / 2 in terms of the weight ratio of "ascorbic acid or its salt initially added" / "ascorbic acid or its salt subsequently added in batches".
34. The method for producing acrylic rubber according to claim 20 or 21, in, The temperature of the emulsion polymerization was controlled below 35°C.
35. The method for producing acrylic rubber according to claim 20 or 21, in, In the emulsion polymerization step, emulsion polymerization is carried out using a phosphate ester salt or a sulfate ester salt as an emulsifier.
36. The method for producing acrylic rubber according to claim 20 or 21, in, The polymerization solution produced in the emulsion polymerization step is coagulated by contacting the polymerization solution with a coagulant containing an alkali metal salt or a metal salt of Group 2 of the periodic table.
37. The method for producing acrylic rubber according to claim 36, in, The polymerization solution generated in the emulsion polymerization step is added to an aqueous solution containing a coagulant and stirred to coagulate the polymerization solution. The coagulant comprises an alkali metal salt or a metal salt of Group 2 of the Periodic Table.
38. The method for producing acrylic rubber according to claim 20 or 21, in, Acrylic rubber is formed by coagulation and drying after emulsion polymerization.
39. The method for producing acrylic rubber according to claim 20 or 21, in, The polymer solution produced in the emulsion polymerization step is brought into contact with a coagulant and coagulated, and then melt-kneaded and dried.
40. The method for producing acrylic rubber according to claim 39, in, The melt-kneading and drying are performed in a state where the mixture contains substantially no water.
41. The method for producing acrylic rubber according to claim 39, in, The melt-kneading and drying are performed under reduced pressure.
42. The method for producing acrylic rubber according to claim 39, in, The melt kneading and drying are performed by a screw-type twin-shaft extrusion dryer.
43. The method for producing acrylic rubber according to claim 42, in, The maximum torque of the screw-type twin-screw extruder dryer during melt kneading and drying is 30 N·m or more.
44. The method for producing acrylic rubber according to claim 42 or 43, in, The specific energy consumption of the screw-type twin-screw extruder dryer during melt kneading and drying is in the range of 0.1 to 0.25 [kw·h / kg].
45. The method for producing acrylic rubber according to claim 42 or 43, in, The specific power of the screw-type twin-screw extruder dryer during melt kneading and drying is in the range of 0.2 to 0.6 [A·h / kg].
46. The method for producing acrylic rubber according to claim 42 or 43, in, The shear rate of the screw-type twin-screw extruder dryer during melt kneading and drying is in the range of 40 to 150 [1 / s].
47. The method for producing acrylic rubber according to claim 42 or 43, in, The shear viscosity of the acrylic rubber in the screw-type twin-screw extruder dryer during melt kneading and drying is in the range of 4000 to 8000 [Pa·s].
48. The method for producing acrylic rubber according to claim 39, in, The melt-kneaded and dried acrylic rubber is cooled at a cooling rate of 40° C. / hour or more.
49. An acrylic rubber molded product obtained by molding the acrylic rubber according to any one of claims 1 to 19.
50. The acrylic rubber molded article according to claim 49, in, The acrylic rubber molded body is an acrylic rubber sheet or an acrylic rubber bag.
51. The acrylic rubber molded article according to claim 49 or 50, in, The acrylic rubber molded body has a specific gravity of 0.8 or more.
52. A rubber composition comprising a rubber component, a filler and a cross-linking agent, wherein the rubber component comprises the acrylic rubber according to any one of claims 1 to 19 or the acrylic rubber molded product according to any one of claims 49 to 51.
53. The rubber composition according to claim 52, in, The filler is a reinforcing filler.
54. The rubber composition according to claim 52, in, The filler is carbon black.
55. The rubber composition according to claim 52, in, The filler is silicon dioxide.
56. The rubber composition according to any one of claims 52 to 55, in, The cross-linking agent is an organic cross-linking agent.
57. The rubber composition according to any one of claims 52 to 55, in, The cross-linking agent is a multi-component compound.
58. The rubber composition according to any one of claims 52 to 55, in, The crosslinking agent is an ionic crosslinking compound.
59. The rubber composition according to claim 58, in, The crosslinking agent is an ion-crosslinking organic compound.
60. The rubber composition according to claim 58, in, The crosslinking agent is a polyionic organic compound.
61. The rubber composition according to any one of claims 52 to 55, in, The crosslinking agent is an ionic crosslinking compound, an ionic crosslinking organic compound or a polyionic organic compound. The ion of the ionic crosslinkable compound, ionic crosslinkable organic compound or polyionic organic compound as the crosslinking agent is at least one ionic reactive group selected from the group consisting of an amino group, an epoxy group, a carboxyl group and a thiol group.
62. The rubber composition according to claim 60, in, The crosslinking agent is at least one polyvalent ion compound selected from the group consisting of polyvalent amine compounds, polyvalent epoxy compounds, polyvalent carboxylic acid compounds and polyvalent thiol compounds.
63. The rubber composition according to any one of claims 52 to 55, in, The content of the crosslinking agent is in the range of 0.001 to 20 parts by weight relative to 100 parts by weight of the rubber component.
64. The rubber composition according to any one of claims 52 to 55, in, The rubber composition further includes an antioxidant.
65. The rubber composition according to claim 64, in, The antioxidant is an amine antioxidant.
66. A method for producing a rubber composition, comprising mixing a rubber component comprising the acrylic rubber according to any one of claims 1 to 19 or the acrylic rubber molded product according to any one of claims 49 to 51, a filler, and an antioxidant as needed, and then mixing a crosslinking agent.
67. A cross-linked rubber product obtained by cross-linking the rubber composition according to any one of claims 52 to 65.
68. The cross-linked rubber according to claim 67, in, The crosslinking of the rubber composition is performed after molding.