Methods for determining the stability of polysilicon doped production lines and related end-use equipment
By analyzing the ECV curves of polycrystalline silicon wafers using the electrochemical differential capacitance (ECV) method, the problem of inaccurate measurement using the four-probe method was solved, enabling the determination of the stability of polycrystalline silicon doped production lines and improving the accuracy of test results and the stability of the production lines.
Patent Information
- Application Number
- CN202310165168.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-24
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-02-24
AI Technical Summary
In existing technologies, the four-probe method for measuring the sheet resistance of polycrystalline silicon wafers is inaccurate, making it impossible to detect production line defects in a timely manner, thus affecting the quality of polycrystalline silicon wafers and production line efficiency.
The electrochemical differential capacitance (ECV) method is used to obtain the ECV curve of silicon wafers. By analyzing the parameters in the ECV curve, such as the tunneling oxide thickness, phosphorus doping concentration and poly-Si thickness, it is possible to determine whether there are any abnormalities in the silicon wafer quality, thereby determining the stability of the production line.
It provides an accurate and simple method to detect production line instability in a timely manner, thereby improving the quality of polycrystalline silicon wafers and production line efficiency.
Smart Images

Figure CN116151007B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polysilicon production technology, and in particular to a method for determining the stability of a polysilicon doping production line and related terminal equipment. Background Technology
[0002] During the production of polysilicon, instability in the production line can lead to defective polysilicon wafers, affecting production line efficiency and yield.
[0003] In existing technologies, four probes are typically used to test the sheet resistance of silicon wafers after phosphorus doping and annealing in production lines. However, due to the influence of poly-Si layer thickness, silicon wafer resistivity, phosphorus diffusion process, etc., the test results are inaccurate and cannot detect production line defects in a timely manner. Summary of the Invention
[0004] This invention provides a method and terminal equipment for determining the stability of a polysilicon doped production line, in order to solve the problem that the four-probe method results are inaccurate and cannot detect production line defects in a timely manner.
[0005] In a first aspect, embodiments of the present invention provide a method for determining the stability of a polysilicon doped production line, comprising:
[0006] Obtain the ECV curves of the first preset number of silicon wafers picked up from the target production line;
[0007] Based on the ECV curves of a first preset number of silicon wafers, determine whether there are any quality abnormalities in the first preset number of silicon wafers;
[0008] If an anomaly is found, the target production line is determined to be unstable.
[0009] In a second aspect, embodiments of the present invention provide a terminal device, including a memory, a processor, and a computer program stored in the memory and executable on the processor. When the processor executes the computer program, it implements the steps of the first aspect or any possible implementation of the first aspect.
[0010] This invention provides a method and terminal equipment for determining the stability of a polysilicon doped production line. The method includes: acquiring the ECV curves of a first preset number of silicon wafers picked up from the target production line; determining whether the quality of the first preset number of silicon wafers is abnormal based on the ECV curves; and determining that the target production line is unstable if an abnormality is found. This invention analyzes the silicon wafers based on their ECV curves to determine whether the production line has abnormalities; the test results are accurate, and the method is simple and effective. Attached Figure Description
[0011] To more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0012] Figure 1 This is a schematic diagram of the circuit structure for measuring sheet resistance using a four-probe method provided in an embodiment of the present invention;
[0013] Figure 2 This is a flowchart illustrating the implementation of a method for determining the stability of a polysilicon doped production line according to an embodiment of the present invention.
[0014] Figure 3 This is a comparison chart of the parameters of the sealing rings;
[0015] Figure 4 This is a schematic diagram of the ECV curve corresponding to the thermal oxidation method;
[0016] Figure 5 This is a schematic diagram of the ECV curve corresponding to the PECVD method;
[0017] Figure 6 This is a schematic diagram of the structure of the device for determining the stability of a polysilicon doped production line provided in an embodiment of the present invention;
[0018] Figure 7 This is a schematic diagram of a terminal device provided in an embodiment of the present invention. Detailed Implementation
[0019] In the following description, specific details such as particular system architectures and techniques are set forth for illustrative purposes and not for limitation, in order to provide a thorough understanding of the embodiments of the invention. However, those skilled in the art will understand that the invention can be implemented in other embodiments without these specific details. In other instances, detailed descriptions of well-known systems, apparatuses, circuits, and methods are omitted so as not to obscure the description of the invention with unnecessary detail.
[0020] To make the objectives, technical solutions, and advantages of the present invention clearer, specific embodiments will be described below in conjunction with the accompanying drawings.
[0021] Existing technologies typically employ the four-probe method to measure the sheet resistance of silicon wafers, referencing... Figure 1The principle of four-probe sheet resistance measurement is that current flows out from probe 1 and back from probe 2. However, due to the blocking effect of the PN junction, it can only pass through the diffusion layer. Since the N-type wafer itself is doped with phosphorus, and the poly film on the back is also doped with phosphorus, albeit at different concentrations, it creates a high / low field (n / n+), lacking the blocking effect of a PN junction. Therefore, the current flowing from probe 1 not only passes through the diffusion layer but also enters the silicon substrate, leading to inaccurate measurement results. For example, when the silicon wafer is polycrystalline silicon on the back of a TOPCon cell, the quality of the tunneling oxide layer is closely related to the quality of the back passivation. The function of the tunneling oxide layer is to prevent phosphorus atoms from diffusing into the substrate, and sheet resistance testing using the four-probe method cannot clearly determine its quality.
[0022] Based on this, see Figure 2 The method for determining the stability of a polysilicon doped production line provided in this embodiment of the invention is described in detail below:
[0023] S101: Obtain the ECV curves of the first preset number of silicon wafers picked up on the target production line;
[0024] S102: Determine whether there is any quality abnormality in the first preset number of silicon wafers based on the ECV curves of the first preset number of silicon wafers;
[0025] S103: If an anomaly is found, the target production line is determined to be unstable.
[0026] Electrochemical Capacitance Voltage (ECV) – This method utilizes an electrolyte to form a Schottky barrier and applies a forward bias (P-type) or reverse bias (N-type with illumination) to the semiconductor surface to etch away the electrolyzed material. An automated device repeats the "etch-measurement" cycle to obtain a measurement curve. Then, by applying Faraday's law and integrating the etching current, the etching depth can be continuously obtained. Although this method is destructive, theoretically its measurement depth is infinite.
[0027] ECV curves can reflect parameters such as the tunneling oxide layer and phosphorus doping concentration of silicon wafers. Therefore, in this embodiment of the invention, the ECV curves of silicon wafers at monitoring points on the target production line are measured. Analysis of the ECV curves of the silicon wafers determines whether there are any abnormalities in their quality, thereby determining whether the target production line is stable. The method is simple and effective, and the test results are accurate, accurately reflecting the stability of the production line, making it suitable for practical applications. For example, 2 groups (each group containing a first preset number of silicon wafers) / 3 groups of silicon wafers can be selected daily for monitoring, with intervals of 12 hours / 8 hours, to promptly identify and address any instability in the target production line.
[0028] Specifically, the above methods can be applied to silicon wafers with poly-Si+ phosphorus diffusion deposited by LPCVD, poly-Si+ annealed silicon wafers with in-situ phosphorus doping deposited by PECVD, and poly-Si+ annealed silicon wafers with in-situ phosphorus doping deposited by PVD.
[0029] In one possible implementation, prior to S101, the following may also be included:
[0030] 1. Cleaning
[0031] Pick up the first preset number of silicon wafers (transfer wafers) at the preset monitoring point of the target production line and perform HF cleaning to remove the PSG layer on the surface after phosphorus diffusion, so as to avoid affecting the ECV test results.
[0032] The specific cleaning process is as follows: ① HF cleaning: solution concentration 14-20% (wt%), time: 5-15 min (adjusted according to the oxidation time after diffusion); ② Water washing, the purpose is to wash away the acid on the surface. After water washing, it is necessary to observe the water repellency of the silicon wafer surface. The surface should be water repellent (indicating that the PSG layer has been completely cleaned); ③ Drying.
[0033] 2. ECV test
[0034] (1) Test sampling requirements: center point + 4 points at a position 5-7cm away from the center point along the diagonal of the silicon wafer, for a total of 5 points.
[0035] (2) The electrolyte is ammonium bifluoride. Ammonium ions have a non-polar symmetrical structure and very low leakage current. Compared with water-based electrolytes, its performance is better.
[0036] (3) The sealing ring is the channel through which the electrolyte contacts the semiconductor, and its size determines the contact area. The sealing ring with a bore diameter of 1.13 mm is used in this method. However, the sealing ring will corrode, deform, bulge, and wear over a long period of use, which will change its contact area and affect the calculation results.
[0037] refer to Figure 3 The sealing ring comes in two sizes, large and small, which can be selected according to the actual application requirements. For example, when the silicon wafer is polycrystalline silicon on the back of an N-type TOPCon cell, the test area is 0.112 cm². 2 You can choose a larger ring.
[0038] (4) The applied pressure can be set to 200 cN.
[0039] (5) The reference electrode is used to provide a stable potential. The reference voltage and current for the electrochemical cell are provided by a potentiostat. The reference electrode in this method can be a silver chloride electrode.
[0040] (6) The resistance between the contacts of the electrodes attached to the silicon wafer surface reflects the conductivity. Before measurement, the contacts are first burned by discharging a capacitor and applying a 40V DC voltage. Burning heats the electrodes and semiconductor, removing obstructions such as organic matter. Then, a scanning voltage of -0.7V to +0.7V is applied, and the system measures the generated current, plotting an ohm curve to obtain the contact resistance. The curve should be linear; if it is non-linear, an error will be reported. The normal range of contact resistance is 0-500 ohms.
[0041] (7) Before starting IV and CV measurements, first measure the electrostatic potential between the semiconductor contact and the reference electrode. This value is significant, affecting the starting voltage and scan range during subsequent CV measurements. The electrostatic potential range is limited as follows: the electrostatic potential should be between -3V and 1V, and the current should be <0.05mA / cm².
[0042] (8) For N-type silicon wafers, there are two adjustment modes depending on the concentration.
[0043] Set the concentration to "1E20++": First, use the voltage control mode "adjust voltage" with an initial voltage of 1.5V. Adjust the voltage to maintain the corrosion current at a level greater than 4mA / cm². When the concentration drops below 5E19, switch to the light control mode "adjust lamp" and adjust the light intensity to maintain the corrosion current at a level greater than 4mA / cm².
[0044] Set the concentration to "1E19-1E20": Start directly using the light control mode "adjust lamp", with lamp power = 100%.
[0045] (9) During the corrosion process, silicon and impurities enter the electrolyte, and hydrogen gas is released, generating bubbles. It is necessary to remove the gas and liquid promptly, otherwise the corrosion rate will be affected. Therefore, it is necessary to control the pump's on / off time during the corrosion process. The control mode selection is as follows:
[0046] Before start: After each CV measurement is completed, the pump cycle is executed.
[0047] During etch: Pump circulation is performed during each corrosion step (circulation occurs while corrosion is underway).
[0048] Relax: Performs pump circulation during the relaxation period after each corrosion cycle. The system default is Relax.
[0049] During testing, it is common to encounter a situation where corrosion does not proceed, meaning the current is very low and the corrosion rate is extremely low. This phenomenon often occurs when there are impurities blocking the corrosion interface or air bubbles accumulating. In this case, corrosion can be paused, and a "Duringetch" operation can be performed to remove the electrolyte and air bubbles from the interface. After replacing the electrolyte with fresh electrolyte, corrosion will resume normally.
[0050] (10) After the corrosion is completed, different frequency voltages are applied to measure the capacitance, carrier concentration and barrier width.
[0051] ① Frequency range: The frequency range set on the device is divided into low frequency, medium frequency, high frequency and ultra-high frequency.
[0052] To obtain good measurement results, the three frequency settings within a range of this method have significant differences, for example, 2nd = 2 * 1st, 3rd = 2 * 2nd.
[0053] ②Applied voltage: To obtain the CV curve, a series of AC voltages need to be applied.
[0054] Starting voltage Vstart: The starting voltage is generally taken near the electrostatic potential. For silicon and electrolyte in this method, its value is generally -0.7V.
[0055] Voltage step Vstep: typically taken as 0.05V
[0056] Scan range: Vmax = Vstart + 6Vstep, Vmin = Vstart - 6Vstep
[0057] Scan direction: Vstart---Vmax----Vmin
[0058] Voltage VN: This value is taken from the starting voltage value or its adjacent value, generally the center value of the scanning range. The slope of 1 / C2 corresponding to this voltage is taken to obtain the value of N.
[0059] (11) Setting the amplitude measurement
[0060] The maximum amplitude should not exceed 50% of the scan step size. The scan step size Vstep is typically 50 mV, which means the maximum amplitude is 25 mV.
[0061] In one possible implementation, S102 may include:
[0062] S1021: Determine whether there are any abnormalities in the tunneling oxide layer of the first preset number of silicon wafers based on the ECV curves of the first preset number of silicon wafers; and / or
[0063] S1022: Determine whether there is an abnormality in the phosphorus doping concentration of the first preset number of silicon wafers based on the ECV curves of the first preset number of silicon wafers; and / or
[0064] S1023: Determine whether there is an abnormality in the poly-si thickness of the first preset number of silicon wafers based on the ECV curve of the first preset number of silicon wafers.
[0065] The two most commonly used processes in production lines are thermal oxidation and PECVD.
[0066] Thermal oxidation, a growth method involving high-temperature oxygen and bulk silicon, produces a thicker (~1.5 nm) and denser oxide layer with strong phosphorus atom barrier properties. The corresponding ECV curve shows a rapid decrease in phosphorus concentration after high-concentration poly-Si doping, down to approximately E17 of the bulk silicon doping concentration. (ECV curve reference...) Figure 4 .
[0067] PECVD (Plasma Enhanced Chemical Vapor Deposition) uses oxygen and silane to grow silicon oxide under plasma conditions. The oxide layer is thin (~1.2 nm) and sparse, resulting in weak phosphorus atom blocking ability. By adjusting the phosphorus doping and annealing processes, the phosphorus doping concentration after poly-Si is made into a stepped pattern. ECV curves are referenced. Figure 5 Compared to the n / n+ field in the thermal oxidation process, adjusting the back field to an n / n+ / n++ field by modifying the doping and annealing process (annealing purpose: activation and advancement) can further improve the back passivation effect.
[0068] In this embodiment of the invention, appropriate parameters can be selected based on the process method to determine production line anomalies. For example, the thermal oxidation method can determine production line anomalies by considering the tunneling oxide layer, phosphorus doping concentration, and poly-Si thickness. Any parameter indicating an anomaly can be used to determine that the production line is abnormal.
[0069] In one possible implementation, the silicon wafer is grown with a tunneling oxide layer using a thermal oxidation method; S1021 may include:
[0070] 1. For each silicon wafer, determine the second and third inflection points in the ECV curve of the silicon wafer and determine the slope of the straight line between the second and third inflection points; determine the tunneling parameters of the silicon wafer based on the slope corresponding to the silicon wafer and the standard slope, and determine whether the tunneling parameters of the silicon wafer are greater than the first preset value.
[0071] 2. If the tunneling parameters of more than a second preset number of silicon wafers in the first preset number are all greater than the first preset value, then it is determined that the tunneling oxide layer of the first preset number of silicon wafers is abnormal.
[0072] refer to Figure 4 The silicon wafers are grown using a thermal oxidation method to create a tunneling oxide layer. The first inflection point in the ECV curve represents the first concentration inflection point of phosphorus doping on the silicon wafer surface after silicon base treatment. A sharp decrease occurs between the second and third inflection points, reflecting the thickness of the tunneling oxide layer. In this embodiment of the invention, based on the inherent characteristics of the silicon wafer, the slope between the second and third inflection points determines whether the tunneling oxide layer is abnormal. If more than a second preset number of silicon wafers out of a first preset number are abnormal, it indicates a production line malfunction, requiring investigation.
[0073] Specifically, the second preset quantity can be set according to actual application needs. For example, if the first preset quantity is 3, then the second preset quantity can be 1.
[0074] The standard slope is the slope of the straight line between the second and third inflection points obtained after ECV testing of a normal silicon wafer. It is used as a standard value to compare with the test silicon wafers (a first preset number of silicon wafers) to determine whether the test silicon wafers are abnormal.
[0075] In one possible implementation, determining the tunneling parameters of the silicon wafer based on the slope corresponding to the silicon wafer and the standard slope may include:
[0076] Based on the slope corresponding to the silicon wafer, the tunneling parameters of the silicon wafer are determined using the first formula;
[0077] The first formula can be:
[0078]
[0079] Where m1 is the tunneling parameter of the silicon wafer, k0 is the standard slope, and k1 is the slope corresponding to the silicon wafer.
[0080] In one possible implementation, the first preset value can be 15%.
[0081] The tunneling parameter reflects the deviation ratio between the thickness of the tunneling oxide layer of the tested silicon wafer and the thickness of the tunneling oxide layer of the standard silicon wafer. If the deviation is too large, it indicates that the tunneling oxide layer of the silicon wafer is abnormal.
[0082] In one possible implementation, the silicon wafer is grown with a tunneling oxide layer using a thermal oxidation method; S1022 may include:
[0083] 1. For each silicon wafer, determine the first inflection point in the ECV curve of the silicon wafer, and take the ordinate of the first inflection point as the phosphorus doping concentration of the silicon wafer; determine the first doping parameter of the silicon wafer based on the phosphorus doping concentration of the silicon wafer and the standard phosphorus doping concentration, and determine whether the first doping parameter of the silicon wafer is greater than the second preset value.
[0084] 2. If the first doping parameter of the first preset number of silicon wafers is greater than the second preset value, then it is determined that the phosphorus doping concentration of the first preset number of silicon wafers is abnormal.
[0085] refer to Figure 4 The first inflection point (point C) represents the phosphorus doping concentration on the silicon wafer surface. The standard phosphorus doping concentration is the ordinate of the first inflection point of a normal silicon wafer, used as a standard value for comparison with the test silicon wafer. If the deviation ratio of the phosphorus doping concentration between each test silicon wafer and the standard silicon wafer (the first doping parameter) exceeds the second preset value, then the phosphorus doping concentration of the silicon wafer is determined to be abnormal.
[0086] In one possible implementation, determining the first doping parameter of the silicon wafer based on the phosphorus doping concentration and a standard phosphorus doping concentration may include:
[0087] The first doping parameter of the silicon wafer is determined based on the phosphorus doping concentration of the silicon wafer and the standard phosphorus doping concentration, combined with the second formula.
[0088] The second formula can be:
[0089]
[0090] Where m2 is the first doping parameter of the silicon wafer, N0 is the standard phosphorus doping concentration, and N1 is the phosphorus doping concentration of the silicon wafer.
[0091] In one possible implementation, the second preset value can be 10%.
[0092] In one possible implementation, the silicon wafer is grown with a tunneling oxide layer using a vapor deposition method; S1022 may include:
[0093] 1. For each silicon wafer, determine the first, second, third, fourth, and fifth inflection points in its ECV curve; based on these inflection points, determine whether the phosphorus doping concentration of the silicon wafer meets the preset conditions.
[0094] 2. If the first doping parameters of the first preset number of silicon wafers do not meet the preset conditions, then it is determined that the phosphorus doping concentration of the first preset number of silicon wafers is abnormal.
[0095] The method of growing tunneling layers by PECVD (corresponding to the growth method of poly-Si as PECVD or PVD, and the phosphorus doping method as in-situ doping) is not able to achieve true tunneling because the tunneling layer grown by PECVD itself has poor density. Therefore, processes such as adjusting the phosphorus doping concentration and annealing are used to adjust the back field to n / n+ / n++ field. The phosphorus doping concentration corresponding to different depths becomes the main control point.
[0096] refer to Figure 5 Point D represents the phosphorus doping concentration on the silicon wafer surface, point F represents the first concentration inflection point after phosphorus atoms pass through the tunneling layer into the silicon substrate, and the slopes between points E and F, and between points G and H, also reflect the phosphorus doping concentration. Therefore, in this embodiment of the invention, the phosphorus doping concentration of the silicon wafer is determined based on the five inflection points.
[0097] In one possible implementation, the preset conditions can be:
[0098] and
[0099] Where k2 is the slope between the second and third inflection points, k 20 k2 is the standard slope; k3 is the slope between the fourth and fifth inflection points. 30 N is the standard slope corresponding to k3; N2 is the ordinate of the first inflection point, N 20 N is the standard phosphorus doping concentration corresponding to the first inflection point; N3 is the ordinate of the third inflection point, N 30 This represents the standard phosphorus doping concentration corresponding to the third inflection point.
[0100] In one possible implementation, S1023 may include:
[0101] 1. For each silicon wafer, determine the first and second inflection points in the ECV curve of the silicon wafer, and take the difference between the x-coordinate of the first inflection point and the x-coordinate of the second inflection point as the poly-si test thickness of the silicon wafer; and obtain the poly-si target thickness of the silicon wafer according to the preset ratio, and determine the absolute value of the difference between the poly-si target thickness and the preset thickness.
[0102] 2. If the absolute value of the difference between the first preset number of silicon wafers and the fourth preset number of silicon wafers is greater than the preset difference, then it is determined that the poly-Si thickness of the first preset number of silicon wafers is abnormal.
[0103] Since phosphorus doping is saturated in poly-Si, reference Figure 4 The difference between the x-coordinates of points A and C represents the poly-Si thickness. However, since the ECV test principle is based on etching and measurement, and the density of poly-Si differs significantly from that of silicon wafers, the test results do not accurately reflect the actual thickness. Therefore, the poly-Si thickness obtained from the ECV curve is used as the poly-Si test thickness. This target poly-Si thickness is multiplied by a preset ratio and compared with the standard value (preset thickness) to determine if the poly-Si thickness of the silicon wafer is abnormal.
[0104] The preset ratio can be used to analyze the ECV curve of a normal silicon wafer to obtain the poly-si test thickness, and then measure the actual poly-si thickness of the silicon wafer. The ratio is the preset ratio.
[0105] It should be understood that the sequence number of each step in the above embodiments does not imply the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present invention.
[0106] The following are device embodiments of the present invention. For details not described in detail, please refer to the corresponding method embodiments described above.
[0107] Figure 6 A schematic diagram of the apparatus for determining the stability of a polysilicon doped production line provided in an embodiment of the present invention is shown. For ease of explanation, only the parts relevant to the embodiment of the present invention are shown, and are described in detail below:
[0108] like Figure 6 As shown, the apparatus for determining the stability of a polysilicon doped production line includes:
[0109] Parameter acquisition module 21 is used to acquire the ECV curves of the first preset number of silicon wafers picked up on the target production line;
[0110] The curve analysis module 22 is used to determine whether there is any quality abnormality in the first preset number of silicon wafers based on the ECV curves of the first preset number of silicon wafers.
[0111] The exception output module 23 is used to determine that the target production line is unstable if an exception exists.
[0112] In one possible implementation, the curve analysis module 22 may include:
[0113] The first judgment unit is used to determine whether there is an abnormality in the tunneling oxide layer of the first preset number of silicon wafers based on the ECV curve of the first preset number of silicon wafers.
[0114] The second judgment unit is used to determine whether there is an abnormality in the phosphorus doping concentration of the first preset number of silicon wafers based on the ECV curve of the first preset number of silicon wafers.
[0115] The third judgment unit is used to determine whether there is an abnormality in the poly-si thickness of the first preset number of silicon wafers based on the ECV curve of the first preset number of silicon wafers.
[0116] In one possible implementation, the silicon wafer is grown with a tunneling oxide layer using a thermal oxidation method; the first determination unit may include:
[0117] The first single-wafer analysis subunit is used to determine the second and third inflection points in the ECV curve of each silicon wafer and the slope of the straight line between the second and third inflection points; determine the tunneling parameters of the silicon wafer based on the slope corresponding to the silicon wafer and the standard slope, and determine whether the tunneling parameters of the silicon wafer are greater than a first preset value.
[0118] The first abnormal output subunit is used to determine that the tunneling oxide layer of the first preset number of silicon wafers is abnormal if the tunneling parameters of more than the second preset number of silicon wafers in the first preset number of silicon wafers are all greater than the first preset value.
[0119] In one possible implementation, the first single-wafer analysis subunit may be specifically used to: determine the tunneling parameters of the silicon wafer based on the slope corresponding to the silicon wafer and in conjunction with a first formula;
[0120] The first formula can be:
[0121]
[0122] Where m1 is the tunneling parameter of the silicon wafer, k0 is the standard slope, and k1 is the slope corresponding to the silicon wafer.
[0123] In one possible implementation, the silicon wafer is grown with a tunneling oxide layer using a thermal oxidation method; the second determination unit may include:
[0124] The second single-wafer analysis subunit is used to determine the first inflection point in the ECV curve of each silicon wafer, and use the ordinate of the first inflection point as the phosphorus doping concentration of the silicon wafer; determine the first doping parameter of the silicon wafer based on the phosphorus doping concentration of the silicon wafer and the standard phosphorus doping concentration, and determine whether the first doping parameter of the silicon wafer is greater than a second preset value.
[0125] The second abnormal output subunit is used to determine that the phosphorus doping concentration of the first preset number of silicon wafers is abnormal if the first doping parameter of the first preset number of silicon wafers is greater than the second preset value.
[0126] In one possible implementation, the second single-wafer analysis subunit may be specifically used to: determine the first doping parameter of the silicon wafer based on the phosphorus doping concentration of the silicon wafer and the standard phosphorus doping concentration, combined with a second formula;
[0127] The second formula can be:
[0128]
[0129] Where m2 is the first doping parameter of the silicon wafer, N0 is the standard phosphorus doping concentration, and N1 is the phosphorus doping concentration of the silicon wafer.
[0130] In one possible implementation, the silicon wafer is grown with a tunneling oxide layer using a vapor deposition method; the second determination unit may include:
[0131] The third single-wafer analysis subunit is used to determine the first, second, third, fourth, and fifth inflection points in the ECV curve of each silicon wafer; and based on the first, second, third, fourth, and fifth inflection points, to determine whether the phosphorus doping concentration of the silicon wafer meets the preset conditions.
[0132] The third abnormal output subunit is used to determine that the phosphorus doping concentration of the first preset number of silicon wafers is abnormal if the first doping parameters of the first preset number of silicon wafers do not meet the preset conditions.
[0133] In one possible implementation, the preset conditions can be:
[0134] and
[0135] Where k2 is the slope between the second and third inflection points, k 20 k2 is the standard slope; k3 is the slope between the fourth and fifth inflection points. 30 N is the standard slope corresponding to k3; N2 is the ordinate of the first inflection point, N 20 N is the standard phosphorus doping concentration corresponding to the first inflection point; N3 is the ordinate of the third inflection point, N 30 This represents the standard phosphorus doping concentration corresponding to the third inflection point.
[0136] In one possible implementation, the third determination unit may include:
[0137] The fourth single-wafer analysis subunit is used to determine the first and second inflection points in the ECV curve of each silicon wafer, take the difference between the x-coordinate of the first inflection point and the x-coordinate of the second inflection point as the poly-si test thickness of the silicon wafer, obtain the poly-si target thickness of the silicon wafer according to a preset ratio, and determine the absolute value of the difference between the poly-si target thickness and the preset thickness.
[0138] The fourth abnormal output subunit is used to determine that the poly-Si thickness of the first preset number of silicon wafers is abnormal if the absolute value of the difference corresponding to the first preset number of silicon wafers is greater than the fourth preset number of silicon wafers.
[0139] Figure 7 This is a schematic diagram of a terminal device provided in an embodiment of the present invention. Figure 7As shown, the terminal device 3 in this embodiment includes a processor 30 and a memory 31. The memory 31 is used to store a computer program 32, and the processor 30 is used to call and run the computer program 32 stored in the memory 31 to execute the steps in the various polysilicon doping production line stability embodiments described above, for example... Figure 2 The steps S101 to S103 are shown. Alternatively, the processor 30 is used to call and run the computer program 32 stored in the memory 31 to implement the functions of each module / unit in the above-described device embodiments, for example... Figure 6 The functions of modules 21 to 23 are shown.
[0140] For example, computer program 32 can be divided into one or more modules / units, one or more of which are stored in memory 31 and executed by processor 30 to complete the present invention. One or more modules / units can be a series of computer program instruction segments capable of performing a specific function, which describe the execution process of computer program 32 in terminal device 3. For example, computer program 32 can be divided into... Figure 6 Modules / units 21 to 23 are shown.
[0141] Terminal device 3 can be a computing device such as a desktop computer, laptop, handheld computer, or cloud server. Terminal device 3 may include, but is not limited to, processor 30 and memory 31. Those skilled in the art will understand that... Figure 7 This is merely an example of terminal device 3 and does not constitute a limitation on terminal device 3. It may include more or fewer components than shown, or combine certain components, or different components. For example, the terminal may also include input / output devices, network access devices, buses, etc.
[0142] The processor 30 may be a Central Processing Unit (CPU), or other general-purpose processors, digital signal processors (DSPs), application-specific integrated circuits (ASICs), field-programmable gate arrays (FPGAs), or other programmable logic devices, discrete gate or transistor logic devices, discrete hardware components, etc. A general-purpose processor may be a microprocessor or any conventional processor.
[0143] The memory 31 can be an internal storage unit of the terminal device 3, such as a hard disk or RAM of the terminal device 3. The memory 31 can also be an external storage device of the terminal device 3, such as a plug-in hard disk, Smart Media Card (SMC), Secure Digital (SD) card, or Flash Card equipped on the terminal device 3. Furthermore, the memory 31 can include both internal and external storage units of the terminal device 3. The memory 31 is used to store computer programs and other programs and data required by the terminal. The memory 31 can also be used to temporarily store data that has been output or will be output.
[0144] Those skilled in the art will clearly understand that, for the sake of convenience and brevity, the above-described division of functional units and modules is merely an example. In practical applications, the above functions can be assigned to different functional units and modules as needed, that is, the internal structure of the device can be divided into different functional units or modules to complete all or part of the functions described above. The functional units and modules in the embodiments can be integrated into one processing unit, or each unit can exist physically separately, or two or more units can be integrated into one unit. The integrated unit can be implemented in hardware or as a software functional unit. Furthermore, the specific names of the functional units and modules are only for easy differentiation and are not intended to limit the scope of protection of this application. The specific working process of the units and modules in the above system can be referred to the corresponding process in the foregoing method embodiments, and will not be repeated here.
[0145] In the above embodiments, the descriptions of each embodiment have different focuses. For parts that are not described in detail or recorded in a certain embodiment, please refer to the relevant descriptions of other embodiments.
[0146] Those skilled in the art will recognize that the units and algorithm steps of the various examples described in conjunction with the embodiments disclosed herein can be implemented in electronic hardware, or a combination of computer software and electronic hardware. Whether these functions are implemented in hardware or software depends on the specific application and design constraints of the technical solution. Those skilled in the art can use different methods to implement the described functions for each specific application, but such implementations should not be considered beyond the scope of this invention.
[0147] In the embodiments provided by this invention, it should be understood that the disclosed devices / terminals and methods can be implemented in other ways. For example, the device / terminal embodiments described above are merely illustrative. For instance, the division of modules or units is only a logical functional division, and in actual implementation, there may be other division methods. For example, multiple units or components may be combined or integrated into another system, or some features may be ignored or not executed. Furthermore, the coupling or direct coupling or communication connection shown or discussed may be through some interfaces; the indirect coupling or communication connection between devices or units may be electrical, mechanical, or other forms.
[0148] The units described as separate components may or may not be physically separate. The components shown as units may or may not be physical units; that is, they may be located in one place or distributed across multiple network units. Some or all of the units can be selected to achieve the purpose of this embodiment according to actual needs.
[0149] Furthermore, the functional units in the various embodiments of the present invention can be integrated into one processing unit, or each unit can exist physically separately, or two or more units can be integrated into one unit. The integrated unit can be implemented in hardware or as a software functional unit.
[0150] If an integrated module / unit is implemented as a software functional unit and sold or used as an independent product, it can be stored in a computer-readable storage medium. Based on this understanding, all or part of the processes in the methods of the above embodiments of the present invention can also be implemented by a computer program instructing related hardware. The computer program can be stored in a computer-readable storage medium, and when executed by a processor, it can implement the steps of the various method embodiments described above. The computer program includes computer program code, which can be in the form of source code, object code, executable files, or certain intermediate forms. The computer-readable medium can include: any entity or device capable of carrying computer program code, recording media, USB flash drives, portable hard drives, magnetic disks, optical disks, computer memory, read-only memory (ROM), random access memory (RAM), electrical carrier signals, telecommunication signals, and software distribution media, etc.
[0151] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should all be included within the protection scope of the present invention.
Claims
1. A method for determining the stability of a polycrystalline silicon doped production line, characterized in that, include: Obtain the ECV curves of the first preset number of silicon wafers picked up from the target production line; Based on the ECV curves of the first preset number of silicon wafers, determine whether there are any quality abnormalities in the first preset number of silicon wafers; If an anomaly is found, the target production line is determined to be unstable; The step of determining whether the quality of the first preset number of silicon wafers is abnormal based on the ECV curves of the first preset number of silicon wafers includes: Determine whether there are any abnormalities in the tunneling oxide layer of the first preset number of silicon wafers based on the ECV curves of the first preset number of silicon wafers; and / or Determine whether there is an abnormality in the phosphorus doping concentration of the first preset number of silicon wafers based on the ECV curves of the first preset number of silicon wafers; and / or Determine whether there is an abnormality in the poly-Si thickness of the first preset number of silicon wafers based on the ECV curves of the first preset number of silicon wafers.
2. The method for determining the stability of a polycrystalline silicon doped production line according to claim 1, characterized in that, The silicon wafers are grown with a tunneling oxide layer using a thermal oxidation method; the step of determining whether the tunneling oxide layer of the first preset number of silicon wafers is abnormal based on the ECV curves of the first preset number of silicon wafers includes: For each silicon wafer, determine the second and third inflection points in the ECV curve of the silicon wafer and determine the slope of the straight line between the second and third inflection points; determine the tunneling parameters of the silicon wafer based on the slope corresponding to the silicon wafer and the standard slope, and determine whether the tunneling parameters of the silicon wafer are greater than a first preset value. If the tunneling parameters of more than a second preset number of silicon wafers in the first preset number of silicon wafers are all greater than the first preset value, then it is determined that the tunneling oxide layer of the first preset number of silicon wafers is abnormal.
3. The method for determining the stability of a polycrystalline silicon doped production line according to claim 2, characterized in that, The process of determining the tunneling parameters of the silicon wafer based on the slope corresponding to the silicon wafer and the standard slope includes: Based on the slope corresponding to the silicon wafer, the tunneling parameters of the silicon wafer are determined using the first formula; The first formula is: in, These are the tunneling parameters of the silicon wafer. The standard slope, This represents the slope corresponding to the silicon wafer.
4. The method for determining the stability of a polycrystalline silicon doped production line according to claim 1, characterized in that, The silicon wafers are grown with a tunneling oxide layer using a thermal oxidation method; the step of determining whether there is an abnormality in the phosphorus doping concentration of the first preset number of silicon wafers based on the ECV curves of the first preset number of silicon wafers includes: For each silicon wafer, the first inflection point in the ECV curve of the silicon wafer is determined, and the ordinate of the first inflection point is used as the phosphorus doping concentration of the silicon wafer; the first doping parameter of the silicon wafer is determined based on the phosphorus doping concentration of the silicon wafer and the standard phosphorus doping concentration, and it is determined whether the first doping parameter of the silicon wafer is greater than a second preset value. If the first doping parameter of the first preset number of silicon wafers is greater than the second preset value, then it is determined that the phosphorus doping concentration of the first preset number of silicon wafers is abnormal.
5. The method for determining the stability of a polycrystalline silicon doped production line according to claim 4, characterized in that, The determination of the first doping parameter of the silicon wafer based on the phosphorus doping concentration and the standard phosphorus doping concentration includes: The first doping parameter of the silicon wafer is determined based on the phosphorus doping concentration of the silicon wafer and the standard phosphorus doping concentration, combined with the second formula. The second formula is: in, This is the first doping parameter of the silicon wafer. The standard phosphorus doping concentration is... This represents the phosphorus doping concentration of the silicon wafer.
6. The method for determining the stability of a polycrystalline silicon doped production line according to claim 1, characterized in that, The silicon wafers are grown with a tunneling oxide layer using a vapor deposition method; the step of determining whether there is an abnormality in the phosphorus doping concentration of the first preset number of silicon wafers based on the ECV curves of the first preset number of silicon wafers includes: For each silicon wafer, determine the first, second, third, fourth, and fifth inflection points in its ECV curve; based on the first, second, third, fourth, and fifth inflection points, determine whether the phosphorus doping concentration of the silicon wafer meets the preset conditions. If none of the first doping parameters of the first preset number of silicon wafers meet the preset conditions, then it is determined that the phosphorus doping concentration of the first preset number of silicon wafers is abnormal.
7. The method for determining the stability of a polycrystalline silicon doped production line according to claim 6, characterized in that, The preset conditions are: , , and ; in, The slope between the second inflection point and the third inflection point. for The corresponding standard slope; The slope between the fourth inflection point and the fifth inflection point. for The corresponding standard slope; Let be the ordinate of the first inflection point. The standard phosphorus doping concentration corresponding to the first inflection point; The ordinate of the third inflection point is... This represents the standard phosphorus doping concentration corresponding to the third inflection point.
8. The method for determining the stability of a polycrystalline silicon doped production line according to claim 1, characterized in that, The step of determining whether there is an abnormality in the poly-Si thickness of the first preset number of silicon wafers based on the ECV curve of the first preset number of silicon wafers includes: For each silicon wafer, the first and second inflection points in the ECV curve of the silicon wafer are determined. The difference between the x-coordinate of the first inflection point and the x-coordinate of the second inflection point is taken as the poly-si test thickness of the silicon wafer. The poly-si test thickness is multiplied by a preset ratio to obtain the poly-si target thickness of the silicon wafer. The absolute value of the difference between the poly-si target thickness and the preset thickness is determined. If the absolute value of the difference between the first preset number of silicon wafers and the fourth preset number of silicon wafers is greater than the preset difference, then it is determined that the poly-Si thickness of the first preset number of silicon wafers is abnormal.
9. A terminal device, characterized in that, It includes a processor and a memory, the memory being used to store a computer program, and the processor being used to call and run the computer program stored in the memory to perform the method for determining the stability of a polysilicon doped production line as described in any one of claims 1 to 8.
Citation Information
Patent Citations
Solar cell and photovoltaic module
CN114695578A
Evaluation method for silicon particle production line