A kind of acrylonitrile modified azo diamine chain extender and preparation method thereof

By introducing acrylonitrile-modified azo diamine chain extender into polyurethane materials, the rigidity of the hard segments is improved and decomposition is promoted, thus solving the problem of the difficulty in degrading polyurethane materials. Effective decomposition of both hard and soft segments is achieved, thereby improving the degradation ability and mechanical properties of the materials.

CN116178205BActive Publication Date: 2024-11-12WANHUA CHEM GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111429888.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-29
Publication Date
2024-11-12
Estimated Expiration
2041-11-29

AI Technical Summary

Technical Problem

Existing polyurethane materials are difficult to completely biodegrade after disposal, especially the hard segments, leading to environmental pollution problems. Furthermore, existing chain extenders cannot effectively improve the degradation performance of the materials.

Method used

Acrylonitrile-modified azo diamine chain extender is used. By introducing acrylonitrile-modified azo structure into the hard segment, the rigidity of the hard segment is improved, and it breaks under external conditions, promoting the decomposition of both hard and soft segments. The alkalinity of the o-alkoxy-p-phenylenediamine monomer is used to promote the decomposition of polyester segments.

Benefits of technology

It effectively improves the mechanical properties of polyurethane materials and achieves complete degradation of hard and soft segments under certain conditions, thus solving the environmental pollution problem of polyurethane materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003379738190000021
    Figure BDA0003379738190000021
  • Figure BDA0003379738190000022
    Figure BDA0003379738190000022
  • Figure BDA0003379738190000031
    Figure BDA0003379738190000031
Patent Text Reader

Abstract

The present invention relates to an acrylonitrile-modified azo diamine chain extender and a preparation method thereof. The obtained acrylonitrile-modified azo diamine chain extender can be used together with isocyanate and biodegradable polyester polyol to produce polyurethane-related products. Due to the special structural design of the chain extender, it can further improve the mechanical properties of polyurethane products, effectively improve the degradability of the products, and promote the degradation rate of the products. Such products can be applied to composite materials, sports paving materials and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polyurethane, and specifically relates to an acrylonitrile-modified azo diamine chain extender and a preparation method thereof. Technical Background

[0002] Chain extenders are commonly used additives in polyurethane formulations. Chain extenders can further extend the polymer hard segment molecular chain to generate linear molecules with larger molecular weight. Among them, diamine is an important type of chain extender. Its strong activity can be used in CPU, RIM and sports paving materials.

[0003] Polyurethane is a cross-linked polymer material obtained by thermal curing reaction of isocyanate, polyester or polyether polyol. The raw materials are completely dependent on petroleum-based resources. With the progress and development of society, petroleum resources are becoming increasingly depleted, which seriously restricts the development of the polyurethane industry. At the same time, polyurethane materials cannot be recycled after being discarded, and are difficult to degrade in the natural environment, causing "white pollution". The methods for treating polyurethane waste are mainly landfill and incineration. "Landfill treatment" occupies land resources and causes soil degradation, while "incineration treatment" produces a large amount of toxic gases, causing serious air pollution. Therefore, the development of environmentally friendly biodegradable polyurethane materials has become the focus of the materials field.

[0004] In recent years, the research on degradable polyurethane has become a hot topic of research. Patent CN111363117A provides a high-strength biodegradable modified polyurethane elastomer, which is reacted by the terminal hydroxyl group of polylactic acid-polycaprolactone block copolymer and the isocyanate group. That is, a degradable polylactic acid-polycaprolactone block copolymer is introduced into the polyurethane segment to give the polyurethane biodegradability. However, the degradable part is only the soft segment part in the polyurethane, which cannot affect the hard segment part therein, and the external factors in the polyurethane cross-linking system have limited internal influence on it, making the decomposition of polylactic acid slow. Thereby the degradation effect of the whole system is limited. Patent CN1314426 provides a method for preparing a modified polyurethane elastomer, that is, adding nitrated lignin to the polyurethane system, and adding degradable lignin to the system in a physical mixing manner to improve the biodegradability of the material. However, this method cannot solve the degradability problem of the cross-linked part of the polyurethane, and cannot effectively degrade the elastomer completely. Summary of the invention

[0005] The purpose of the present invention is to provide an acrylonitrile-modified azo diamine chain extender. Due to its own structural characteristics, the chain extender can improve the rigidity of the hard segment part and effectively improve the mechanical properties of the polyurethane product. At the same time, the polyurethane product using the chain extender can be guaranteed to decompose under certain external conditions. Since the chain extender belongs to the hard segment part of the polyurethane, the degradation problem of the hard segment of the polyurethane can be solved by its own degradation; the o-alkoxy-p-phenylenediamine monomer decomposed during the degradation process can effectively promote the decomposition of the polyester polyol in the system due to its own alkalinity, so that effective degradation can be achieved in both the soft and hard segments, and the degradation ability of the polyurethane product can be improved.

[0006] The technical solution of the present invention is as follows:

[0007] An acrylonitrile-modified azo diamine, the structural formula of which is:

[0008]

[0009] Wherein R1 is a C1-C20 alkyl group, and R2 is an alkylene group or an alicyclic group or an aromatic group bridging group. Further, R1 is preferably a C1-C4 alkyl group, such as methyl, ethyl, propyl, isopropyl or butyl; R2 is preferably an alicyclic group or a phenyl group bridging group, such as a methylene group, an ethylidene group or a propyl group, a butyl group, a phenyl group, a cyclohexyl group, a substituted cyclohexyl group, or a dicyclohexyl group bridging group.

[0010] In some specific embodiments, the structure of the acrylonitrile-modified azo diamine is as follows:

[0011]

[0012]

[0013] Preferably, the preparation method of the acrylonitrile-modified azo diamine comprises: adding primary amino azo diamine, acrylonitrile and a copper oxide catalyst into a reactor, reacting at 70-120° C. for 2-3 hours to generate acrylonitrile-modified azo diamine.

[0014] Among them, the primary amino azo diamine structure is:

[0015]

[0016] The reaction equation is:

[0017]

[0018] Wherein, the definitions of R1 and R2 are as described above.

[0019] Wherein, the molar ratio of primary amino azo diamine to acrylonitrile is 1:2-5;

[0020] The added amount of the catalyst is 0.1-1% of the sum of the mass of the primary amino azo diamine and acrylonitrile.

[0021] The preparation method of primary amino azo diamine comprises: reacting o-alkoxy p-phenylenediamine and diamine monomer under the action of a metal catalyst at 60-120° C. for 2-3 hours to generate primary amino azo diamine.

[0022] Preferably, the molar ratio of the o-alkoxy-p-phenylenediamine to the diamine monomer is 1:2-4;

[0023] The metal catalyst can be manganese dioxide, potassium dioxide, titanium dioxide, and the amount used is 1-5% of the sum of the amount of o-alkoxy-p-phenylenediamine and diamine monomer substances.

[0024] The reaction scheme of this reaction is as follows:

[0025]

[0026] Preferably, the diamine monomer is preferably one or more of aliphatic primary diamines, alicyclic primary diamines, and aromatic primary diamines, such as ethylenediamine, propylenediamine, butylenediamine, meta-xylene diamine, meta-phenylenediamine, 4,4'-diaminodicyclohexylmethane, isophoronediamine, etc., and 4,4'-diaminodicyclohexylmethane or isophoronediamine is further preferred, such as 4,4'-diaminodicyclohexylmethane or isophoronediamine of Wanhua Chemical;

[0027] Preferably, the o-alkoxy p-phenylenediamine is o-methoxy p-phenylenediamine, o-ethoxy p-phenylenediamine, o-propoxy p-phenylenediamine, and the like.

[0028] The acrylonitrile-modified azo diamine chain extender of the present invention can be used alone or in combination with other chain extenders, and after being mixed with polyether and plasticizer, it can be used as a curing agent component for producing polyurethane-related products. The related products can be applied to the fields of composite materials, elastomers and sports paving materials.

[0029] The beneficial effects of the present invention are:

[0030] 1. The present invention provides an acrylonitrile-modified azo diamine chain extender. The chain extender reacts after being mixed with isocyanate and polyol, and the benzene ring structure it contains can enhance the strength of the hard segment itself and improve the mechanical properties of the product. At the same time, after being modified by acrylonitrile, the chain extender has a secondary amine structure, and its activity is significantly lower than that of the primary amine. It can have enough time to fully react with the isocyanate monomer, ensuring that the soft and hard segments are fully separated, and improving the mechanical properties of the product. At the same time, the operation time can be extended, so that it has operability during use.

[0031] 2. The azo diamine structure in the present invention can be decomposed under certain external conditions (for example, under alkaline conditions, the azo bond breaks at an ambient temperature of 50°C to 70°C to generate two primary amino structures), wherein the azo bond breaks, and the o-alkoxy-p-phenylenediamine monomer is released in the system, that is, the hard segment is decomposed in the manner of chain extender decomposition. At the same time, due to the presence of the o-alkoxy-p-phenylenediamine monomer, the system is alkaline, and the o-alkoxy group can effectively improve its alkalinity, and under alkaline conditions, it can effectively promote the decomposition of polyester segments such as polylactic acid and polycaprolactone, thereby achieving the decomposition of the hard segment and effectively promoting the degradation of the soft segment containing the polyester segment, thereby enhancing the overall degradation capacity of the polyurethane product. DETAILED DESCRIPTION

[0032] The following examples will further illustrate the method provided by the present invention, but the present invention is not limited to the listed examples, and should also include any other known changes within the scope of the rights claimed by the present invention.

[0033] Some raw material sources:

[0034] o-Methoxy-p-phenylenediamine and o-ethoxy-p-phenylenediamine were purchased from Zhejiang Zhongcheng Co., Ltd.

[0035] MDI prepolymer: 200g C2020 polyether and 400g F3135 polyether were dehydrated at 120℃ for 2 hours, then cooled to 80℃ and added with 200g MDI50 for polymerization reaction to generate MDI prepolymer. Both polyether and MDI50 were from Wanhua Chemical Group Co., Ltd.

[0036] Example 1

[0037] (1) Add 2 mol of o-methoxy-p-phenylenediamine and 4 mol of 4,4'-diaminodicyclohexylmethane into a dry reactor, add 0.08 mol of titanium dioxide metal catalyst, and react at 120°C for 2 hours. After distillation, primary amino azo diamine is obtained.

[0038] (2) Take 1 mol of the primary amino azo diamine prepared in step 1 and 2 mol of acrylonitrile, add them into a dry reactor, add 0.03 mol of copper oxide catalyst, and react at 70°C for 2 hours. After distillation, acrylonitrile-modified azo diamine is obtained.

[0039] (3) 2g of the chain extender prepared in step (2) was mixed with 20g of C2020 polyether, 23g of long-chain chlorinated paraffin, and 55g of 400-mesh calcium carbonate filler, and after dehydration at 100°C for 2 hours, it was mixed with the MDI prepolymer in a mass ratio of 5:1 and mixed evenly using a stirrer.

[0040] According to the national standard GB 36246-2018, 13mm thick standard mechanical properties test specimens were cast and cured at room temperature for 7 days before mechanical properties testing. The specimens were tested on a universal tensile testing machine within the tensile speed range required by the national standard. The tensile shear strength of the specimens can reach 1.4Mpa and the elongation at break can reach 140%.

[0041] Degradation test: Cut a small sample of 10mm×10mm×5mm from the sample plate, immerse it in 25ml phosphate buffer solution (PH value = 7.2), place it in an environment of 37±1℃, take it out every 6-7 days, dry it in vacuum at 80℃ until it reaches constant weight, then weigh it and calculate its mass reduction percentage. After immersion for 20 days, the weight loss rate reaches 15.3%.

[0042] Example 2

[0043] (1) Add 2 mol of o-methoxy-p-phenylenediamine and 4 mol of isophorone diamine into a dry reactor, add 0.18 mol of manganese dioxide metal catalyst, and react at 60°C for 3 hours. After distillation, primary amino azo diamine is obtained.

[0044] (2) Take 1 mol of the primary amino azo diamine prepared in step 1 and 3 mol of acrylonitrile, add them into a dry reactor, add 0.03 mol of copper oxide catalyst, and react at 80°C for 2 hours. After distillation, acrylonitrile-modified azo diamine is obtained.

[0045] (3) 2 g of the chain extender prepared in step 2 was mixed with 18 g of F3135 polyether, 25 g of long-chain chlorinated paraffin, and 55 g of 400-mesh calcium carbonate filler. After dehydration at 100°C for 2 hours, it was mixed with the MDI prepolymer in a mass ratio of 4:1 and mixed evenly using a stirrer.

[0046] According to the national standard GB 36246-2018, 13mm thick standard mechanical properties test specimens were cast and cured at room temperature for 7 days before mechanical properties testing. The specimens were tested on a universal tensile testing machine within the tensile speed range required by the national standard. The tensile shear strength of the specimens can reach 1.3Mpa and the elongation at break can reach 138%.

[0047] Degradation test: Cut a small sample of 10mm×10mm×5mm from the sample plate, immerse it in 25ml phosphate buffer solution (PH value = 7.2), place it in an environment of 37±1℃, take it out every 6-7 days, vacuum dry it at 80℃ until it reaches constant weight, then weigh it and calculate its mass reduction percentage. After immersion for 20 days, the weight loss rate reaches 14.8%.

[0048] Example 3

[0049] (1) Add 2.2 mol of o-ethoxy-p-phenylenediamine and 4.5 mol of propylene diamine into a dry reactor, add 0.3 mol of potassium dioxide metal catalyst, and react at 100°C for 2.5 hours. After distillation, primary amino azo diamine is obtained.

[0050] (2) Take 2 mol of the primary amino azo diamine prepared in step 1 and 4 mol of acrylonitrile and add them into a dry reactor, add 0.04 mol of copper oxide catalyst, and react at 85°C for 2 hours. After distillation, acrylonitrile-modified azo diamine is obtained.

[0051] (3) 3 g of the chain extender prepared in step 2 was mixed with 19 g of C2020 polyether, 22 g of long-chain chlorinated paraffin, and 56 g of 400-mesh calcium carbonate filler. After dehydration at 100°C for 2 hours, it was mixed with the MDI prepolymer in a mass ratio of 3:1 and mixed evenly using a stirrer.

[0052] According to the national standard GB 36246-2018, 13mm thick standard mechanical properties test specimens were cast and cured at room temperature for 7 days before mechanical properties testing. The specimens were tested on a universal tensile testing machine within the tensile speed range required by the national standard. The tensile shear strength of the specimens can reach 1.2Mpa and the elongation at break can reach 130%.

[0053] Degradation test: Cut a small sample of 10mm×10mm×5mm from the sample plate, immerse it in 25ml phosphate buffer solution (PH value = 7.2), place it in an environment of 37±1℃, take it out every 6-7 days, vacuum dry it at 80℃ until it reaches constant weight, then weigh it and calculate its mass reduction percentage. After immersion for 20 days, the weight loss rate reaches 13.5%.

[0054] Comparative Example

[0055] 2g of 3,3'-dichloro-4,4'-diaminodiphenylmethane was mixed with 20g of C2020 polyether, 23g of long-chain chlorinated paraffin, and 55g of 400-mesh calcium carbonate filler. After dehydration at 100°C for 2 hours, it was mixed with MDI prepolymer at a mass ratio of 5:1 and mixed evenly with a stirrer. According to the requirements of the national standard GB 36246-2018, 13mm thick standard mechanical properties test specimens were cast and cured at room temperature for 7 days before mechanical properties testing. The specimen was tested by a universal tensile testing machine within the tensile speed range required by the national standard. The tensile shear strength of the specimen can reach 1.0Mpa and the elongation at break can reach 120%.

[0056] Degradation test: Cut a small sample of 10mm×10mm×5mm from the sample plate, immerse it in 25ml phosphate buffer solution (PH value = 7.2), place it in an environment of 37±1℃, take it out every 6-7 days, dry it in vacuum at 80℃ until it reaches constant weight, and then weigh it to calculate the percentage of mass reduction. After immersion for 20 days, the weight loss rate is 1%.

Claims

1. An acrylonitrile-modified azo diamine, characterized in that: Its structural formula is: Among them, R1 is a C1-C4 alkyl group; R2 is a bridging group of methylene, ethylene or propyl, butyl, phenyl or cyclohexyl.

2. The acrylonitrile-modified azo diamine according to claim 1, characterized in that: R1 is methyl, ethyl, propyl, isopropyl or butyl.

3. An acrylonitrile-modified azo diamine, characterized in that: Its structural formula is: Wherein, R1 is a C1-C4 alkyl group.

4. An acrylonitrile-modified azo diamine, characterized in that: Its structural formula is: Wherein, R1 is a C1-C4 alkyl group.

5. A method for preparing the acrylonitrile-modified azo diamine according to claim 1, comprising: Adding primary amino azo diamine, acrylonitrile and a catalyst into a reactor to react and generate acrylonitrile-modified azo diamine; Wherein, the structure of the primary amino azo diamine is: Among them, R1 is a C1-C4 alkyl group; R2 is a bridging group of methylene, ethylene or propyl, butyl, phenyl or cyclohexyl.

6. The method according to claim 5, characterized in that The molar ratio of primary amino azo diamine to acrylonitrile is 1:2-5.

7. The method according to claim 5 or 6, characterized in that: The catalyst is copper oxide, and the dosage is 0.1-1% of the sum of the mass of primary amino azo diamine and acrylonitrile.

8. The method according to any one of claims 5-6, characterized in that: The reaction conditions are 70-120°C for 2-3 hours.

9. The method according to claim 5, characterized in that The preparation method of primary amino azo diamine comprises: reacting o-alkoxy p-phenylenediamine and diamine monomer under the action of a metal catalyst to generate primary amino azo diamine, 10. The method according to claim 9, characterized in that The molar ratio of the o-alkoxy p-phenylenediamine to the diamine monomer is 1:2-4.

11. The method according to claim 9, characterized in that The metal catalyst is selected from manganese dioxide, potassium dioxide and titanium dioxide, and the amount used is 1-5% of the sum of the molar amounts of the o-alkoxy-p-phenylenediamine and the diamine monomers.

12. The method according to claim 9, characterized in that The reaction conditions are 60-120°C for 2-3 hours.

13. Use of the acrylonitrile-modified azo diamine according to any one of claims 1 to 4 in the preparation of polyurethane.