Hot-rolled wire rod for galvanized steel wire of bridge cables with a grade of 2100MPa or above and production method thereof

By using high-C and high-Si composition systems in the production of bridge cable wires, adding trace carbon nitride-forming elements, and combining controlled rolling and online water bath cooling technology, the production problems and high-energy of high-strength steel wires in the existing technology are solved. The problem of consumption and low efficiency has achieved high-efficiency and low energy consumption of high-strength steel wire production.

CN116145036BActive Publication Date: 2024-11-29JIANGYIN XINGCHENG GOLD MATERIALS CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310091571.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-10
Publication Date
2024-11-29
Estimated Expiration
2043-02-10

AI Technical Summary

Technical Problem

It is difficult to produce bridge cable wires with high strength ≥2100MPa grade, and the traditional coil production process consumes high energy, has large waste discharge, and is low production efficiency, which cannot meet the needs of low-energy-consuming and green environmentally friendly production.

Method used

Using high C and high Si composition systems, add trace amounts of Nb, V, Ti and other carbon nitride forming elements, and use controlled rolling and controlled cooling methods during the rolling process, combined with online water bath cooling technology to improve the material anti-hydrogen cracking properties and strength.

Benefits of technology

The galvanized steel wire of bridge cable with tensile strength ≥2100MPa and twisting times ≥8 times was achieved, and the specification range of the strip was expanded to Φ11.0mm-Φ16.5mm, which reduced the hydrogen content and improved the work hardening rate of the material and Resistant to hydrogen-induced delayed cracking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116145036B_ABST
    Figure CN116145036B_ABST
Patent Text Reader

Abstract

The present invention relates to a hot-rolled wire rod for galvanized steel wire of bridge cables of 2100MPa grade and above and a production method, wherein the content of sorbite structure of the wire rod is ≥95%, the range of tensile strength through the wire rod is ≤70MPa according to the wire rod circle diameter of 1.1-1.2 meters, the tensile strength is above 1550MPa, the tensile strength of the galvanized steel wire obtained after drawing and galvanizing is ≥2100MPa, and the torsion test is carried out according to the GB / T239.1 standard, and the torsion index is ≥8 times. A high C and high Si component system is adopted, and a trace amount of Nb, V, and Ti carbonitride forming elements are added, which improves the strength and plasticity while also improving the resistance to hydrogen-induced cracking. The molten steel is subjected to converter smelting + LF refining + RH vacuum degassing + large round billet continuous casting + intermediate round billet rolling and finishing + round billet controlled rolling and controlled cooling + wire rod online water bath toughening treatment. The controlled rolling and controlled cooling methods are used in the production process of wire rod, which matches the online water bath cooling speed very well, so that the specification range of the produced wire rod is expanded to Φ11.0mm-Φ16.5mm, breaking through the technical bottleneck of the previous production of this level of wire rod using salt bath or lead bath toughening heat treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of wire rod steel, and in particular relates to a hot-rolled wire rod for high-strength bridge cable steel wire with a grade of ≥2100MPa and a production method. Background Art

[0002] As the country's demand for road construction node projects becomes more and more stringent, my country has many gullies, many mountains, and the Yangtze River and the Yellow River run through the terrain, which puts higher requirements on bridge construction. Data shows that for every 100MPa increase in the strength of the bridge cable wire, its deadweight can be reduced by 10%, the cable diameter is reduced accordingly, and the windward resistance is reduced accordingly, which will reduce the impact of wind force and wind direction on the bridge, and also improve the safety of the bridge.

[0003] With the continuous advancement of technology in steel enterprises and downstream metal products processing industries, domestic wire rods can now stably produce 1860MPa, 1960MPa, 2000MPa and 2060MPa grade galvanized aluminum steel wires. The wire rods currently produced domestically for the manufacture of this type of galvanized steel wires use a high C and high Si composition system, and the toughening treatment generally uses the Stelmor air cooling process or online air cooling + offline salt bath or lead bath heat treatment process. Due to the low cooling rate of air-cooled wire rods, the sorbite content of the organization is below 90%, the tensile strength of the wire rod fluctuates around 100MPa, the upper limit of the wire rod production specification can only reach around Φ13.5mm, and the produced wire rod can only meet the 1860MPa level. There are no online mass production cases of wire rods at the 2100MPa level in China. The wire rod online air cooling + wire rod offline salt bath (or lead bath) heat treatment process is adopted, which requires the wire rod to be air-cooled to room temperature, and then the wire rod is laid out in a straight line and continuously fed into the heating furnace for re-austenitization and heating. After being taken out of the furnace, it is cooled in a salt bath or lead bath. This process has high energy consumption, large production waste emissions, and low production efficiency, which does not conform to the development trend of low-energy consumption and green environmentally friendly production.

[0004] The patent information currently published in China is: the patent document with publication number CN 102719643A involves quickly placing the hot-rolled wire rod into a lead tank or a salt tank for sorbitization of the wire rod. The wire rod cooling medium is liquid lead or liquid salt, which is highly corrosive to the equipment and has certain pollution to the environment. The produced wire rod is mainly used to manufacture wire ropes and has not been actually applied to the production of galvanized steel wire for bridge cables.

[0005] The patent document with publication number CN 107587071A involves steel for bridge cables with a capacity of ≥2100MPa and a production method. The patent wire rod composition C: 0.92-0.94%, Si: 0.70-0.90%, Mn: 0.45-0.55%, P≤0.01%, S≤0.01%, Cr: 0.07-0.09%, Nb: 0.04-0.08%, Al: 0.16-0.20%, N: 0.0040-0.0080%, B: 0.0010-0.0015%, Zr: 0.0020-0.0050%. The composition is designed as a high Si composition design, with trace amounts of Cr, Nb, B, and Zr added. The production process involves longitudinal flame cutting of the continuous casting billet, which increases the production cost, and it is recorded that the wire rod is air-cooled after spinning and is ready for use.

[0006] The patent document with publication number CN107299280A involves heat-treated wire rods for 2000MPa cable steel wire and production methods. The patent wire rod composition C: 0.85%-1.0%, Si: 0.80-1.50%, Mn: 0.30-0.80%, P≤0.015%, S≤0.010%, Cr: 0.20-0.80%, Al: 0.010-0.080%. The patent composition is designed as a high Si composition design, and certain alloy elements such as Mn, Cr, and Al are added. The production process is that the continuous casting billet is rolled into a wire rod, and the wire rod is reheated and austenitized and then heat treated in an offline salt bath, which has high production costs and low production efficiency.

[0007] The patent document with publication number CN 102936688B describes a wire rod for bridge cables with a tensile strength of ≥2000MPa and a production method. The chemical composition of the wire rod is C: 0.95-1.20%, Si: 0.10-0.48%, Mn: 0.60-1.00%, P≤0.025%, S≤0.015%, Cr: 0.10-0.50%, Al: 0.05-0.15%, N: 0.0100-0.0300%. It adopts a medium and low Si composition design, and appropriately adds Mn, Cr, Al alloys, and non-alloy elements N. The production process is that the continuous casting billet is rolled into a wire rod, and the wire rod is air-cooled after spinning.

[0008] The patent document with publication number CN 107354380 A describes a steel for bridge cables with a tensile strength ≥ 2300MPa and a production method. The smelting composition of the molten steel is: C: 0.92-0.94%, Si: 0.70-1.00%, Mn: 0.45-0.55%, V: 0.16-0.20%, Al: 0.16-0.20%, and trace amounts of Cr, B, and Zr are added; in addition, the production process does not involve specific measures such as controlled rolling and controlled cooling of wire rods. The cooling process uses air cooling, and the next step of processing is carried out after the wire rods are air-cooled.

[0009] The patent document with publication number CN 107686944 A describes a steel for bridge cables with a tensile strength of ≥2500MPa and a production method, and the smelting composition involved is: C: 1.21-1.25%, Si: 1.10-1.50%, Mn: 0.20-0.50%, Cr: 0.07-0.09%, Ti: 0.06-0.08%, Al: 0.16-0.20%, and trace amounts of B and Zr are added. The controlled rolling process of the wire rod is not disclosed in the document, and the wire rod is air-cooled.

[0010] The patent document with publication number CN 109468530A describes a hot-rolled wire rod and a production method for galvanized steel wire for bridge cables above 2000MPa, and the smelting components involved are C: 0.90-1.10%, Si: 0.20-0.60%, Mn: 0.30-0.90%, P≤0.010%, S≤0.005%, Cr: 0.10-0.40%, Al: 0.010-0.070%, V: 0.02-0.15%, Cu: ≤0.05%, Ca: 20-40ppm, N: 20- 90ppm, the rest are Fe and inevitable residual elements; in the composition of the above hot rolled wire rod, the C content is further 0.95-1.10%; the Si content is further 0.40-0.60%; the Mn content is further 0.60-0.90%; the Cr content is further 0.30-0.40%; the Al content is further 0.030-0.070%; the V content is further 0.05-0.15%; the Ca content is 25-40ppm by weight, and the N content is 40-90ppm by weight.

[0011] The wire rods manufactured by the above-listed existing technologies have small production specifications and are difficult to meet the high-end market demand in terms of strength. Summary of the invention

[0012] The purpose of the present invention is to make up for the performance deficiencies of existing products. Starting from the chemical composition and production process, the wire rod composition design adopts a high C and high Si composition system, and a trace amount of Nb, V, and Ti carbonitride forming elements are added at the same time. While improving the material's resistance to hydrogen-induced cracking, a controlled rolling and controlled cooling method is adopted during the rolling process, breaking through the technical bottleneck of using salt bath or lead bath toughening heat treatment in the past to produce wire rods of this level. On this basis, trace alloy elements are added to refine the grains during the rolling process, and controlled rolling and controlled cooling measures are adopted to well match the online water bath cooling speed, so that the specification range of the produced wire rod is expanded to Φ11.0mm-Φ16.5mm. The tensile strength of the galvanized steel wire for bridge cables produced using the wire rod is ≥2100MPa, and the number of torsions is ≥8 times, filling the international gap.

[0013] The technical solution adopted by the present invention is: a hot-rolled wire rod for galvanized steel wire of bridge cables of grade 2100MPa and above, with a troostite content of ≥95% and the rest being pearlite. The tensile strength range is ≤70MPa based on a wire rod diameter of 1.1-1.2 meters, and the tensile strength of the wire rod is above 1550MPa. The tensile strength of the galvanized steel wire obtained after drawing and galvanizing is ≥2100MPa. Torsion testing is performed according to GB / T239.1 standard, and the torsion index is ≥8 times, or even ≥12 times.

[0014] The wire rod specifications produced in this application are Φ11.0mm-Φ16.5mm.

[0015] The chemical composition of the wire rod of the present application includes high carbon, high silicon, high manganese, trace chromium, trace aluminum, and also includes elements precipitated as carbides, nitrides, and carbonitrides: one or more of niobium, vanadium, and titanium. The range content of calcium and nitrogen in the chemical composition must be precisely controlled, and the minimum content of phosphorus, sulfur, copper, and hydrogen must be precisely controlled. The weight percentages of specific chemical elements are: C: 0.80-1.20%, Si: 0.60 -1.50%, Mn: 0.60-0.90%, Cr: 0.10-0.70%, Al: 0.010-0.070%, V: 0.02-0.20%, Nb: 0.005-0.035%, Ti: 0.005-0.025%, Ca: 20-40ppm, N: 20-90ppm, P≤0.015%, S≤0.006%, Cu: ≤0.05%, H≤1.0ppm, and the others are Fe and unavoidable residual elements.

[0016] The mechanism of action of adding chemical elements to the wire rod for bridge cables of 2100MPa and above of the present invention is as follows:

[0017] Carbon (C): Carbon is the main strengthening element in steel. On the one hand, it plays the role of interstitial solid solution strengthening; on the other hand, it forms compounds with carbide-forming elements and precipitates, playing the role of precipitation strengthening. The weight percentage of carbon in the present invention is 0.80-1.20%, which fully considers the dissolution amount of carbon in austenite and the subsequent XDWP water bath cooling intensity. The stronger the cooling capacity, the more it can inhibit the precipitation of secondary cementite, which plays the role of solid solution strengthening to improve the strength of the wire rod.

[0018] Silicon (Si): Silicon has a very high solid solution strengthening ability and can significantly improve the cold work hardening index of steel. During the phase transformation process, Si is mainly distributed in ferrite, thereby improving the stability of cementite, hindering the spheroidization of cementite lamellae during the hot-dip galvanizing of cold-drawn steel wire, and reducing the strength loss during the hot-dip galvanizing process. The weight percentage of Si in the present invention is 0.60-1.50%.

[0019] Manganese (Mn): Manganese tends to be distributed in the cementite phase. When the distance between Si-Mn atoms is small, there is a strong repulsion between Si and Mn atoms. When the Si content in ferrite is high, Mn atoms are repelled into the cementite. Manganese is easy to segregate in steel and is easy to form low-temperature martensitic structure during cooling. Considering the above aspects, the weight percentage of Mn in the present invention is 0.60-0.90%.

[0020] Chromium (Cr): Chromium addition can improve the stability of cementite, hinder the spheroidization of cementite lamellae during the hot-dip galvanizing process of cold-drawn steel wire, and reduce the strength loss during the hot-dip galvanizing process. Adding Cr elements can also refine the pearlite lamella spacing, which is beneficial to the improvement of the plasticity index of the wire rod, and at the same time improve the work hardening rate of the material during the wire drawing process. Chromium can reduce the activity of carbon in steel and is also a carbide-forming element, so it can increase the diffusion activation energy of carbon in steel. The weight percentage of carbon in the present invention is 0.10-0.70%.

[0021] Vanadium (V): Vanadium is a carbide-forming element. At the end of rolling and during phase transformation, vanadium can play a role in grain refinement and precipitation strengthening. The latest research shows that the carbon (nitride) phase of vanadium can capture hydrogen atoms in the matrix, forming a hydrogen trap to avoid the harm of hydrogen in high-strength steel. The weight percentage of vanadium in the present invention is 0.02-0.20%.

[0022] Titanium (Ti): Titanium plays a role in grain refinement, precipitation strengthening, improving wire rod strength, and improving resistance to hydrogen-induced cracking. The precipitation temperature of titanium compounds is relatively high. During the smelting process, the type and particle size of titanium compounds can be controlled by controlling the addition time of titanium wire and the titanium and nitrogen content. However, adding too much titanium is likely to form large particles of titanium nitride precipitation. Taking all factors into consideration, the weight percentage of titanium in the present invention is 0.005-0.025%.

[0023] Niobium (Nb): The precipitation temperature of niobium compounds is mostly concentrated in the rolling temperature range of the billet. Appropriate addition and application of controlled rolling and controlled cooling measures can control the precipitation size and type of such compounds and improve the comprehensive performance of the wire rod. Generally speaking, the effects of niobium in different states are as follows: (1) Undissolved niobium. In actual production, in order to reduce deformation resistance, a higher heating temperature is generally used. The amount of undissolved niobium is small, and it has little effect on precipitation strengthening and grain refinement; (2) Niobium in solid solution. Niobium dissolved in steel interacts with dislocations in austenite, increases the recrystallization temperature of austenite, and prevents austenite grains from recrystallizing. (3) Niobium carbon and niobium nitride formed by precipitation. This compound is fine and dispersed. Together with niobium in solid solution, it inhibits recrystallization and prevents grain growth. Dispersed precipitation at low temperatures plays a role in precipitation strengthening. Taking all factors into consideration, the weight percentage of niobium in the present invention is 0.005-0.035%.

[0024] Nitrogen (N): Nitrogen mainly plays a role in aging strengthening, and forms nitride precipitation with the added trace alloys Nb, V, Ti, and Al, which plays a role in reducing grain size and precipitation strengthening. In the present invention, the nitrogen content is controlled to be 20ppm-90ppm.

[0025] Calcium (Ca): Calcium modifies the inclusions formed during the steelmaking process, forming a low-melting-point, easily deformable 7Al2O3·12CaO compound to ensure castability while improving the plasticity of the wire rod and subsequent drawing performance. Considering the Al2O3 content during the steelmaking process, the Ca addition amount is 20-40ppm.

[0026] Phosphorus, sulfur, copper, hydrogen (P, S, Cu, H): These four elements are harmful elements in the wire rod of the present invention, and their contents should be strictly controlled.

[0027] Another object of the present invention is to provide a method for producing the above-mentioned hot-rolled wire rod for galvanized steel wire of bridge cables of 2100 MPa or above, comprising the following steps:

[0028] (1) Molten steel smelting

[0029] Select high-grade iron ore for molten iron smelting, control the harmful element content in the molten iron, perform KR pretreatment on the molten iron to reduce the P and S content; use converter to make steel, control the steel tapping end point C ≥ 0.35%; LF furnace refining for deoxidation and inclusion removal, and the refining white slag retention time ≥ 15min; RH control high vacuum ≥ 15min, and ensure the total vacuum time ≥ 20min;

[0030] (2) Billet continuous casting

[0031] The large round billet with diameter of 600mm or above is used, and the tundish is heated by electromagnetic induction. The superheat of each furnace is stably controlled at ≤15℃. The crystallizer is equipped with electromagnetic stirring and electromagnetic stirring at the end of solidification. The billet is produced by light reduction.

[0032] (3) Intermediate billet production

[0033] The surface of the round billet is peeled and ground to eliminate surface defects. After finishing, high-temperature diffusion is performed: the round billet is heated to above 1220℃, and the total heating time is more than 13 hours to ensure the uniformity of the cross-sectional composition of the billet. The billet is rolled into an intermediate billet of φ150-200mm. The intermediate billet is fully kept warm for more than 48 hours within the hydrogen expansion temperature range; while reducing the hydrogen content in the material, the surface hardness is reduced, which is more conducive to subsequent finishing. The billet is slowly cooled (for example, with a hood) to room temperature before surface finishing is performed to ensure that the surface quality of the billet meets internal control requirements.

[0034] (4) Billet controlled rolling

[0035] Reheat the intermediate billet at a temperature of 1000-1200°C, with a total heating time of ≥3 hours. After the billet is taken out of the furnace, it is rolled under control, with a start rolling temperature of 950-1150°C. In the rough rolling pass, a large reduction ratio is used for rolling, with a cumulative rolling ratio of ≥4 (the rough rolling is accumulated over 7 rolling mills). After the rough rolling, it is turned to finishing rolling. The start rolling temperature is 900-970°C, and the final rolling temperature is 800-950°C.

[0036] (5) Wire rod controlled cooling

[0037] The wire rod is treated with XDWP water bath toughening heat treatment online. The wire rod is treated according to the following process parameters:

[0038] (5.1) The wire rod spinning temperature is 800℃-950℃;

[0039] (5.2) After the wire rod is spun, it is subjected to online thermal relaxation, the thermal relaxation temperature is 790-940°C, and the thermal relaxation time is 10s-60s;

[0040] (5.3) After online thermal relaxation, the wire rod is cooled in a water bath at a temperature of 80°C-100°C and a cooling time of 20s-100s;

[0041] (5.4) The outlet water temperature of the wire rod after cooling in the XDWP water bath is 500℃-650℃;

[0042] (5.5) After the wire rod is discharged from the water, it is heat-collected and coiled. The heat collection temperature is 230℃-530℃, and the heat collection and insulation time is 30min to 3h, which plays a role in reducing the hydrogen content and shortening the natural aging.

[0043] As one of the preferred embodiments of the present application, in step (2), electromagnetic induction heating is used in the intermediate ladle during the continuous casting process, the superheat of the molten steel in each furnace is controlled to be ≤15°C, electromagnetic stirring is used in the crystallizer, electromagnetic stirring is used at the end of solidification, and the billet is lightly pressed down.

[0044] As one of the preferred embodiments of the present application, in step (3), the hydrogen expansion temperature of the intermediate billet is in the range of 200-600°C.

[0045] As one of the preferred embodiments of the present application, in step (5), 2%-10% by weight of sodium chloride process salt is added to the XDWP cooling water in step (5.4), and the cooling rate reaches 10-30°C / s. The temperature difference of the wire rod in the same circle in step (5.5) is controlled at ≤25°C, and the diameter of the wire rod circle is 1.1-1.2 meters; the heat collection method of step (5.5) is tunnel-type slow cooling with insulation function.

[0046] As one of the preferred embodiments of the present application, in step (4), during the rolling process, the billet is cooled by setting up a cooling water tank (the cooling water volume and water pressure are adjusted to achieve the purpose of online cooling of the billet) to control the temperature of the billet to meet the temperature design requirements of each rolling node.

[0047] Compared with the prior art, the advantages of the present invention are:

[0048] (1) The chemical composition of the wire rod adopts high carbon, high silicon, high manganese, low chromium and low aluminum as the basic elements. On this basis, trace amounts of carbonitride-forming elements such as niobium, vanadium and titanium are added to refine the grains and improve the strength while taking into account the effect of improving the resistance to hydrogen-induced delayed cracking. The total hydrogen content in the wire rod has been reduced from the previous 1.5ppm to the current 1.0ppm or less, and the peak diffusion temperature of hydrogen is about 100℃ higher than that of the wire rod with the traditional composition system. The addition of Ca during the smelting process plays a role in modifying the inclusions; the precipitation of large particles of TiN is avoided, and the precipitation of fine and dispersed nitrides is obtained, which plays a role in precipitation strengthening.

[0049] (2) The production of wire rods in this patent adopts a combination of controlled rolling and controlled cooling technologies, which breaks through the technical deficiency of using an offline lead bath or salt bath with only controlled cooling but no controlled rolling when high silicon content design is adopted at home and abroad. When this patent produces wire rods for 2100MPa-grade bridge cable steel wire, the difference from the production process in previous patents is that the production of wire rods in this patent adopts a controlled rolling and controlled cooling process production method. After the billet is taken out of the furnace, it undergoes rough rolling, fine rolling, final rolling and wire drawing. The deformation amount of each rolling pass is accurately designed, the rough rolling ratio is ≥4, and the temperature of each node is strictly controlled within the fluctuation range. On the above basis, after the wire rod is spun, an online XDWP water bath (with a certain amount of industrial salt added) is used for controlled cooling to ensure the cooling effect of large-size wire rods.

[0050] (3) Continuous casting is produced using large round billets of 600 mm or more, and the round billets are finished and high-temperature diffused before being rolled into round billets of 150 mm to 200 mm. The raw materials in the present invention adjust and optimize the previous continuous casting large square billets into continuous casting round billets for rolling production. The advantages are that the problem of poor quality of the square billet corners is greatly improved, and the uniformity of the cross-sectional composition of the billet is improved. The surface of the round billet is peeled before reheating to avoid the problems of peeling leakage and depth not meeting the requirements due to excessive unevenness of the four corners of the square billet; the finished round billet is reheated to avoid the problem of high silicon steel decarburization caused by the large curvature of the square billet corners.

[0051] (4) After spinning, the wire rod is thermally relaxed online before entering the water. Depending on the specifications, the thermal relaxation time is 10s-60s, which is used to strengthen the precipitation of carbides and nitrides before phase transformation and fully reduce the dislocation density.

[0052] (5) After the wire rod is out of water, the heat collection temperature range is controlled at 230℃-530℃, and the insulation time is controlled at 30min-3h. This plays the role of online annealing, eliminating internal stress, shortening natural aging, and fully releasing the diffusible hydrogen in the wire rod.

[0053] (6) The water bath cooling medium is a mixture of water and a certain amount of industrial salt. The cooling rate of the wire rod is increased by 5-10°C / s. While inhibiting the precipitation of high-carbon steel network cementite, the tensile strength of the wire rod is increased by 20MPa under the same composition.

[0054] (7) The content of troostite is as high as 95% or more (the rest is pearlite). The tensile strength range is ≤70MPa (the diameter of the wire rod is 1.1-1.2 meters), and there is no abnormal structure such as bainite and martensite.

[0055] (8) The tensile strength of the wire rod of the present application is above 1500 MPa. After drawing and galvanizing, the tensile strength of the galvanized steel wire is ≥2100 MPa. The torsion test is carried out according to GB / T239.1 standard, and the number of torsion times is ≥8 times. All other indicators meet the standard requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 This is a metallographic microstructure picture of XDWP water bath toughening heat treatment in Example 1 of the present invention;

[0057] Figure 2 This is a SEM image of the XDWP water bath toughening heat treatment in Example 2 of the present invention. DETAILED DESCRIPTION

[0058] The present invention is further described in detail below in conjunction with examples. The examples are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0059] No limitation to the scope of the present invention is intended.

[0060] Example 1

[0061] The steelmaking plant produces grade XCQ2100LS1. The molten steel is smelted in a converter, refined by LF, and degassed by RH. The high vacuum degree is controlled for 15 minutes, and the total vacuum time is guaranteed to be 20 minutes. The weight percentage of the smelting chemical composition is:

[0062] C: 0.80-1.20%, Si: 0.60 -1.50%, Mn: 0.60-0.90%, Cr: 0.10-0.70%, Al: 0.010-0.070%, V: 0.02-0.20%, Nb: 0.005-0.035%, Ti: 0.005-0.025%, Ca: 20-40ppm, N: 20-90ppm, P≤0.015%, S≤0.006%, Cu: ≤0.05%, H≤1.0ppm, others are Fe and inevitable residual elements.

[0063] The superheat of molten steel is 15℃. Continuous casting is produced with Ф600mm large round billet. The billet is produced by light reduction and hot charging process. After the surface of the round billet is finished, high-temperature diffusion treatment is carried out. The furnace is heated to 1250℃ for 14 hours and rolled into a round steel (intermediate billet) with a size of φ200mm. After rolling, the billet is pit cooled and the surface of the billet is finished at room temperature. It is then put into the heating furnace for secondary heating at 1200℃ and the holding time is 3.0 hours. After the billet is taken out of the furnace, controlled rolling production is carried out. The temperatures of each node of rolling are as follows: the billet starting rolling temperature is in the range of 950℃-1150℃, the billet rolling ratio in the rough rolling stage is controlled at ≥4, the temperature entering the finishing mill is controlled at 900-970℃, the final rolling temperature is controlled at the temperature range of 800℃-950℃, the wire laying temperature is controlled at the temperature range of 800℃-950℃, and the wire rod rolling specification is Φ15.0mm.

[0064] After the wire rod is rolled into the specified specifications through high-speed wire rod, it is spun and subjected to online XDWP water bath toughening treatment according to the following process parameters: the wire rod spun temperature is 800℃-950℃; the wire rod is subjected to online thermal relaxation after spun, the thermal relaxation temperature is 790℃-940℃, and the thermal relaxation time is 10s-30s; the wire rod is cooled by water bath after online thermal relaxation, the water bath temperature is 80℃-100℃, the water bath cooling time is 20s-100s, and 6%wt NaCl industrial salt is added to the water bath; the outlet water temperature of the wire rod after XDWP water bath cooling is 500℃-650℃. The heat collection temperature after the wire rod is discharged from the water is 330℃-530℃, and the tunnel-type slow cooling and heat preservation time is controlled at 3 hours.

[0065] The wire rod produced by the water bath toughening treatment of the present invention has a tensile strength Rm≥1500MPa, a cross-sectional shrinkage Z≥30%, a 1.2-meter circle diameter pass range ≤70MPa, a metallographic structure sorbite content ≥95%, and the rest is pearlite. The specification of the drawn steel wire is Φ7.0mm, the tensile strength Rm of the steel wire after galvanizing is ≥2150MPa, and the number of twisting times of the steel wire after galvanizing is ≥8 times.

[0066] Example 2

[0067] The steelmaking plant produces grade XCQ2200LS1. The molten steel is smelted in a converter, refined by LF, and vacuum degassed by RH. The high vacuum degree is controlled for 17 minutes, and the total vacuum time is guaranteed to be 25 minutes. The weight percentage of the smelting chemical composition is:

[0068] C: 0.85-0.99%, Si: 0.95-1.25%, Mn: 0.60-0.90%, Cr: 0.25-0.35%, Al: 0.015-0.035%, V: 0.04-0.10%, Nb: 0.005-0.025%, Ti: 0.005-0.015%, Ca: 20-40ppm, N: 20-90ppm, P≤0.015%, S≤0.006%, Cu: ≤0.05%, H≤1.0ppm, others are Fe and inevitable residual elements.

[0069] The superheat of molten steel is 10℃-15℃. The continuous casting adopts Ф600mm large round billet shape and adopts light pressing process. The furnace heating temperature is 1220℃, the holding time is 15 hours, and the intermediate billet size is rolled into round steel with a size of φ150mm. After rolling, the billet is pit cooled, and the billet surface is finished at room temperature. Then it is put into the heating furnace for secondary heating. The heating temperature is 1180℃, and the holding time is 3.5 hours. After the billet is taken out of the furnace, controlled rolling production is carried out. The temperatures of each rolling node are as follows: the rough temperature of the billet is in the range of 1100℃-1120℃, the temperature entering the finishing mill is controlled at 950-970℃, the final rolling temperature is controlled at the temperature range of 900℃-950℃, the wire laying temperature is controlled at the temperature range of 900℃-950℃, and the wire drawing temperature is controlled at the temperature range of 900℃-950℃. The wire rod rolling specification is Φ14.0mm.

[0070] After the wire rod is rolled into the specified specifications through high-speed wire rod, it is spun and subjected to online XDWP water bath toughening treatment according to the following process parameters: the wire rod spun temperature is 900℃-950℃; the wire rod is subjected to online thermal relaxation after spun, the thermal relaxation temperature is 890℃-940℃, and the thermal relaxation time is 50s; after online thermal relaxation, the wire rod is cooled by water bath, the water bath temperature is 80℃-100℃, the water bath cooling time is 20s-100s, and 10%wt NaCl industrial salt is added to the water bath; after the wire rod is cooled by XDWP water bath, the outlet water temperature is 550℃-650℃. After the wire rod is discharged from the water, the heat collection temperature is 350℃-530℃, and the tunnel-type slow cooling and heat preservation time is 2 hours.

[0071] The wire rod produced by the water bath toughening treatment of the present invention has a tensile strength Rm≥1550MPa, a cross-sectional shrinkage Z≥29%, a pass range ≤50MPa, and a metallographic structure sorbite content ≥95%. The specification of the drawn steel wire is Φ6.2mm, the tensile strength Rm of the galvanized steel wire is ≥2250MPa, and the number of torsion times of the galvanized steel wire is ≥8 times.

[0072] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.

Claims

1. A method for producing hot-rolled wire rods for galvanized steel wires for bridge cables of 2100MPa or above, characterized in that: The weight percentage of chemical elements of the wire rod is: C: 0.80-1.20%, Si: 0.60 -1.50%, Mn: 0.60-0.90%, Cr: 0.10-0.70%, Al: 0.010-0.070%, V: 0.02-0.20%, Nb: 0.005-0.035%, Ti: 0.005-0.025%, Ca: 20-40ppm, N: 20-90ppm, P≤0.015%, S≤0.006%, Cu: ≤0.05%, H≤1.0ppm, and the others are Fe and unavoidable residual elements; The production method comprises the following steps, (1) Molten steel smelting It includes molten iron pretreatment + converter steelmaking + LF refining + RH vacuum degassing. The molten iron is pretreated with KR to reduce the P and S content; converter steelmaking is used to control the steel tapping end point C ≥ 0.35%; LF furnace refining is used for deoxidation and inclusion removal, and the refining white slag is kept for ≥ 15 minutes; RH controls the high vacuum degree for ≥ 15 minutes, and ensures that the total vacuum time is ≥ 20 minutes; (2) Billet continuous casting The large round billet with diameter of 600mm or above is used, and the tundish is heated by electromagnetic induction. The superheat of each furnace is stably controlled at ≤15℃. The crystallizer is equipped with electromagnetic stirring and electromagnetic stirring at the end of solidification. The billet is produced by light reduction. (3) Intermediate billet production The surface of the round billet is peeled and ground to eliminate surface defects, and then high-temperature diffusion is performed after finishing: the heating temperature of the round billet is above 1220℃, and the total heating time is more than 13 hours to ensure the uniformity of the cross-sectional composition of the billet. The billet is rolled into an intermediate billet of φ150-200mm, and the intermediate billet is fully kept warm for more than 48 hours within the hydrogen expansion temperature range; (4) Billet controlled rolling Reheat the intermediate billet at a heating temperature of 1000°C-1200°C, with a total heating time of ≥3 hours. After the billet is taken out of the furnace, it is subjected to controlled rolling, with a start rolling temperature of 950°C-1150°C. In the rough rolling stage, a large reduction ratio is used for rolling, and after rough rolling, it is turned to finish rolling, with a start rolling temperature of 900-970°C and a final rolling temperature of 800°C-950°C. (5) Online toughening and controlled cooling of wire rod The wire rod is processed according to the following process parameters: (5.1) The wire rod spinning temperature is 800℃-950℃; (5.2) After the wire rod is spun, it undergoes online thermal relaxation, with the thermal relaxation temperature being 790-940°C and the thermal relaxation time being 10s-60s; (5.3) After online thermal relaxation, the wire rod is cooled in a water bath at a temperature of 80°C-100°C and a cooling time of 20s-100s; (5.4) After the wire rod is cooled in an XDWP water bath, the outlet water temperature is 500℃-650℃. 2%-10% by weight of sodium chloride industrial salt is added to the XDWP cooling water, and the corresponding water bath cooling rate is 10-30℃ / s; (5.5) After the wire rod is discharged from the water, it is heat-collected and rolled. The heat collection and insulation method is a tunnel-type slow cooling with insulation function. The heat collection temperature is 230℃-530℃, and the heat collection and insulation time is 30min to 3h. The temperature difference of the wire rod in the same circle is controlled at ≤25℃, and the wire rod circle diameter is 1.1-1.2 meters.

2. The method according to claim 1, characterized in that: In step (3), the hydrogen expansion temperature of the intermediate billet is in the range of 200-600°C.

3. The method according to claim 1, characterized in that: In step (4), during the rolling process, a cooling water tank is provided to cool the billet so as to control the temperature of the billet to meet the temperature design of each rolling node; in step (4), the rolling ratio of the rough rolling 7 passes is ≥4.

4. The method according to claim 1, characterized in that: The content of troostite structure in wire rod is ≥95%, and the rest is pearlite structure. The range of tensile strength is ≤70MPa based on the wire rod diameter of 1.1-1.2 meters, and the tensile strength of wire rod is above 1550MPa. The tensile strength of galvanized steel wire obtained after drawing and galvanizing is ≥2100MPa. Torsion test is carried out according to GB / T239.1 standard, and the torsion index is ≥8 times.

5. The method according to claim 1, characterized in that: The production specifications of wire rod are Φ11.0mm-Φ16.5mm.

Citation Information

Patent Citations

  • Heat processing technology of high-carbon carbon steel coil rod for steel wire rope

    CN102719643A

  • Wire with tensile strength>=2000MPa for bridge cable and production method

    CN102936688B

  • Thermal treatment wire rod for 2000MPa-grade cable steel wire and production method

    CN107299280A

  • Steel for bridge cable with tensile strength larger than or equal to 2300 MPa and production method

    CN107354380A

  • Steel with tensile strength of no less than 2100 MPa and for bridge cable, and production method thereof