A micro oil-containing bearing material containing fluidized high-efficiency oxidized fibrous copper powder
By using fluidized and efficient oxidized fiber-like copper powder and water-atomized copper powder, tin powder and graphite, combined with low-temperature sintering technology, the problem of synchronous improvement of the strength and oil content of micro-oil bearings is solved, and high strength and high strength are achieved The micro-oil bearings with oil content and low noise meet the performance requirements of new electronic equipment and new energy vehicles.
Patent Information
- Application Number
- CN202211546118.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-12-05
AI Technical Summary
Existing micro-oil-containing bearings are difficult to have excellent performance of high oil content and high strength, and the preparation process is costly and noise-free, which cannot meet the higher requirements of micro-oil-oil-containing bearings by new electronic equipment and new energy vehicles.
Using fluidized and efficient oxidized fibrous copper powder and water-atomized copper powder, tin powder and graphite, through mixing, pressing and low-temperature sintering processes, a micro-oil-containing bearing with high strength and high oil content is formed, and a fiber-like copper base is used. The complex porous structure and high specific surface area of the powder improve the moldability and sintering driving force of the material.
The strength of micro oil-containing bearings has been increased to >200MPa, and the oil content rate is ≥24%, while reducing the preparation cost and noise, meeting the requirements of smart electronic equipment and new energy vehicles for high precision and comfort.
Smart Images

Figure CN116174708B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a micro oil-containing bearing material containing fluidized high-efficiency oxidized fibrous copper powder, belonging to the technical field of bearing design and development. Background Art
[0002] As a basic part of mechanical equipment, micro oil-impregnated bearings are typical metal parts made of copper-based powder as raw materials. They have been widely used in various industries such as new energy vehicles, home appliances, power tools, computer equipment, etc. High-strength, high-oil-content, low-noise micro oil-impregnated bearings are the guarantee for low-noise, high-speed and long-life operation of precision equipment such as the new generation of 5G signal boxes, 3C electronic equipment vibration micromotors and new energy vehicle instruments. Domestic and foreign bearing manufacturers produce copper-based micro oil-impregnated bearings in accordance with international standards. For example, the bronze-based oil-impregnated bearings with a diameter of 1.2-8mm developed by the Japanese company Porite have been used in silent equipment bearings (axial fan motors), household microwave ovens and mobile phone vibration micromotors.
[0003] The chemical composition of domestic and foreign copper-based oil-containing bearings is generally 90-95% Cu, 5-10% Sn and a small amount of C. There are two main types of raw material metal powders: copper and tin mixed powder and bronze powder. The metal powder and other trace component powders are mixed and pressed into shape, and then sintered at 700℃-800℃ in a hydrogen atmosphere. The radial crushing strength is generally 120-170MPa, and the oil content is generally 19-22%.
[0004] In order to improve the strength and oil content of the product, people have made some attempts, such as patent ZL201310533340.6, which selects BRO-AG1L3-YY-150 (copper-tin diffusion powder), DFRCU-CSA-100 (copper-tin pre-alloyed powder), HJT-CE-300 (iron powder), zinc stearate, nickel-coated molybdenum disulfide, and graphite components, supplemented by dispersion strengthening agent SD-8000, zinc powder, tin powder, etc., and distributes insoluble dispersion strengthening phase particles in the metal matrix to strengthen the metal. This preparation method has the disadvantages of high cost, too complex material components, and easy to cause component segregation during mixing, thus affecting the uniformity of the product. Moreover, the sintering temperature of this technology is as high as 855 degrees Celsius; and the oil content of the product is only 22.5%. Patent ZL201010514791.1 uses copper powder bal, aluminum powder 8-12%, tin powder 4-8%, nickel powder 0.6-4%, hard particles 1-5%, and zinc stearate 1-5% to prepare high-performance copper-based powder metallurgy oil-containing self-lubricating bearings through mixing, pressing and sintering. The hard particles introduced into the oil-containing bearings prepared by this method have the hidden danger of damaging the matching materials, and the oil content is only 12-18%, which has not yet exceeded 22%, and does not meet the requirements of new electronic products and new energy vehicle micro-motors for high oil content (>22%) of micro oil-containing bearings. The ultimate bearing pressure of this material is 90-100MPa, and the strength is insufficient. Patent ZL201811505327.9 uses copper atomized alloy powder and alumina dispersion strengthened copper-tin expanded alloy powder according to the mass ratio of 60-90:10-40, adds a small amount of zinc stearate pore-forming agent, and prepares high-strength and high-toughness oil-containing bearings through mixing, pressing and sintering. Since this material introduces large-particle alumina dispersion-strengthened copper-tin alloy powder, the sintering temperature of 900℃ is 150-200℃ higher than the general 700-750℃. The raw material cost and preparation cost are high. The hard alumina particles are easily damaged during long-term use, which reduces the service life and easily produces high noise. Summary of the invention
[0005] In order to achieve simultaneous improvement of the mechanical strength and oil content of a micro oil-containing bearing, the present invention uses fibrous copper powder to prepare a micro oil-containing bearing with excellent performance.
[0006] Research has found that the atomized copper powder and its alloy powder, the raw materials of micro oil-containing bearings, are mostly spherical and quasi-spherical, with high loose density, poor powder formability, and low pressed green strength. It is difficult for micro oil-containing bearings prepared with this raw material to have both high oil content and high strength. The higher requirements for the strength and oil content performance indicators of micro oil-containing bearings for high precision, high intelligence and comfort of intelligent electronic devices are no longer met. Therefore, from the perspective that material structure determines performance, structural design research on raw materials for micro oil-containing bearings is carried out, the matrix structure of micro oil-containing bearings is regulated, the strength and oil content of micro oil-containing bearings are simultaneously improved, and high-efficiency, low-energy consumption, and pollution-free preparation are developed. Based on this, the present invention is proposed.
[0007] The present invention discloses a micro oil-containing bearing material containing fluidized high-efficiency oxidized fibrous copper powder, wherein the raw materials used include, by mass:
[0008] 0-60 parts of water atomized copper powder;
[0009] 20-100 parts of fluidized high-efficiency oxidation-reduction fibrous copper powder; preferably 40-100 parts, more preferably 60-100 parts;
[0010] 8-11 parts of tin powder;
[0011] Graphite 0.5-2.0 parts;
[0012] or
[0013] The raw materials used include: bronze powder and graphite, and the mass ratio of each component is 98-99.5:0.5-2.0;
[0014] The raw materials are mixed and then pressed and sintered to obtain an oil-containing bearing. During sintering, a hydrogen atmosphere is used and the sintering temperature is controlled to be 720-750°C.
[0015] Preferably, the raw materials used include: water atomized copper powder, fluidized high-efficiency oxidation fibrous copper powder, tin powder, and graphite, and the mass ratio of each component is 40-60:40-60:8-11:0.5-2.0; that is, the mass ratio of atomized copper powder, fluidized high-efficiency oxidation-reduction fibrous copper powder, tin powder, and graphite; atomized copper powder: fluidized high-efficiency oxidation-reduction fibrous copper powder: tin powder: graphite = 40-60:40-60:8-11:0.5-2.0. This scheme is mainly considered from the perspective of cost. Because research has found that when the amount of fluidized high-efficiency oxidation-reduction fibrous copper powder in copper powder is 40% or more of the total copper powder mass, the oil content and strength of the product are relatively excellent.
[0016] Preferably, the raw materials used include: fluidized high-efficiency oxidation-reduction fibrous copper powder, copper powder, tin, and graphite powder, and the fluidized high-efficiency oxidation-reduction fibrous copper powder, copper powder, tin, and graphite powder are configured in a mass ratio of 90:9:1.
[0017] As a further preference, the content of fluidized high-efficiency oxidation-reduction fibrous copper powder in the raw materials used is greater than or equal to 60wt%.
[0018] The bulk density of the fluidized high-efficiency redox fibrous copper powder is less than or equal to 1.7 g / cm 3 , preferably 1.2-1.7g / cm 3 Specific surface area is 0.35-0.50m 2 / g. The fluidized high-efficiency oxidation-reduction fibrous copper powder is pure copper powder, and its purity is greater than or equal to 99.9%. The particle size distribution composition of the fluidized high-efficiency oxidation-reduction fibrous copper powder is: copper powder with a particle size of less than 5μm: 3-5v%; copper powder with a particle size of 5 to 20μm: 55-65v%; copper powder with a particle size greater than 20μm and less than or equal to 45μm: 28-35v%.
[0019] Preferably, the fluidized high-efficiency redox fibrous copper powder is prepared by the following method:
[0020] Pure copper is melted to form copper liquid, and then non-spherical copper powder is obtained by water atomization. The atomized copper powder is then subjected to fluidized oxidation on a copper powder fluidized bed device, and the oxygen content of the powder after oxidation is ≥10%, and the oxidation efficiency is 15-20% / min. The oxidized powder is subjected to bidirectional grinding and dispersion to obtain fibrous powder. The oxygen content of the powder is ≤0.1% after hydrogen reduction.
[0021] In industrial application environments, when fluidized oxidation is carried out, natural gas and air inlets are set at the bottom of the fluidized bed, and the volume ratio of natural gas to air is 0.8~1:1.1~3.
[0022] The water-atomized copper powder used in the present invention can be commonly used copper powder on the market, but preferably; the bulk density of the water-atomized copper powder is controlled to be 1.8-2.0 g / cm 3 ; preferably 1.85-1.9g / cm 3 The specific surface area is 0.18-0.25, preferably 0.18-0.2m 2 / g, more preferably 0.2m 2 / g. The particle size of the water atomized copper powder is less than or equal to 350 meshes.
[0023] The particle size of the tin powder is less than or equal to 300 mesh.
[0024] The particle size of graphite is less than or equal to 300 mesh.
[0025] The bronze powder is composed of 89.7wt.% Cu and 9.8wt.% Sn, and 0.5wt.% others. The preparation method is as follows: fluidized high-efficiency oxidation-reduction fibrous copper powder and 10wt% Sn powder are three-dimensionally mixed for 120 minutes, sintered and granulated in a reduction furnace at a granulation temperature of 550-600°C, and the sintered and granulated powder is crushed, sieved, and the particle size distribution is adjusted to obtain the finished powder.
[0026] The bulk density of the fluidized high-efficiency redox fibrous bronze powder is less than 2.9 g / cm 3 , preferably 2.3-2.9g / cm 3 ; More preferably 2.6-2.65g / cm 3 . The specific surface area is 0.04m 2 / g, preferably 0.03-0.06m 2 / g. The fluidized high-efficiency redox fibrous bronze powder has a particle size of less than or equal to 100 meshes.
[0027] The fluidized high-efficiency redox fibrous bronze powder has a particle size distribution composition of: 0-20 μm: <1 v%; 20-45 μm: 8-10 v%; 45-100 μm: 35-45 v%; 100-200 μm: 40-45 v%; 200-400 μm: 9-10 v%.
[0028] The present invention discloses a micro oil-containing bearing material containing fluidized high-efficiency oxidized fibrous copper powder, which is prepared by the following steps:
[0029] Step 1
[0030] Take each raw material according to the group, mix them evenly, and obtain the spare material;
[0031] Step 2
[0032] The spare material is pressed to obtain a green body; during pressing, the pressure of the hydraulic press is controlled to be 15-17MPa and the holding time is 3-5s;
[0033] Step 3
[0034] The green body is placed in a sintering furnace for sintering at a temperature of 720-750°C for 2-3 hours to obtain a sintered part; during sintering, the hydrogen atmosphere is controlled;
[0035] Step 4
[0036] The sintered parts are impregnated with oil and finished to produce miniature oil-containing bearings.
[0037] The present invention discloses a micro oil-containing bearing material containing fluidized high-efficiency oxidized fibrous copper powder; each raw material is taken according to the group, and mixed evenly at a speed of 100-150 revolutions per minute to obtain a standby material. When used in industry, a mixer is generally controlled to mix the materials, and the mixing time is controlled to be 5-7 hours. Kerosene is used as a dispersant during mixing. The amount of kerosene used is 10-11wt.% of the material.
[0038] The green strength of the micro oil-containing bearing containing fluidized fibrous copper-based powder is greater than 12MPa, the crushing strength of the finished product is greater than 200MPa, and the oil content is greater than or equal to 24%.
[0039] Principles and advantages
[0040] The main raw material of the high-strength, high-oil-content micro oil-containing bearing designed and prepared by the present invention is high-strength atomized redox copper powder with a special fibrous morphology. A single particle is composed of multiple bundles of copper fiber clusters and has a complex porous morphology. The bulk density is generally 1.2-1.7g / cm 3 , the specific surface area is generally 0.3-0.5cm 2 / g. Compared with conventional spherical / quasi-spherical atomized redox copper powder, fluidized high-efficiency oxidized fibrous copper-based powder has lower bulk density and larger specific surface area. Compared with electrolytic copper powder, the material itself is not grown by single copper crystal dendrites, and the bonding between grains is stronger. Under the same pressing pressure, it has higher green compact strength. During the pressing process, the loosely stacked fibrous powders are entangled with each other after being subjected to vertical forces. The bent and deformed copper-based fibers connected to each other build a continuous arch bridge structure inside the green compact. On the one hand, this structure solves the problem of insufficient bonding strength between the original conventional spherical / quasi-spherical powders, and on the other hand, it improves the pore structure of the green compact material, so that the green compact has the comprehensive properties of low density, high formability and high pressure green compact strength. During the sintering process, the fibrous powder bridges stably during sintering, eliminating a large number of closed holes and forming more blind holes, which effectively solves the problem that oil-containing bearings are difficult to have high oil content, high strength and low noise. At the same time, the fibrous copper-based powder has a larger specific surface area. The high specific surface area makes the material have a higher material surface energy, improves the solid-liquid and solid-gas sintering driving force, and promotes reactive sintering. Solid-phase sintering and fusion occur at the fiber entanglement inside the compact. The fibrous copper-based powder is fused and combined after sintering to construct a 3D high-strength copper-based network structure, which further improves the mechanical strength and oil content of the micro oil-containing bearing.
[0041] The present invention can obtain high-quality products with a crushing strength greater than 200Mpa and an oil content greater than or equal to 24% by adopting a lower sintering temperature without adding other reinforcement bodies. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is the morphology of the fibrous copper powder used in Example 1;
[0043] Figure 2 This is a morphology picture of the fluidized high-efficiency redox bronze powder used in Example 3;
[0044] Figure 3 This is the metallographic structure diagram of the product obtained in Example 6. DETAILED DESCRIPTION
[0045] Embodiment 1:
[0046] 1. Raw material mixing: spherical / quasi-spherical water-atomized copper powder, fluidized high-efficiency redox fibrous copper powder, tin powder, and graphite are prepared in a mass ratio of 45:45:9:1, first manually mixed for 20 minutes, added to a mixer and mixed for 6 hours, and then left to stand for use; when the mixer is mixing, the speed is controlled to be 120 rpm, and the dispersant used during mixing is kerosene, and the amount of kerosene is 10wt.%. The D10 of the water-atomized copper powder used is 12.79μm; the D50 is 28.28μm, and the D90 is 56.72μm.
[0047] The fluidized high-efficiency oxidation-reduction fibrous copper powder is prepared by the following steps:
[0048] After pure copper is melted to form copper liquid, non-spherical copper powder is obtained by water atomization; the atomized copper powder is then subjected to fluidized oxidation on a copper powder fluidized bed device, and natural gas and air inlets are set at the bottom of the fluidized bed, with a volume ratio of natural gas to air of 1:1.5. The oxygen content of the powder after oxidation is ≥10%, and the oxidation efficiency is about 18% / min; the oxidized powder is subjected to bidirectional grinding and dispersion to obtain fibrous powder; the oxygen content of the powder after hydrogen reduction is ≤0.1%, and the obtained fluidized high-efficiency oxidation-reduction fibrous copper powder is sieved (the mesh number of the sieve is 400 mesh, and the sieve under is taken).
[0049] The particle size distribution composition of the obtained fluidized high-efficiency redox fibrous copper powder is as follows: copper powder with a particle size of less than 5 μm: 5.10 v%; copper powder with a particle size of 5 to 20 μm: 65.98 v%; copper powder with a particle size greater than 20 μm and less than or equal to 45 μm: 28.92 v%. The bulk density of the obtained fluidized high-efficiency redox fibrous copper powder is 1.26 g / cm 3 , specific surface area is 0.43m 2 / g;
[0050] The particle size of the tin powder used is 300 mesh; the particle size of the graphite used is 300 mesh.
[0051] 2. Mixing and molding: The mixed powders are loaded into a mold and pressed to obtain a green body; the pressure of the hydraulic press is 6 MPa and the holding time is 3 s; the strength of the green body is shown in Table 1;
[0052] 3. Sintering: The green body is sintered in a sintering furnace at a sintering temperature of 720°C for 2.5 hours.
[0053] The sintering atmosphere is hydrogen;
[0054] 4. The sintered parts are impregnated with oil and finished to obtain miniature oil-containing bearings. The cleaned products are dried, placed in a vacuum pump, heated to 80°C after vacuum extraction, and impregnated with imported Kanto oil 916P for 60 minutes. The strength and oil content of the miniature oil-containing bearings are shown in Table 1.
[0055] Embodiment 2:
[0056] 1. Raw material mixing: conventional spherical / quasi-spherical water-atomized copper powder, fluidized high-efficiency redox fibrous copper powder (fluidized high-efficiency redox fibrous copper powder is consistent with Example 1), tin, and graphite powder are configured in a mass ratio of 60:30:9:1, first manually mixed for 20 minutes, added to a mixer and mixed for 6 hours, and then allowed to stand for use; when the mixer is mixing, the speed is controlled to be 120 rpm, and the dispersant used during mixing is kerosene, and the amount of kerosene is 10wt.%. The water-atomized copper powder used is consistent with the water-atomized copper powder used in Example 1;
[0057] The particle size of the tin powder used is -300 mesh; the particle size of the graphite used is -300 mesh;
[0058] 2. Mixing and molding: The mixed powders are loaded into a mold and pressed to obtain a green body; the pressure of the hydraulic press is 6 MPa and the holding time is 3 s; the strength of the green body is shown in Table 1;
[0059] 3. Sintering: The green body is sintered in a sintering furnace at a sintering temperature of 720°C for 2.5 hours.
[0060] The sintering atmosphere is hydrogen;
[0061] 4. The sintered parts are impregnated with oil and finished to obtain miniature oil-containing bearings. The cleaned products are dried, placed in a vacuum pump, heated to 80°C after vacuum extraction, and impregnated with imported Kanto oil 916P for 60 minutes. The strength and oil content of the miniature oil-containing bearings are shown in Table 1.
[0062] The strength and oil content of the obtained miniature oil-containing bearing are shown in Table 1.
[0063] Example 3
[0064] 1. Mixing of raw materials: conventional spherical / quasi-spherical water-atomized copper powder, fluidized high-efficiency redox fibrous copper powder, copper powder, tin and graphite powder are prepared in a mass ratio of 0:90:9:1, first manually mixed for 20 minutes, added to a mixer and mixed for 6 hours, and then allowed to stand for use; when the mixer is mixing, the speed is controlled to be 120 rpm, and the lubricant used during mixing is kerosene, and the amount of kerosene is 10wt.%.
[0065] The particle size of the tin powder used is 300 mesh; the particle size of the graphite used is 300 mesh
[0066] The copper powder of the fibrous copper powder using fluidized high-efficiency oxidation-reduction is consistent with that in the embodiment; the water-atomized copper powder used is consistent with the water-atomized copper powder used in embodiment 1;
[0067] 2. Mixing and molding: The mixed powders are loaded into a mold and pressed to obtain a green body; the pressure of the hydraulic press is 6 MPa and the holding time is 3 s; the strength of the green body is shown in Table 1;
[0068] 3. Sintering: The green body is sintered in a sintering furnace at a sintering temperature of 720°C for 2.5 hours.
[0069] The sintering atmosphere is hydrogen;
[0070] 4. The sintered parts are impregnated with oil and finished to obtain miniature oil-containing bearings. The cleaned products are dried, placed in a vacuum pump, heated to 80°C after vacuum extraction, and impregnated with imported Kanto oil 916P for 60 minutes. The strength and oil content of the miniature oil-containing bearings are shown in Table 1.
[0071] Example 4
[0072] 1. Raw material mixing: conventional spherical / quasi-spherical water-atomized copper powder, fluidized high-efficiency redox fibrous copper powder (consistent with Example 1), tin, and graphite powder are prepared in a mass ratio of 30:60:9:1, first manually mixed for 20 minutes, added to a mixer and mixed for 6 hours, and then allowed to stand for use; when the mixer is mixing, the speed is controlled to be 120 rpm, and the dispersant used during mixing is kerosene, and the amount of kerosene is 10wt.%. The water-atomized copper powder used is consistent with the water-atomized copper powder used in Example 1;
[0073] The particle size of the tin powder used is 300 mesh; the particle size of the graphite used is 300 mesh 2. Mixing and molding: The mixed powders are loaded into a mold and molded into a green body; the pressure of the hydraulic press is 6 MPa and the holding time is 3 s; the strength of the green body is shown in Table 1;
[0074] 3. Sintering: The green body is sintered in a sintering furnace at a sintering temperature of 720°C for 2.5 hours.
[0075] The sintering atmosphere is hydrogen;
[0076] 4. The sintered parts are impregnated with oil and finished to obtain miniature oil-containing bearings. The cleaned products are dried, placed in a vacuum pump, heated to 80°C after vacuum extraction, and impregnated with imported Kanto oil 916P for 60 minutes. The strength and oil content of the miniature oil-containing bearings are shown in Table 1.
[0077] Comparative Example 1
[0078] 1. Raw material mixing: conventional spherical / quasi-spherical water-atomized copper powder, fluidized high-efficiency redox fibrous copper powder, copper powder, tin, and graphite powder are prepared in a mass ratio of 90:0:9:1, manually mixed for 20 minutes, added to a mixer and mixed for 6 hours, and then allowed to stand for use; when the mixer is mixing, the speed is controlled to be 120 rpm, and the lubricant used during mixing is kerosene, and the amount of kerosene is 10wt.%. The water-atomized copper powder used is exactly the same as the water-atomized copper powder used in Example 1.
[0079] The particle size of the tin powder used is -300 mesh; the particle size of the graphite used is -300 mesh
[0080] 2. Mixing and molding: The mixed powders are loaded into a mold and pressed to obtain a green body; the pressure of the hydraulic press is 6 MPa and the holding time is 3 s; the strength of the green body is shown in Table 1;
[0081] 3. Sintering: The green body is sintered in a sintering furnace at a sintering temperature of 720°C for 2.5 hours.
[0082] The sintering atmosphere is hydrogen;
[0083] 4. The sintered parts are impregnated with oil and finished to obtain miniature oil-containing bearings. The cleaned products are dried, placed in a vacuum pump, heated to 80°C after vacuum extraction, and impregnated with imported Kanto oil 916P for 60 minutes. The strength and oil content of the miniature oil-containing bearings are shown in Table 1.
[0084] Comparative Example 2
[0085] The other conditions are exactly the same as those in Example 1, except that: 3. Sintering: the green body is sintered in a sintering furnace at a sintering temperature for 2.5 hours.
[0086] The strength and oil content of the obtained miniature oil-containing bearing are shown in Table 1.
[0087] Comparative Example 3
[0088] The other conditions are exactly the same as those in Example 1; the difference is that the particle size distribution composition of the fluidized high-efficiency redox fibrous copper powder used is: copper powder with a particle size of less than 5 μm: 8.87 v%; copper powder with a particle size of 5 to 20 μm: 40.33 v%; copper powder with a particle size greater than 20 μm and less than or equal to 45 μm: 45.68 v%; copper powder with a particle size greater than 45 μm and less than or equal to 75 μm: 5.12 v%.
[0089] The strength and oil content of the obtained miniature oil-containing bearing are shown in Table 1.
[0090] Example 5
[0091] 1. Raw material mixing: Mix the redox fibrous bronze powder and graphite in a mass ratio of 98:2.
[0092] After 20 minutes of manual mixing, add the mixture into a mixer and mix for 6 hours, then let it stand for later use;
[0093] When the mixer is mixing, the speed is controlled to be 120 rpm, and the dispersant used during mixing is kerosene, and the amount of kerosene used is 10 wt.%.
[0094] Redox fibrous bronze powder is prepared by the following steps:
[0095] The fluidized high-efficiency redox fibrous copper powder obtained in Example 1 and 10wt% Sn powder were three-dimensionally mixed for 120 minutes and then sintered and granulated in a reduction furnace at a granulation temperature of 550-600°C. The sintered and granulated powder was crushed, sieved, and the particle size distribution was adjusted to obtain the finished powder.
[0096] The particle size distribution composition of the obtained fluidized high-efficiency redox fibrous bronze powder is: 0-20 μm: 0.71 v%; 20-45 μm: 8.92 v%; 45-100 μm: 43.77 v%; 100-200 μm: 44.28 v%; 200-400 μm: 2.32 v%. The bulk density of the obtained fluidized high-efficiency redox fibrous bronze powder is 2.68 g / cm 3 , specific surface area is 0.11m 2 / g; the particle size of the graphite used is 300 mesh;
[0097] 2. Mixing and molding: The mixed powders are loaded into a mold and pressed to obtain a green body; the pressure of the hydraulic press is 6 MPa and the holding time is 3 s; the strength of the green body is shown in Table 1;
[0098] 3. Sintering: The green body is sintered in a sintering furnace at a sintering temperature of 720°C for 2.5 hours.
[0099] The sintering atmosphere is hydrogen;
[0100] 4. The sintered parts are impregnated with oil and finished to obtain miniature oil-containing bearings. The cleaned products are dried, placed in a vacuum pump, heated to 80°C after vacuum extraction, and impregnated with imported Kanto oil 916P for 60 minutes. The strength and oil content of the miniature oil-containing bearings are shown in Table 1.
[0101] Example 6
[0102] The other conditions are the same as those in Example 5, except that: the redox fibrous bronze powder
[0103] , graphite was manually mixed for 20 minutes at a mass ratio of 99:1, added into a mixer and mixed for 6 hours and then allowed to stand for use; the strength and oil content of the obtained miniature oil-containing bearing are shown in Table 1.
[0104] Comparative Example 4
[0105] The other conditions are the same as those in Example 5, except that: 3. Sintering: The green body is sintered in a sintering furnace at a temperature of 850° C. for 2.5 h. The strength and oil content of the obtained micro oil-containing bearing are shown in Table 1.
[0106] Comparative Example 5
[0107] 1. Raw material mixing: commercial conventional bronze powder and graphite are used in a mass ratio of 99:1 and manually mixed for 20 minutes, added into a mixer and mixed for 6 hours and then left to stand for use; the particle size of the bronze powder is less than 400 microns; the composition of the bronze powder is exactly the same as that of Example 5;
[0108] When the mixer is mixing, the speed is controlled to be 120 rpm, and the dispersant used during mixing is kerosene, and the amount of kerosene used is 10 wt.%.
[0109] The bulk density of commercial bronze powder is 2.68g / cm 3 , specific surface area is 0.11m 2 / g; the particle size of the graphite used is 300 mesh;
[0110] 2. Mixing and molding: The mixed powders are loaded into a mold and pressed to obtain a green body; the pressure of the hydraulic press is 6 MPa and the holding time is 3 s; the strength of the green body is shown in Table 1;
[0111] 3. Sintering: The green body is sintered in a sintering furnace at a sintering temperature of 850°C for 2.5 hours.
[0112] The sintering atmosphere is hydrogen;
[0113] 4. The sintered parts are impregnated with oil and finished to obtain miniature oil-containing bearings. The cleaned products are dried, placed in a vacuum pump, heated to 80°C after vacuum extraction, and impregnated with imported Kanto oil 916P for 60 minutes. The strength and oil content of the miniature oil-containing bearings are shown in Table 1.
[0114] Comparative Example 6
[0115] The other conditions are the same as those in Example 5; the difference is that the particle size distribution composition of the redox fibrous bronze powder used is: 0-20 μm: 1.74 v%; 20-45 μm: 12.06 v%; 45-100 μm: 38.83 v%; 100-200 μm: 43.11 v%; 200-400 μm: 2.32 v%; 400-600 μm: balance. The bulk density of the obtained fluidized high-efficiency redox fibrous bronze powder is 2.68 g / cm 3 , specific surface area is 0.11m 2 / g; the particle size of the graphite used is 300 mesh;
[0116] The strength and oil content of the obtained miniature oil-containing bearing are shown in Table 1.
[0117] The crushing strength and oil content test performance of the bearings obtained in the embodiments and comparative examples are shown in Table
[0118]
[0119]
Claims
1. A micro oil-containing bearing material containing fluidized high-efficiency oxidized fibrous copper powder, Features: The raw materials used include by mass: 0-60 parts of water atomized copper powder; 20-100 parts of fluidized high-efficiency oxidation-reduction fibrous copper powder; 8-11 parts of tin powder; Graphite 0.5-2.0 parts; or The raw materials used include: bronze powder and graphite, and the mass ratio of each component is 98-99.5:0.5-2.0; The raw materials are mixed and then pressed and sintered to obtain an oil-containing bearing, and a hydrogen atmosphere is used during sintering and the sintering temperature is controlled to be 720-750° C.; The bulk density of the fluidized high-efficiency oxidation-reduction fibrous copper powder is 1.2-1.7 g / cm 3 , specific surface area is 0.35-0.50 m 2 / g; the fluidized high-efficiency redox fibrous copper powder is pure copper powder, and its purity is greater than or equal to 99.9%; the particle size distribution composition of the fluidized high-efficiency redox fibrous copper powder is: copper powder with a particle size of less than 5μm: 3-5v%; copper powder with a particle size of 5 to 20μm: 55-65v%; copper powder with a particle size greater than 20μm and less than or equal to 45μm: 28-35v%; The composition of the bronze powder is Cu 89.7 wt.%, Sn 9.8 wt.%, and other 0.5 wt.%; the preparation method is: fluidized high-efficiency oxidation-reduction fibrous copper powder and 10wt% Sn powder are three-dimensionally mixed for 120 minutes, sintered and granulated in a reduction furnace, the granulation temperature is 550-600°C, the sintered and granulated powder is crushed and sieved, and the particle size distribution is adjusted to obtain the finished product.
2. A micro oil-containing bearing material containing fluidized high-efficiency oxidized fibrous copper powder according to claim 1, Features: The raw materials used include: water atomized copper powder, fluidized high-efficiency oxidation-reduction fibrous copper powder, tin powder, and graphite, and the mass ratio of each component is 40-60:40-60:8-11:0.5-2.0; or The raw materials used include: fluidized high-efficiency oxidation-reduction fibrous copper powder, copper powder, tin, and graphite powder, which are configured in a mass ratio of 90:9:
1.
3. A micro oil-containing bearing material containing fluidized high-efficiency oxidized fibrous copper powder according to claim 1, Features: The fluidized high-efficiency redox fibrous copper powder is prepared by the following method: Pure copper is melted to form copper liquid, and then non-spherical copper powder is obtained by water atomization. Then, fluidized oxidation is carried out on a fluidized bed device, and the oxygen content after oxidation is ≥10%, and the oxidation efficiency is 15-20% / min. The oxidized powder is bidirectionally ground to obtain fibrous powder; hydrogen reduction is used before powdering, and the oxygen content of the reduced powder is ≤0.12%, and finally the reduced fibrous powder is obtained by screening.
4. A micro oil-containing bearing material containing fluidized high-efficiency oxidized fibrous copper powder according to claim 3, Features: The fibrous copper powder is in a suspended state during oxidation and is also in a suspended state during subsequent reduction.
5. A micro oil-containing bearing material containing fluidized high-efficiency oxidized fibrous copper powder according to claim 3, Features: The bulk density of the water atomized copper powder is controlled to be 1.8-2.0 g / cm 3 , specific surface area is 0.18-0.25m 2 / g; the particle size of the water atomized copper powder is less than or equal to 350 mesh; The particle size of tin powder is less than or equal to 300 mesh; The particle size of graphite is less than or equal to 300 mesh.
6. A micro oil-containing bearing material containing fluidized high-efficiency oxidized fibrous copper powder according to claim 1, Features: The bulk density of the bronze powder is 2.3-2.9 g / cm 3 , specific surface area is 0.04 m 2 / g; the bronze powder particle size is less than or equal to 100 mesh.
7. A micro oil-containing bearing material containing fluidized high-efficiency oxidized fibrous copper powder according to claim 6, Features: The bronze powder has a particle size distribution composition of: 0-20μm: <1v%; 20-45μm: 8-10v%; 45-100μm: 35-45v%; 100-200μm: 40-45v%; 200-400μm: 9-10v%.
8. A micro oil-containing bearing material containing fluidized high-efficiency oxidized fibrous copper powder according to any one of claims 1 to 7, Features: Prepared by the following steps: Step 1 Take each raw material according to the group, mix them evenly, and obtain the spare material; Step 2 The spare material is pressed to obtain a green body; during pressing, the pressure of the hydraulic press is controlled to be 15-17MPa and the holding time is 3-5s; Step 3 The green body is placed in a sintering furnace for sintering at a temperature of 720-750°C for 2-3 hours to obtain a sintered part; during sintering, the hydrogen atmosphere is controlled; Step 4 The sintered parts are impregnated with oil and finished to produce miniature oil-containing bearings.
9. A micro oil-containing bearing material containing fluidized high-efficiency oxidized fibrous copper powder according to any one of claims 1 to 7, Features: The obtained micro oil-containing bearing containing fluidized fibrous copper-based powder has a green strength of >12MPa, a crushing strength of the finished product of >200MPa, and an oil content of ≥24%.