Aluminum alloy powder for additive manufacturing and preparation method and application thereof

By adding Ti-22Al-25Nb powder to aluminum alloy powder and utilizing its chemical reaction in a high-temperature molten pool, the problem of hot cracking in aluminum alloys during additive manufacturing was solved, achieving the preparation of crack-free high-strength aluminum alloys and reducing energy consumption.

CN116159992BActive Publication Date: 2024-11-15SOUTHERN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211595428.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-13
Publication Date
2024-11-15
Estimated Expiration
2042-12-13

AI Technical Summary

Technical Problem

2xxx and 7xxx series aluminum alloys are prone to hot cracking during additive manufacturing, which affects the material's formability and mechanical properties.

Method used

Aluminum alloy powder is mixed with Ti-22Al-25Nb powder, and a heterogeneous nucleating agent Al3(Ti,Nb) is generated by chemical reaction in a high-temperature molten pool. This process restricts grain growth, inhibits crack formation, and reduces laser reflectivity to improve absorption efficiency.

Benefits of technology

The fabrication of crack-free high-strength aluminum alloys has been achieved, improving mechanical properties and laser input efficiency while reducing energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116159992B_ABST
    Figure CN116159992B_ABST
Patent Text Reader

Abstract

In order to overcome the problem that high-strength aluminum alloys such as existing 2xxx series aluminum alloys and 7xxx series aluminum alloys are prone to thermal cracking during additive manufacturing, the present invention provides an aluminum alloy powder for additive manufacturing, comprising the following weight components: 90 to 99 parts of aluminum alloy powder, 1 to 10 parts of Ti‑22Al‑25Nb powder; wherein the aluminum alloy powder includes one or more of 2xxx series aluminum alloys and 7xxx series aluminum alloys. At the same time, the present invention also discloses a preparation method and application of the above-mentioned aluminum alloy powder for additive manufacturing. The aluminum alloy powder for additive manufacturing provided by the present invention can achieve grain refinement, inhibit cracking of aluminum alloys, and improve mechanical properties during additive manufacturing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of additive manufacturing materials, and specifically relates to an aluminum alloy powder for additive manufacturing and a preparation method and application thereof. Background Art

[0002] Additive manufacturing (also known as 3D printing or additive manufacturing) is a technology that uses digital model files as the basis and uses powdered metal and other bondable materials to construct objects by printing layer by layer.

[0003] 2xxx series aluminum alloys and 7xxx series aluminum alloys can be used as light and high-strength structural materials due to their high specific strength, low density, high hardness, and good machinability. They are often used to manufacture various light and high-load parts and structural parts, and are widely used in civil and military fields such as automobiles, ships, and aerospace. However, due to the wide solidification temperature range, high-strength aluminum alloys are very likely to produce thermal crack defects due to large thermal stress during the additive manufacturing (3D printing) process based on high-energy beams, thereby sharply reducing the formability and mechanical properties of the material. Summary of the invention

[0004] In view of the problem that high-strength aluminum alloys such as existing 2xxx series aluminum alloys and 7xxx series aluminum alloys are prone to thermal cracks during additive manufacturing, the present invention provides an aluminum alloy powder for additive manufacturing and a preparation method and application thereof.

[0005] The technical solution adopted by the present invention to solve the above technical problems is as follows:

[0006] In one aspect, the present invention provides an aluminum alloy powder for additive manufacturing, comprising the following weight components:

[0007] 90-99 parts of aluminum alloy powder, 1-10 parts of Ti-22Al-25Nb powder;

[0008] Wherein, the aluminum alloy powder includes one or more of 2xxx series aluminum alloy and 7xxx series aluminum alloy.

[0009] Optionally, the aluminum alloy powder for additive manufacturing includes the following weight components:

[0010] 95-99 parts of aluminum alloy powder and 1-5 parts of Ti-22Al-25Nb powder.

[0011] Optionally, the particle size of the aluminum alloy powder is 1 to 100 microns, and the particle size of the Ti-22Al-25Nb powder is 1 to 100 microns.

[0012] Optionally, the aluminum alloy powder includes one or more of 2024 aluminum alloy powder, 2219 aluminum alloy powder, 7070 aluminum alloy powder and 7075 aluminum alloy powder.

[0013] Optionally, the Ti-22Al-25Nb powder comprises the following components by weight:

[0014] Ti: 51.6~52.6%

[0015] Al: 21.9~22.7%

[0016] Nb: 25.4~25.7%

[0017] N:≤0.00032%

[0018] O:≤0.020%

[0019] H:≤0.0017%.

[0020] On the other hand, the present invention provides a method for preparing the aluminum alloy powder for additive manufacturing as described above, comprising the following steps:

[0021] The aluminum alloy powder and the Ti-22Al-25Nb powder are fully mixed to obtain an aluminum alloy powder for additive manufacturing.

[0022] Optionally, a drying operation is performed before and / or after the powders are mixed.

[0023] On the other hand, the present invention provides use of the aluminum alloy powder for additive manufacturing as described above in additive manufacturing of aluminum alloys.

[0024] Optionally, the additive manufacturing method is laser additive manufacturing.

[0025] Optionally, the laser power is 200-400W and the scanning rate is 400-2000mm / s.

[0026] According to the aluminum alloy powder for additive manufacturing provided by the present invention, Ti-22Al-25Nb powder is mixed in high-strength aluminum alloy powders such as 2xxx aluminum alloy powders and / or 7xxx aluminum alloys. When additive manufacturing is performed, the Ti-22Al-25Nb alloy can be introduced into the high-strength aluminum alloy in the selective melting additive manufacturing forming process, and chemical reactions occur in the high-temperature molten pool, playing its role of "in-situ compounding" and "in-situ alloying", which can not only produce a highly efficient heterogeneous nucleating agent Al3 (Ti, Nb) that is conducive to nucleation, but also Ti and Nb elements can effectively limit the growth of grains during grain growth, thereby achieving grain refinement, inhibiting crack generation, and improving the effect of mechanical properties. At the same time, after being mixed with Ti-22Al-25Nb powder, the reflectivity of the aluminum alloy powder for additive manufacturing to the laser is reduced to a certain extent, which is conducive to improving the absorption efficiency of the laser and improving the laser input efficiency to reduce energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a microscopic morphology of the 7075 high-strength aluminum alloy prepared in Example 1 of the present invention;

[0028] Figure 2 This is a microscopic morphology of the 7075 high-strength aluminum alloy prepared in Comparative Example 1 of the present invention;

[0029] Figure 3 This is a microscopic morphology of the 2024 high-strength aluminum alloy prepared in Example 2 of the present invention;

[0030] Figure 4 This is a microscopic morphology of the 2024 high-strength aluminum alloy prepared in Comparative Example 2 of the present invention;

[0031] Figure 5 This is a microscopic morphology of the 7075 high-strength aluminum alloy prepared in Example 3 of the present invention;

[0032] Figure 6 This is a microscopic morphology of the 7075 high-strength aluminum alloy prepared in Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0033] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0034] In the description of the present invention, "additive manufacturing" means "a process of connecting materials layer by layer to make an object according to 3D model data". The aluminum alloy described herein can be manufactured by any appropriate additive manufacturing technology such as binder jetting, directed energy deposition, material extrusion, material jetting, powder bed melting or lamination. In one embodiment, the additive manufacturing process includes depositing successive layers of one or more powders, and then selectively melting and / or sintering the powders to form an aluminum alloy product layer by layer. In one embodiment, the additive manufacturing process uses one or more of selective laser sintering (SLS), selective laser melting (SLM), and electron beam melting (EBM).

[0035] An embodiment of the present invention provides an aluminum alloy powder for additive manufacturing, comprising the following weight components:

[0036] 90-99 parts of aluminum alloy powder, 1-10 parts of Ti-22Al-25Nb powder;

[0037] Wherein, the aluminum alloy powder includes one or more of 2xxx series aluminum alloy and 7xxx series aluminum alloy.

[0038] The aluminum alloy powder for additive manufacturing is mixed with Ti-22Al-25Nb powder in high-strength aluminum alloy powders such as 2xxx aluminum alloy powders and / or 7xxx aluminum alloys. When additive manufacturing is performed, the Ti-22Al-25Nb alloy can be introduced into the high-strength aluminum alloy during the selective melting additive manufacturing forming process, and chemical reactions occur in the high-temperature molten pool, playing its role of "in-situ compounding" and "in-situ alloying", which can not only produce an efficient heterogeneous nucleating agent Al3 (Ti, Nb) that is conducive to nucleation, but also Ti and Nb elements can effectively limit the growth of grains during grain growth, thereby achieving grain refinement, inhibiting crack generation, and improving mechanical properties. At the same time, after being mixed with Ti-22Al-25Nb powder, the reflectivity of the aluminum alloy powder for additive manufacturing to the laser is reduced to a certain extent, which is conducive to improving the absorption efficiency of the laser and improving the laser input efficiency to reduce energy consumption.

[0039] In a preferred embodiment, the aluminum alloy powder for additive manufacturing comprises the following weight components:

[0040] 94-98 parts of aluminum alloy powder and 2-6 parts of Ti-22Al-25Nb powder.

[0041] When the weight proportions of the aluminum alloy powder and the Ti-22Al-25Nb powder are within the above range, it is beneficial to improve the nucleation rate during the grain nucleation process, and can also limit the grain growth during the grain growth process, and can significantly refine the grains.

[0042] In some embodiments, the particle size of the aluminum alloy powder is 1 to 100 microns, and the particle size of the Ti-22Al-25Nb powder is 1 to 100 microns.

[0043] Selecting micron-level aluminum alloy powder is beneficial to controlling the thickness and uniformity of the powder layer in additive manufacturing, while using micron-level Ti-22Al-25Nb powder is beneficial to fully mixing with the aluminum alloy powder. If the particle size of the aluminum alloy powder or the Ti-22Al-25Nb powder is too large, it is easy to cause material differences between different molten pools during the melting process, and the composition of some molten pools is also very close to the original aluminum alloy, which leads to thermal cracking.

[0044] The aluminum alloy powder and the Ti-22Al-25Nb powder can be prepared by gas atomization.

[0045] In some embodiments, the aluminum alloy powder includes one or more of 2024 aluminum alloy powder, 2219 aluminum alloy powder, 7070 aluminum alloy powder, and 7075 aluminum alloy powder.

[0046] It should be noted that the Ti-22Al-25Nb powder is a general term for a type of Ti-Al-Nb alloy, and the volume content of its components will fluctuate within the range of Ti-(18-30)Al-(12.5~30)Nb.

[0047] As an example, in some embodiments, the Ti-22Al-25Nb powder includes the following weight components:

[0048] Ti: 51.6~52.6%

[0049] Al: 21.9~22.7%

[0050] Nb: 25.4~25.7%

[0051] N:≤0.00032%

[0052] O:≤0.020%

[0053] H:≤0.0017%.

[0054] Another embodiment of the present invention provides a method for preparing the aluminum alloy powder for additive manufacturing as described above, comprising the following steps:

[0055] The aluminum alloy powder and the Ti-22Al-25Nb powder are fully mixed to obtain an aluminum alloy powder for additive manufacturing.

[0056] In some embodiments, a drying operation is performed before and / or after the powders are mixed.

[0057] For example, before mixing the powders, the aluminum alloy powder and the Ti-22Al-25Nb powder are dried separately, and then the aluminum alloy powder and the Ti-22Al-25Nb powder are mixed to obtain the aluminum alloy powder for additive manufacturing. Or, the aluminum alloy powder and the Ti-22Al-25Nb powder are mixed to obtain the aluminum alloy powder for additive manufacturing, and then the powder is dried.

[0058] In some embodiments, the drying operation adopts vacuum drying, which can effectively remove moisture in the powder gaps and prevent the aluminum alloy powder or Ti-22Al-25Nb powder from being oxidized during the drying process.

[0059] In one embodiment, the vacuum drying temperature is 70° C. and the drying time is 12 hours.

[0060] Another embodiment of the present invention provides the use of the aluminum alloy powder for additive manufacturing as described above in additive manufacturing of aluminum alloys.

[0061] The application of the aluminum alloy powder for additive manufacturing in additive manufacturing has the advantages of simple preparation process, wide source of raw materials, low cost, and stable properties of the prepared crack-free high-strength aluminum alloy. In addition, the aluminum alloy powder for additive manufacturing is easy to store and transport, and easy to achieve large-scale industrial production.

[0062] In some embodiments, the additive manufacturing method is laser additive manufacturing.

[0063] Specifically, the dried powder is placed in a laser melting molding device, and the powder is spread layer by layer in the laser melting molding device. At the same time, the laser is started to scan, melt, and solidify to obtain an additively manufactured aluminum alloy.

[0064] In some embodiments, the laser power is 200-400 W and the scanning rate is 400-2000 mm / s.

[0065] In some embodiments, the laser power is 240-320 W, and the scanning rate is 1000-2000 mm / s. The present invention is further described below by way of examples.

[0066] Example 1

[0067] This embodiment is used to illustrate the additive manufacturing aluminum alloy and the preparation method thereof disclosed in the present invention, and includes the following steps:

[0068] (1) 7075 aluminum alloy powder and 5% Ti-22Al-25Nb alloy powder by mass were rapidly turned over, inverted, and shaken in a three-dimensional swinging powder mixer for 2 hours to mix them evenly.

[0069] (2) drying the mixed powder obtained in step (1) in a vacuum dryer at 70° C. for 12 hours;

[0070] (3) The dried powder was placed in a selective laser melting device and formed at a laser power of 260 W, a scanning rate of 1200 mm / s, and a scanning interval of 100 μm to obtain a crack-free 7075 high-strength aluminum alloy.

[0071] Example 2

[0072] This embodiment is used to illustrate the additive manufacturing aluminum alloy and the preparation method thereof disclosed in the present invention, and includes the following steps:

[0073] (1) 2024 aluminum alloy powder and 2% Ti-22Al-25Nb alloy powder by mass were rapidly flipped, inverted, and shaken in a three-dimensional swinging powder mixer for 2 hours to mix them evenly.

[0074] (2) drying the mixed powder obtained in step (1) in a vacuum dryer at 70° C. for 12 hours;

[0075] (3) The dried powder was placed in a selective laser melting device and formed at a laser power of 300 W, a scanning rate of 1600 mm / s, and a scanning interval of 100 μm to obtain a crack-free 2024 high-strength aluminum alloy.

[0076] Example 3

[0077] This comparative example is used to illustrate the additive manufacturing aluminum alloy and the preparation method thereof disclosed in the present invention, and includes the following steps:

[0078] (1) 7075 aluminum alloy powder and 10% Ti-22Al-25Nb alloy powder by mass were rapidly turned over, inverted, and shaken in a three-dimensional swinging powder mixer for 2 hours to mix them evenly.

[0079] (2) drying the mixed powder obtained in step (1) in a vacuum dryer at 70° C. for 12 hours;

[0080] (3) The dried powder was placed in a selective laser melting device and formed at a laser power of 260 W, a scanning rate of 1200 mm / s, and a scanning interval of 100 μm to obtain a crack-free 7075 high-strength aluminum alloy.

[0081] Comparative Example 1

[0082] This comparative example is used to compare and illustrate the additive manufacturing aluminum alloy and the preparation method thereof disclosed in the present invention, and includes the following steps:

[0083] (1) Dry the 7075 aluminum alloy powder in a vacuum dryer at 70° C. for 12 hours;

[0084] (2) The dried powder was placed in a selective laser melting device and formed at a laser power of 260 W, a scanning rate of 1200 mm / s, and a scanning interval of 100 μm to obtain a 7075 aluminum alloy.

[0085] Comparative Example 2

[0086] This comparative example is used to compare and illustrate the additive manufacturing aluminum alloy and the preparation method thereof disclosed in the present invention, and includes the following steps:

[0087] (1) Drying the 2024 aluminum alloy powder in a vacuum dryer at 70° C. for 12 hours;

[0088] (2) The dried powder was placed in a selective laser melting device and formed at a laser power of 300 W, a scanning rate of 1600 mm / s, and a scanning interval of 100 μm to obtain a 2024 aluminum alloy.

[0089] Comparative Example 3:

[0090] This comparative example is used to compare and illustrate the additive manufacturing aluminum alloy and the preparation method thereof disclosed in the present invention, and includes the following steps:

[0091] (1) 7075 aluminum alloy powder and Ti-22Al-25Nb alloy powder with a mass ratio of 15% were rapidly turned over, inverted, and shaken in a three-dimensional swinging powder mixer for 2 hours to mix them evenly.

[0092] (2) drying the mixed powder obtained in step (1) in a vacuum dryer at 70° C. for 12 hours;

[0093] (3) The dried powder was placed in a selective laser melting device and formed at a laser power of 260 W, a scanning rate of 1200 mm / s, and a scanning interval of 100 μm to obtain a crack-free 7075 high-strength aluminum alloy.

[0094] Performance Testing

[0095] The powder and aluminum alloy prepared above were subjected to the following performance tests:

[0096] 1. The mixed powder provided in the embodiment and the powder provided in the comparative example were respectively tested by a spectrometer to test the reflectivity of the powder to a laser with a wavelength of 1070 nm.

[0097] Table 1

[0098] sample Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Reflectivity 37.2% 37.6% 34.8% 42.5% 39.3% 32.6%

[0099] It can be seen from the test results in Table 1 that the aluminum alloy powder for additive manufacturing provided by the present invention has a lower reflectivity for laser, indicating that compared with the existing aluminum alloy powder, the aluminum alloy powder for additive manufacturing doped with Ti-22Al-25Nb alloy powder provided by the present invention has a higher absorptivity for laser, which is beneficial to reduce laser power and energy consumption.

[0100] 2. Microscopic observations were performed on the additively manufactured aluminum alloys provided in the examples and the additively manufactured aluminum alloys provided in the comparative examples, and the obtained microscopic photographs are as follows: Figures 1 to 6 shown.

[0101] Figure 1 This is a morphology diagram of the crack-free 7075 high-strength aluminum alloy prepared in Example 1. As can be seen from the diagram, the crack-free high-strength aluminum alloy has no thermal cracks, only a few small pores, and a density of 99.9%.

[0102] Figure 2 This is a morphology diagram of the 7075 high-strength aluminum alloy prepared in Comparative Example 1. As can be seen from the figure, the 7075 aluminum alloy without adding Ti-22Al-25Nb has obvious thermal cracks and a density of 98.8%.

[0103] Figure 3 This is a morphology diagram of the crack-free 2024 high-strength aluminum alloy prepared in Example 2. As can be seen from the figure, the crack-free high-strength aluminum alloy has no thermal cracks, only some pores, and a density of 99.7%.

[0104] Figure 4 This is a morphology diagram of the 2024 high-strength aluminum alloy prepared in Comparative Example 2. As can be seen from the figure, the 2024 aluminum alloy without adding Ti-22Al-25Nb has obvious thermal cracks and a density of 98.3%.

[0105] Figure 5 This is a morphology diagram of the crack-free 7075 high-strength aluminum alloy prepared in Example 3. As can be seen from the diagram, the crack-free high-strength aluminum alloy has no thermal cracks, only some small pores, and a density of 99.4%.

[0106] Figure 6 This is a morphology diagram of the crack-free 7075 high-strength aluminum alloy prepared in Comparative Example 3. As can be seen from the diagram, the crack-free high-strength aluminum alloy has no thermal cracks, but has some obvious pores, and the density is 98.8%.

[0107] 3. According to GB / T228-2010 standard, mechanical property tests were performed on the additively manufactured aluminum alloy provided in the embodiment and the additively manufactured aluminum alloy provided in the comparative example, and the obtained test results were filled in Table 2.

[0108] Table 2

[0109]

[0110] It can be seen from the test results in Table 2 that compared with the aluminum alloy prepared from the aluminum alloy powder without adding Ti-22Al-25Nb alloy powder, the aluminum alloy prepared from the aluminum alloy powder for additive manufacturing provided by the present invention has higher microhardness.

[0111] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An aluminum alloy powder for additive manufacturing, characterized in that: It consists of the following components by weight: 90-99 parts of aluminum alloy powder, 1-10 parts of Ti-22Al-25Nb powder; Wherein, the aluminum alloy powder includes one or more of 2xxx series aluminum alloy and 7xxx series aluminum alloy; The Ti-22Al-25Nb powder comprises the following components by weight: Ti: 51.6~52.6% Al: 21.9~22.7% Nb: 25.4~25.7% N: ≤0.00032% O: ≤0.020% H: ≤0.0017%。 2. The aluminum alloy powder for additive manufacturing according to claim 1, characterized in that: It consists of the following components by weight: 95~99 parts of aluminum alloy powder and 1~5 parts of Ti-22Al-25Nb powder.

3. The aluminum alloy powder for additive manufacturing according to claim 1, characterized in that: The particle size of the aluminum alloy powder is 1 to 100 microns, and the particle size of the Ti-22Al-25Nb powder is 1 to 100 microns.

4. The aluminum alloy powder for additive manufacturing according to claim 1, characterized in that: The aluminum alloy powder includes one or more of 2024 aluminum alloy powder, 2219 aluminum alloy powder, 7070 aluminum alloy powder and 7075 aluminum alloy powder.

5. The method for preparing aluminum alloy powder for additive manufacturing according to any one of claims 1 to 4, characterized in that: The steps include: The aluminum alloy powder and the Ti-22Al-25Nb powder are fully mixed to obtain an aluminum alloy powder for additive manufacturing.

6. The preparation method according to claim 5, characterized in that: Before and / or after the powders are mixed, a drying operation is performed.

7. Use of the aluminum alloy powder for additive manufacturing according to any one of claims 1 to 4 in additive manufacturing of aluminum alloys.

8. The use according to claim 7, characterized in that: The additive manufacturing method is laser additive manufacturing.

9. The use according to claim 8, characterized in that: The laser power is 200-400W and the scanning rate is 400-2000mm / s.