A method for manufacturing composite material steel ingot

The composite steel ingots are manufactured through vacuum induction furnace smelting and natural cooling solidification, which solves the problems of high manufacturing cost and low repair efficiency of steel for rolls, and realizes efficient and low-cost metallurgical fusion of composite layers, avoiding the defects of internal shrinkage holes. .

CN116174662BActive Publication Date: 2024-11-05HUBEI SHANGDA MODEL MATERIAL TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202111422797.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-26
Publication Date
2024-11-05
Estimated Expiration
2041-11-26

AI Technical Summary

Technical Problem

In the prior art, the manufacturing process of steel for rolling rolls leads to high manufacturing costs and low repair efficiency, and internal shrinkage problems are prone to occur during traditional electric furnace smelting and electroslag remelting.

Method used

The composite steel ingots are made of smelted by vacuum induction furnace. By naturally cooling and solidifying in the ingot mold, a composite steel ingot with high alloy outer layer and low alloy inner layer is formed, achieving overall composite solidification, overcoming the low efficiency of surfacing and restoration and electroslag weight The high cost of melting and the problem of shrinkage.

Benefits of technology

The manufacturing efficiency of steel for rolling rolls is improved, the manufacturing cost is reduced, and the complete combination of the composite layer and the substrate is achieved through metallurgical fusion, avoiding the defects of internal shrinkage holes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116174662B_ABST
    Figure CN116174662B_ABST
Patent Text Reader

Abstract

The invention discloses a method for manufacturing a composite material steel ingot, which comprises the steps of pouring low alloy steel liquid into a round cross-section steel ingot, grinding the surface of the steel ingot until the metal color is visible, preparing a larger round cross-section steel ingot mold, heating and insulating the processed steel ingot for standby use, injecting the smelted high alloy steel liquid into the larger steel ingot mold, aligning the center of the heated steel ingot with the steel ingot mold containing the high alloy steel liquid, inserting the heated steel ingot into the steel ingot mold containing the high alloy steel liquid until the bottom of the steel ingot mold, and the high temperature steel liquid will cover the surface of the low alloy steel ingot and melt its surface layer, and then solidify as a whole, demold after solidification, and obtain a steel ingot with a composite layer of metal. The invention overcomes the disadvantages of low efficiency and high cost of existing surfacing repair and the disadvantage of internal shrinkage cavities of the electroslag ingot in the production of multi-layer metals by electroslag remelting, and improves the production efficiency of metal composites, is easy to operate, and has adjustable thickness of the composite layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to metal smelting in the metallurgical industry, and in particular to a method for manufacturing a composite material steel ingot. Background Art

[0002] Steel is the most widely used metal. Steels that require high wear resistance, such as roll steel, have a high alloying element content. Alloying elements such as Cr, Mo, and V are added to form high-hardness carbides with C to improve the wear resistance of steel. Since the surface of the roll is worn during use, the thickness of the working layer is usually 20 to 30 mm. After the working layer is worn out, the roll is scrapped. Typical roll steel grades are 9Cr3MoV, 9Cr5MoV, and Cr12MoV. These roll steels are used for rolling cold-rolled steel plates. The working surface of the roll is hardened by induction heating quenching, and the inside is a low-hardness area. The traditional manufacturing process of steel for rolls is to cast the steel into an ingot as a whole after smelting in an electric furnace, and then use the cast ingot for electroslag remelting. The obtained electroslag ingot is a steel ingot of a single material. The rolls made of such ingots are made of a single material as a whole, and are composed of the same chemical composition from the surface to the core. For the parts other than the working layer of the roll, high hardness is not required. Such chemical composition causes excess quality, resulting in an increase in the manufacturing cost of the roll. Repairing scrapped rolls can reduce the waste caused by scrapping of rolls. The repair method uses surfacing to weld the same material or a surfacing layer with higher wear resistance layer by layer on the working surface of the scrapped roll. The roll repaired by surfacing with a material with higher wear resistance is a composite material roll. The use of surfacing to repair rolls has the disadvantages of low efficiency and high cost.

[0003] Composite steel is usually produced by composite rolling, welding two steel plates with different chemical compositions, heating them in a vacuum environment, and then rolling them to deform them. The two steel plates are deformed at high temperature, and metallurgical bonding of the interface is achieved under high temperature and pressure to form an integrated composite steel plate. Searching for patents in the field of composite electroslag, the existing patent publication number is CN1721117A, which uses a horizontal surfacing method to repair scrap crankshafts and rollers; the invention patent publication number is CN1736634A, which uses segmented electrodes of different compositions to be welded together, and then electroslag remelting is performed. The electroslag remelting process requires power outage, and then power is turned on to lower the current and then electroslag remelting is performed. Such an operation has the disadvantage of easily causing shrinkage cavities inside the electroslag ingot. Summary of the invention

[0004] The object of the present invention is to provide a method for manufacturing a composite material steel ingot to solve the above technical problems.

[0005] To achieve the above purpose, the present invention adopts the following technical solutions:

[0006] A method for manufacturing a composite material steel ingot comprises the following steps:

[0007] Step 1, using a vacuum induction furnace to melt molten steel with a weight ratio of 0.4% C, 0.2% Si, 0.3% Mn, 1.2% Cr, 0.3% Mo, and the balance Fe, and casting it into a round cross-section steel ingot;

[0008] Step 2: After cooling in the casting mold for 15 hours, demould the mold, and then grind the round-section steel ingot on a grinder to reveal the original color of the metal;

[0009] Step 3: After the metal color is seen, put it into the heating furnace and heat it to 1200-1300℃ and keep it warm for 0.5-1 hour for standby use;

[0010] Step 4, pre-smelting molten steel with a chemical composition weight ratio of 0.9% C, 0.8% Si, 0.3% Mn, 5% Cr, 0.3% Mo, 0.2% V and a remainder of Fe in a 1-ton vacuum induction furnace, the molten steel temperature is 1550-1580° C., preparing an ingot mold for pouring, and filling the ingot mold with Ar gas;

[0011] Step 5, then inject the molten steel melted in step 4 into an ingot mold filled with Ar gas, and the amount of molten steel injected is 600-1000 kg;

[0012] Step 6, immediately lift the heated ingot to the top of the ingot mold, align it with the ingot mold, and then vertically lower the ingot into the ingot mold until the bottom of the ingot mold remains vertically upright. At this time, the liquid level of the molten steel in the ingot mold rises to a height of 1400 mm;

[0013] Step 7, covering the steel liquid surface with 100 mm thick carbonized rice husk, keeping the steel ingot mold still, allowing the liquid steel to naturally cool and solidify in the steel ingot mold, and demolding after 18-20 hours to obtain a composite steel ingot with a high alloy outer layer and a low alloy inner layer;

[0014] Step 8: Slice the steel ingot transversely, polish and observe the interface of the composite layer. The interface of the composite layer is completely fused without stratification, and metallurgical fusion of the composite layer and the matrix is ​​achieved.

[0015] As a further solution of the present invention, step 1 adopts a 1-ton vacuum induction furnace for smelting and casting into a circular cross-section steel ingot of Φ300×1500mm.

[0016] As a further solution of the present invention, step 2 is to grind the circular cross-section steel ingot of Φ300×1500mm on a grinder to a size of Φ290×1500mm.

[0017] As a further solution of the present invention, step 4 prepares a steel ingot mold with an inner wall specification of Φ420×1500mm for pouring.

[0018] As a further solution of the present invention, in step 6, the heated Φ290×1500mm steel ingot is immediately hoisted above the Φ400×1500mm steel ingot mold, and after being centered with the ingot mold, the Φ290×1500mm steel ingot is vertically lowered and inserted into the ingot mold until the bottom of the ingot mold remains in a vertical upright state.

[0019] Compared with the prior art, the present invention has the following advantages: the present invention adopts an overall composite solidification method to overcome the shortcomings of low efficiency and high cost of existing surfacing welding to repair composite material rollers and the shortcomings of the existence of shrinkage cavities inside the electroslag ingots in the production of multi-layer metals by electroslag remelting. The overall composite solidification improves the efficiency and is easy to operate, and the thickness of the composite layer can be adjusted. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic diagram of the composite solidified steel ingot of the present invention.

[0021] In the figure: 1. Steel ingot, 2. High alloy, 3. Steel ingot mold. DETAILED DESCRIPTION

[0022] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0023] Example 1

[0024] A 1-ton vacuum induction furnace is used to melt molten steel with a chemical composition of 0.4% C, 0.2% Si, 0.3% Mn, 1.2% Cr, 0.3% Mo and a remainder of Fe, and the steel is cast into a circular cross-section steel ingot 1 of Φ300×1500mm. The steel ingot is demolded after cooling in the mold for 15 hours, and then the circular cross-section steel ingot of Φ300×1500mm is ground on a grinder to a size of Φ290×1500mm, and the original color of the metal is seen. The steel ingot is then placed in a heating furnace and heated to 1200°C and kept warm for 0.5 hours. A 1-ton vacuum induction furnace is used in advance to melt molten steel with a chemical composition of 0.9% C, 0.8% Si, 0.3% Mn, 5% Cr, 0.3% Mo, 0.2% V and a remainder of Fe. The temperature of the molten steel is 1550°C, and an inner wall specification of Φ420×1500mm is prepared. m steel ingot mold 3 is ready for pouring, and the steel ingot mold is filled with Ar gas, and then the smelted molten steel is injected into the steel ingot mold filled with Ar gas, and the amount of molten steel injected is 600 kg. After that, the heated Φ290×1500mm steel ingot 1 is immediately hoisted to the top of the Φ400×1500mm steel ingot mold 3, and after being aligned with the ingot mold, the Φ290×1500mm steel ingot is vertically lowered and inserted into the steel ingot mold until the bottom of the ingot mold remains vertically upright. At this time, the liquid molten steel in the steel ingot mold rises to a height of 1400mm, and the steel liquid surface is covered with 100mm thick carbonized rice husk, and the steel ingot mold is kept stationary. The liquid molten steel is naturally cooled and solidified in the steel ingot mold, and demolded after 18 hours to obtain a composite material steel ingot with an outer layer of high alloy 2 and an inner layer of low alloy 1. The steel ingot is sliced ​​horizontally, and the interface of the composite layer is observed after polishing. The interface of the composite layer has been completely fused without stratification, and the metallurgical fusion of the composite layer and the matrix is ​​achieved.

[0025] Example 2

[0026] A 1-ton vacuum induction furnace is used to melt molten steel with a chemical composition of 0.4% C, 0.2% Si, 0.3% Mn, 1.2% Cr, 0.3% Mo and a remainder of Fe, and the steel is cast into a circular cross-section steel ingot of Φ300×1500mm. After cooling in the mold for 15 hours, the steel ingot is demolded, and then the circular cross-section steel ingot of Φ300×1500mm is ground on a grinder to a size of Φ290×1500mm, and the metal color is seen. The steel ingot is placed in a heating furnace and heated to 1300°C for 1 hour. A 1-ton vacuum induction furnace is used to melt molten steel with a chemical composition of 0.9% C, 0.8% Si, 0.3% Mn, 5% Cr, 0.3% Mo, 0.2% V and a remainder of Fe in advance. The temperature of the molten steel is 1580°C, and an inner wall specification of Φ450×15 is prepared. 00mm ingot mold is to be poured, and the ingot mold is filled with Ar gas, and then the smelted molten steel is injected into the ingot mold filled with Ar gas, and the amount of molten steel injected is 970 kg. After that, the heated Φ290×1500mm ingot is immediately hoisted to the top of the Φ450×1500mm ingot mold, and after aligning with the ingot mold, the Φ290×1500mm ingot is vertically lowered and inserted into the ingot mold until the bottom of the ingot mold is fixed. At this time, the liquid molten steel in the ingot mold rises to a height of 1400mm, and the 100mm thick carbonized rice husk is covered on the steel liquid surface. The ingot mold is kept stationary, and the liquid molten steel is naturally cooled and solidified in the ingot mold. After 20 hours, the mold is demolded to obtain a composite material steel ingot with a high alloy outer layer and a low alloy inner layer. The ingot is sliced ​​horizontally, and the interface of the composite layer is observed after polishing. The interface of the composite layer has been completely fused without stratification, and the metallurgical fusion of the composite layer and the matrix is ​​achieved.

[0027] Example 3

[0028] A 1-ton vacuum induction furnace is used to melt molten steel with a chemical composition of 0.4% C, 0.2% Si, 0.3% Mn, 1.2% Cr, 0.3% Mo and a remainder of Fe, and the steel is cast into a circular cross-section steel ingot of Φ300×1500mm. The steel is demolded after cooling in the mold for 15 hours, and then the circular cross-section steel ingot of Φ300×1500mm is ground on a grinder to a size of Φ290×1500mm, and the original color of the metal is seen. The steel is then placed in a heating furnace and heated to 1250°C for 0.8 hours. A 1-ton vacuum induction furnace is used in advance to melt molten steel with a chemical composition of 0.9% C, 0.8% Si, 0.3% Mn, 5% Cr, 0.3% Mo, 0.2% V and a remainder of Fe. The temperature of the molten steel is 1560°C, and an inner wall specification of Φ425×1 The 500mm ingot mold is ready for pouring, and the ingot mold is filled with Ar gas, and then the smelted molten steel is injected into the ingot mold filled with Ar gas, and the amount of molten steel injected is 780 kg. After that, the heated Φ290×1500mm ingot is immediately hoisted to the top of the Φ425×1500mm ingot mold, and after aligning with the ingot mold, the Φ290×1500mm ingot is vertically lowered and inserted into the ingot mold until the bottom of the ingot mold is fixed. At this time, the liquid molten steel in the ingot mold rises to a height of 1400mm, and the 100mm thick carbonized rice husk is covered on the steel liquid surface. The ingot mold is kept stationary, and the liquid molten steel is naturally cooled and solidified in the ingot mold. After 20 hours, the mold is demolded to obtain a composite material steel ingot with a high alloy outer layer and a low alloy inner layer. The ingot is sliced ​​horizontally, and the interface of the composite layer is observed after polishing. The interface of the composite layer has been completely fused without stratification, and the metallurgical fusion of the composite layer and the matrix is ​​achieved.

[0029] The above is a preferred embodiment of the present invention. For ordinary technicians in this field, according to the teachings of the present invention, without departing from the principles and spirit of the present invention, changes, modifications, substitutions and variations made to the implementation methods are still within the scope of protection of the present invention.

Claims

1. A method for manufacturing a composite steel ingot, characterized in that: The steps include: Step 1, using a vacuum induction furnace to melt molten steel with a weight ratio of 0.4% C, 0.2% Si, 0.3% Mn, 1.2% Cr, 0.3% Mo, and the balance Fe, and casting it into a round cross-section steel ingot; Step 2: After cooling in the casting mold for 15 hours, demould the mold, and then grind the round-section steel ingot on a grinder to reveal the original color of the metal; Step 3: After the metal color is seen, put it into a heating furnace and heat it to 1200-1300℃ and keep it warm for 0.5-1 hour for standby use; Step 4: Preliminarily melt molten steel with a chemical composition weight ratio of 0.9% C, 0.8% Si, 0.3% Mn, 5% Cr, 0.3% Mo, 0.2% V and a remainder of Fe in a vacuum induction furnace, the temperature of the molten steel being 1550-1580° C., prepare an ingot mold for pouring, and fill the ingot mold with Ar gas; Step 5, then inject the molten steel melted in step 4 into an ingot mold filled with Ar gas, and the amount of molten steel injected is 600-1000 kg; Step 6, immediately lift the heated steel ingot 1 to the top of the steel ingot mold, align it with the ingot mold, and then vertically lower the steel ingot into the steel ingot mold until the bottom of the ingot mold remains vertically upright. At this time, the liquid level of the molten steel in the steel ingot mold rises to a height of 1400 mm; Step 7, covering the steel liquid surface with 100 mm thick carbonized rice husk, keeping the steel ingot mold still, allowing the liquid steel to naturally cool and solidify in the steel ingot mold, and demolding after 18-20 hours to obtain a composite steel ingot with a high alloy outer layer and a low alloy inner layer; Step 8: Slice the steel ingot transversely, polish and observe the interface of the composite layer. The interface of the composite layer is completely fused without stratification, and metallurgical fusion of the composite layer and the matrix is ​​achieved.

2. The method for manufacturing a composite steel ingot according to claim 1, characterized in that: Step 1 uses a 1-ton vacuum induction furnace for smelting and casting into a Φ300×1500mm round-section steel ingot (1).

3. The method for manufacturing a composite steel ingot according to claim 2, characterized in that: Step 2: Grind the Φ300×1500mm circular cross-section steel ingot on a grinder to a size of Φ290×1500mm.

4. The method for manufacturing a composite steel ingot according to claim 3, characterized in that: Step 4: Preliminary melting in a 1-ton vacuum induction furnace is used to prepare a steel ingot mold (3) with an inner wall specification of Φ420×1500mm for pouring.

5. The method for manufacturing a composite steel ingot according to claim 4, characterized in that: Step 6: Immediately lift the heated Φ290×1500mm steel ingot 1 to the top of the Φ400×1500mm steel ingot mold (3), align it with the ingot mold, and then vertically lower the Φ290×1500mm steel ingot into the ingot mold until the bottom of the ingot mold remains in a vertical upright state.

Citation Information

Patent Citations

  • Method for producing surface compound cutter billet by horizontal electro-slag surfacing

    CN1721117A

  • Production method of multiple layer metal surface composite billet using electroslag remelting

    CN1736634A

  • Method for producing large-sized capless steel ingot by using vacuum pouring method

    CN103386470A

  • Roughing roll made of graphitizable steel material and manufacturing method thereof

    CN103469109A

  • Reduction casting compositing method and device for large iron ingots

    CN104475693A