A kind of PET open-cell foam material and preparation method thereof
Through the combination of PET, PMDA and PTFE and supercritical fluid foaming technology, the problem of poor heat resistance of polymer open-cell foam in high-temperature environments is solved, and high-performance PET open-cell foam materials are prepared, which are suitable for high-temperature environments and exhibit It has excellent oil absorption performance and various excellent properties.
Patent Information
- Application Number
- CN202310128831.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-02-17
AI Technical Summary
Existing polymer open-cell foam materials have poor heat resistance in high-temperature environments and are difficult to be used in high-temperature environments. In particular, there is a lack of research on polymer open-cell foam materials.
Polyethylene terephthalate (PET) is used as the main material, combined with pyromellitic dianhydride (PMDA) and polytetrafluoroethylene (PTFE), and PET openings are prepared through melt blending and supercritical fluid foaming technology Foam material to achieve high opening ratio, small cell size and high foaming ratio.
Successfully prepared PET open-cell foam material with high open cell ratio (90%-96%), small cell size (10μm-100μm), high foaming ratio (35-40 times) and excellent oil absorption performance, suitable for high temperature environment, and has good thermal insulation, mechanical and chemical resistance properties.
Smart Images

Figure CN116178911B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a PET open-cell foam material and a preparation method thereof, belonging to the technical field of foam materials. Background Art
[0002] Compared with ordinary closed-cell foam, open-cell foam is a special foam material, especially reticulated foam, in which there is no cell wall between adjacent cells, and the entire volume of the material is a three-dimensional network composed of interconnected solid edges. This special open-cell structure not only makes the material have a very low density, but also gives it excellent adsorption properties. Therefore, open-cell foam materials can be widely used in fields such as filtration, adsorption and tissue engineering.
[0003] At present, the preparation of polymer open-cell foam materials is mostly concentrated on polyolefins, such as polypropylene, polyethylene, etc. Due to their poor heat resistance, these open-cell foam materials cannot be used in high-temperature environments.
[0004] As an engineering thermoplastic material, polyethylene terephthalate (PET) has excellent high temperature resistance, thermal insulation, good mechanical properties and chemical resistance. Closed-cell PET foam has been widely used in wind turbine blades, transportation, aerospace and other fields. However, there are few reports on the research of PET open-cell foam.
[0005] Therefore, developing a PET open-cell foam material and a preparation method thereof has become one of the problems to be solved urgently in this field. Summary of the invention
[0006] In order to solve the above technical problems, the object of the present invention is to provide a PET open-cell foam material and a preparation method thereof. The PET open-cell foam material of the present invention has a high open-cell ratio, a small cell size and a high foaming ratio.
[0007] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a PET open-cell foam material, whose raw material composition includes, by weight: 100 parts of polyethylene terephthalate (PET), 0.3-0.75 parts of pyromellitic dianhydride (PMDA) and 0.1-0.5 parts of polytetrafluoroethylene (PTFE).
[0008] According to a specific embodiment of the present invention, preferably, in parts by weight, the raw material composition of the PET open-cell foam material comprises: 100 parts of polyethylene terephthalate (PET), 0.45-0.6 parts of pyromellitic anhydride (PMDA) and 0.1-0.5 parts of polytetrafluoroethylene (PTFE). More preferably, in parts by weight, the raw material composition of the PET open-cell foam material comprises: 100 parts of polyethylene terephthalate, 0.45 parts of pyromellitic anhydride and 0.1-0.5 parts of polytetrafluoroethylene.
[0009] According to a specific embodiment of the present invention, preferably, the PET open-cell foam material has an open porosity of 90% to 96%, a cell size of 10 μm to 100 μm, and a foaming ratio of 35 to 40 times.
[0010] According to a specific embodiment of the present invention, preferably, the cell density of the PET open-cell foam material is 50 to 200 cells / mm 2 .
[0011] According to a specific embodiment of the present invention, preferably, the density of the PET open-cell foam material is 0.014-0.03 g / cm 3 The density is the density after removing the non-foam skin of the foam material.
[0012] According to a specific embodiment of the present invention, preferably, the oil absorption rate of the PET open-cell foam material is 12 g / g to 30 g / g, more preferably 20 g / g to 30 g / g. The oil absorption rate is the oil absorption rate obtained by testing after removing the non-foam skin of the foam material.
[0013] According to a specific embodiment of the present invention, preferably, the foaming temperature window of the PET open-cell foam material is 222°C to 228°C.
[0014] According to a specific embodiment of the present invention, preferably, the PET open-cell foam material is a reticular foam. That is, there is almost no cell wall between adjacent cells of the PET open-cell foam material, and only a reticular open-cell structure supported by a skeleton, and the entire volume of the material is a three-dimensional network composed of interconnected solid edges.
[0015] According to a specific embodiment of the present invention, preferably, the PET open-cell foam material is prepared by the following steps: polyethylene terephthalate, pyromellitic anhydride and polytetrafluoroethylene are melt-blended according to the weight of the raw materials, and then molded and foamed, and the foaming temperature is 222°C to 228°C to obtain the PET open-cell foam material.
[0016] According to a specific embodiment of the present invention, preferably, the preparation step of the above-mentioned PET open-cell foam material also includes, before melt blending, drying polyethylene terephthalate, pyromellitic anhydride and polytetrafluoroethylene. More preferably, the drying temperature of the polyethylene terephthalate is 150°C to 160°C, and the drying time is 5h to 7h. More preferably, the drying temperature of the pyromellitic anhydride and the polytetrafluoroethylene is 70°C to 80°C, and the drying time is 5h to 7h. The drying temperature and time of pyromellitic anhydride and polytetrafluoroethylene may be the same or different, as long as they are within the above range. The drying may be carried out using conventional drying equipment in the art, such as, but not limited to, a vacuum oven.
[0017] According to a specific embodiment of the present invention, preferably, in the preparation step of the above-mentioned PET open-cell foam material, the temperature of the melt blending is 270°C to 280°C. The melt blending and molding can be carried out using conventional blending and molding equipment in the art, such as but not limited to high-speed mixers, open mixers, internal mixers, torque rheometers, tablet presses, etc. The present invention preferably uses a torque rheometer for melt blending; more preferably, the rotation speed of the torque rheometer is 60rpm to 70rpm, and the melt blending time is 10min to 15min. The present invention preferably uses a tablet press for molding; more preferably, the blend pressed by the tablet press is a square sheet, the size of which can be 100mm×100mm×1mm, but not limited to this.
[0018] According to a specific embodiment of the present invention, preferably, in the preparation step of the above-mentioned PET open-cell foam material, the foaming specifically includes: using a supercritical fluid to perform foaming in an autoclave, maintaining the pressure in the autoclave at 18MPa to 23MPa, first raising the temperature to 265°C to 267°C, and keeping it warm for 1min to 5min to fully melt the formed blend, then reducing the temperature to 222°C to 228°C, keeping it warm for 1min to 5min, and then reducing the pressure in the autoclave to normal pressure to obtain the PET open-cell foam material.
[0019] According to a specific embodiment of the present invention, preferably, in the above-mentioned step of preparing the PET open-cell foam material, the supercritical fluid includes supercritical CO2 and / or supercritical nitrogen, etc. More preferably, the supercritical fluid is supercritical CO2.
[0020] The second aspect of the present invention provides a method for preparing the above-mentioned PET open-cell foam material, which comprises the following steps: according to the weight parts of the raw materials, polyethylene terephthalate, pyromellitic dianhydride and polytetrafluoroethylene are melt-blended, then molded, and then foamed, the foaming temperature is 222°C to 228°C, to obtain the above-mentioned PET open-cell foam material.
[0021] According to a specific embodiment of the present invention, preferably, the above-mentioned preparation method further comprises the following steps before melt blending: drying polyethylene terephthalate, pyromellitic anhydride and polytetrafluoroethylene. More preferably, the drying temperature of the polyethylene terephthalate is 150°C to 160°C, and the drying time is 5h to 7h. More preferably, the drying temperature of the pyromellitic anhydride and the polytetrafluoroethylene is 70°C to 80°C, and the drying time is 5h to 7h. The drying temperature and time of pyromellitic anhydride and polytetrafluoroethylene can be the same or different, as long as they are within the above range. The drying can be carried out using conventional drying equipment in the art, such as but not limited to a vacuum oven.
[0022] In the above-mentioned preparation method, preferably, the temperature of the melt blending is 270°C to 280°C. The melt blending and molding can be carried out using conventional blending and molding equipment in the art, such as but not limited to high-speed mixers, open mixers, internal mixers, torque rheometers, tablet presses, etc. The present invention preferably uses a torque rheometer for melt blending; more preferably, the rotation speed of the torque rheometer is 60rpm to 70rpm, and the melt blending time is 10min to 15min. The present invention preferably uses a tablet press for molding; more preferably, the blend pressed by the tablet press is a square sheet, the size of which can be 100mm×100mm×1mm, but is not limited thereto.
[0023] In the above preparation method, preferably, the foaming specifically includes: using a supercritical fluid to foam in an autoclave, maintaining the pressure in the autoclave at 18MPa to 23MPa, first raising the temperature to 265°C to 267°C, keeping it warm for 1min to 5min, so that the formed blend is fully melted, and then reducing the temperature to 222°C to 228°C, keeping it warm for 1min to 5min, and then reducing the pressure in the autoclave to normal pressure to obtain the PET open-cell foam material.
[0024] In the above preparation method, preferably, the supercritical fluid includes supercritical CO2 and / or supercritical nitrogen, etc. More preferably, the supercritical fluid is supercritical CO2.
[0025] The present invention preferably uses supercritical CO2 as a foaming agent, maintains the pressure in the autoclave at 18MPa to 23MPa, uses a temperature rise and fall foaming method, first raises the temperature to 265°C to 267°C, keeps the temperature for 1min to 5min, allows the formed blend to fully melt, then reduces the temperature to a suitable foaming temperature (i.e., 222°C to 228°C), keeps the temperature for 1min to 5min, and then quickly releases the pressure in the autoclave to normal pressure. A large pressure drop is formed by rapid pressure release, which provides power for the nucleation and growth of the bubbles and creates conditions for the formation of an open-cell structure, thereby preparing the PET open-cell foam material.
[0026] The present invention adopts pyromellitic dianhydride (PMDA) as a chain extender and polytetrafluoroethylene (PTFE) as a nucleating agent, adopts a melt blending method to prepare a PET / PMDA / PTFE blend, and then adopts a supercritical fluid as a foaming agent to prepare a high-performance PET open-cell foam material. The present invention studies the mechanism of PET open-cell foaming molding and the influence of heterogeneous nucleation on the open-cell foaming process. The present invention successfully prepares a PET open-cell foam material with a small cell size (10-100 μm) and uniform cell distribution, an open cell rate of 90-96%, and a foaming ratio of up to 35-40 times in a wide foaming temperature window range (222-228°C). In addition, the PET open-cell foam material of the present invention has an oil absorption ratio of up to 20-30 g / g, has excellent oil absorption performance, and can be widely used in the fields of filtration, adsorption and tissue engineering. In addition, the PET open-cell foam material of the present invention has excellent high temperature resistance, and still has excellent oil absorption performance in a high temperature (above 180°C) environment. At the same time, the PET open-cell foam material of the present invention also has excellent heat insulation performance, good mechanical properties, chemical resistance and other properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the foam morphology diagram of the PET foam material prepared in Comparative Example 2 at a foaming temperature of 216°C.
[0028] Figure 2 This is the foam morphology diagram of the PET foam material prepared at a foaming temperature of 216°C in Comparative Example 3.
[0029] Figure 3 This is the foam morphology diagram of the PET foam material prepared in Comparative Example 6 at a foaming temperature of 216°C.
[0030] Figure 4 These are the foam morphology diagrams of PET open-cell foam materials prepared in Comparative Examples 4 and 5 with different PMDA addition amounts at different foaming temperatures.
[0031] Figure 5This is the cell size distribution diagram of the PET open-cell foam materials prepared in Comparative Examples 4 and 5 with different PMDA addition amounts at different foaming temperatures.
[0032] Figure 6 These are the foam morphology diagrams of PET foam materials prepared in Comparative Examples 7, 8 and 9 with different MMT addition amounts at different foaming temperatures.
[0033] Figure 7a , Figure 7b and Figure 7c The pore size distribution diagrams of PET foam materials prepared by using different MMT addition amounts at different foaming temperatures are shown in Comparative Examples 7, 8 and 9 respectively.
[0034] Figure 8 This is the foam morphology diagram of the PET open-cell foam material prepared by CNCs at different foaming temperatures in Comparative Example 10.
[0035] Fig. 9 This is the cell size distribution diagram of the PET open-cell foam material prepared by CNCs at different foaming temperatures in Comparative Example 10.
[0036] Fig.10 These are the foam morphology diagrams of PET foam materials prepared by using SiO2 and carbon nanotubes at different foaming temperatures in Comparative Examples 11 and 12, respectively.
[0037] Fig.11 These are foam morphology diagrams of PET foam materials prepared at different foaming temperatures using different PTFE addition amounts in Example 1, Example 2, Example 3, and Comparative Example 1.
[0038] Fig.12 This is a diagram of the cell density of PET foam materials prepared in the examples and comparative examples at different PMDA addition amounts, different PTFE addition amounts, and different foaming temperatures.
[0039] Fig.13a , Fig.13b , Fig.13c and Fig.13d The pore size distribution diagrams of PET foam materials prepared at different foaming temperatures with different PTFE addition amounts in Example 1, Example 2, Example 3 and Comparative Example 1 are respectively shown.
[0040] Fig.14 It is a foaming temperature window diagram of the foam materials of Comparative Example 5, Comparative Example 4 and Examples 1 to 3.
[0041] Fig.15The oil absorption ratio and open porosity of the PET foam materials prepared in Comparative Example 4, Comparative Example 5, Comparative Example 7, Example 1, and Example 2 are shown.
[0042] Fig.16 This is a comparison chart of the oil absorption ratios of the PET open-cell foam materials prepared in Example 1 and Example 2 under normal temperature and high temperature conditions. DETAILED DESCRIPTION
[0043] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0044] Example 1
[0045] This embodiment provides a PET open-cell foam material, and its raw material composition includes, by weight: 100 parts of polyethylene terephthalate (PET), 0.45 parts of pyromellitic dianhydride (PMDA) and 0.1 parts of polytetrafluoroethylene (PTFE).
[0046] The PET open-cell foam material is prepared by the following steps:
[0047] The PET slices were placed in a vacuum oven and dried at 160°C for 6 hours, and the PMDA powder and PTFE powder were placed in a vacuum oven and dried at 80°C for 6 hours to remove moisture from the raw materials. According to the above weight parts, the dried PET, PMDA and PTFE were melt blended in a torque rheometer, wherein the temperature was set to 280°C, the speed was 60 rpm, and the time was 10 minutes;
[0048] The composite material obtained by melt blending in the torque rheometer was pressed into a square sheet of 100 mm×100 mm×1 mm by a tablet press to obtain a PET / PMDA / PTFE blend sheet for subsequent test characterization and preparation of open-cell foam;
[0049] The blend tablet (2cm×1cm×1mm) was placed in an autoclave, supercritical CO2 was used as a foaming agent, the pressure in the autoclave was maintained at 20MPa, and the temperature was first raised to 266°C and kept warm for 1min to fully melt the blend tablet, and then the temperature was lowered to a suitable foaming temperature (222°C, 224°C, 226°C, and 228°C, respectively). After keeping warm for 1min, the pressure in the autoclave was quickly released to normal pressure to obtain the PET open-cell foam material, and the sample number was recorded as 9. # The sample number represents 4 samples, corresponding to the above-mentioned different foaming temperatures.
[0050] Example 2
[0051] This embodiment provides a PET open-cell foam material, which comprises, by weight, 100 parts of polyethylene terephthalate (PET), 0.45 parts of pyromellitic dianhydride (PMDA), and 0.3 parts of polytetrafluoroethylene (PTFE). The preparation steps of the PET open-cell foam material are the same as those of Example 1. The sample number of the PET open-cell foam material is 10 # The sample number represents 4 samples, corresponding to the above-mentioned different foaming temperatures.
[0052] Example 3
[0053] This embodiment provides a PET open-cell foam material, and its raw material composition includes, by weight, 100 parts of polyethylene terephthalate (PET), 0.45 parts of pyromellitic dianhydride (PMDA), and 0.5 parts of polytetrafluoroethylene (PTFE). The preparation steps of the PET open-cell foam material are the same as those of Example 1. The sample number of the PET open-cell foam material is 11 # The sample number represents 4 samples, corresponding to the above-mentioned different foaming temperatures.
[0054] Comparative Example 1
[0055] This comparative example provides a PET foam material, which comprises, by weight, 100 parts of polyethylene terephthalate (PET), 0.45 parts of pyromellitic dianhydride (PMDA), and 0.7 parts of polytetrafluoroethylene (PTFE). The preparation steps of the PET foam material are the same as those of Example 1. The sample number of the PET foam material is 12 # The sample number represents 4 samples, corresponding to the above-mentioned different foaming temperatures.
[0056] The raw material compositions of the PET foam materials of Examples 1 to 3 and Comparative Example 1 are shown in Table 1.
[0057] Table 1
[0058] <![CDATA[Example 1 (9 # )]]> <![CDATA[Example 2 (10 # )]]> <![CDATA[Example 3 (11 # )]]> <![CDATA[Comparative Example 1 (12 # )]]> PET / phr 100 100 100 100 PMDA / phr 0.45 0.45 0.45 0.45 PTFE / phr 0.1 0.3 0.5 0.7
[0059] Comparative Examples 2 to 6
[0060] Comparative Examples 2 to 6 respectively provide PET foam materials, and the raw material composition thereof includes, by weight, 100 parts of polyethylene terephthalate (PET) and 0 to 0.75 parts of pyromellitic dianhydride (PMDA), and the specific composition is shown in Table 2. The sample numbers of the PET foam materials provided in Comparative Examples 2 to 6 are respectively 1 # , 2 # , 3 # , 4 # , 5 #The preparation steps of the PET foam materials of Comparative Examples 2 to 6 are basically the same as those of Example 1, except that the foaming temperatures are 216° C. and 218° C., respectively. Each sample number represents 2 samples, corresponding to two different foaming temperatures.
[0061] Table 2
[0062] <![CDATA[Comparative Example 2(1 # )]]> <![CDATA[Comparative Example 3(2 # )]]> <![CDATA[Comparative Example 4 (3 # )]]> <![CDATA[Comparative Example 5(4 # )]]> <![CDATA[Comparative Example 6(5 # )]]> PET / phr 100 100 100 100 100 PMDA / phr 0 0.3 0.45 0.6 0.75
[0063] Comparative Examples 7 to 9
[0064] Comparative Examples 7 to 9 respectively provide PET foam materials, and the raw material composition thereof includes, by weight, 100 parts of polyethylene terephthalate (PET), 0.75 parts of pyromellitic dianhydride (PMDA) and 0.05 to 0.15 parts of organic modified montmorillonite (MMT), and the specific composition is shown in Table 3. The sample numbers of the PET foam materials provided in Comparative Examples 7 to 9 are respectively recorded as 6 # , 7 # , 8 # The preparation steps of the PET foam materials of Comparative Examples 7 to 9 are basically the same as those of Example 1, except that the foaming temperatures are 214° C., 216° C., and 218° C., respectively. Each sample number represents 3 samples, corresponding to three different foaming temperatures.
[0065] Table 3
[0066] <![CDATA[Comparative Example 7 (6 # )]]> <![CDATA[Comparative Example 8 (7 # )]]> <![CDATA[Comparative Example 9 (8 # ) <!-- 5 -->]]> PET / phr 100 100 100 PMDA / phr 0.75 0.75 0.75 MMT / phr 0.05 0.1 0.15
[0067] Comparative Example 10
[0068] This comparative example provides a PET open-cell foam material, which comprises, by weight, 100 parts of polyethylene terephthalate (PET), 0.6 parts of pyromellitic dianhydride (PMDA) and 0.3 parts of cellulose nanocrystals (CNCs). The preparation steps of the PET open-cell foam material are the same as those of Example 1, and the foaming temperatures are 224° C. and 226° C. respectively.
[0069] Comparative Example 11
[0070] This comparative example provides a PET foam material, which comprises, by weight, 100 parts of polyethylene terephthalate (PET), 0.6 parts of pyromellitic dianhydride (PMDA) and 0.1 parts of SiO2. The preparation steps of the PET foam material are the same as those of Example 1, and the foaming temperatures are 214°C, 216°C and 218°C respectively.
[0071] Comparative Example 12
[0072] This comparative example provides a PET foam material, which comprises, by weight, 100 parts of polyethylene terephthalate (PET), 0.6 parts of pyromellitic dianhydride (PMDA) and 0.5 parts of carbon nanotubes. The preparation steps of the PET foam material are the same as those of Example 1, and the foaming temperatures are 214°C, 216°C and 218°C respectively.
[0073] The structure, performance, etc. of the foam materials prepared in the above examples and comparative examples are characterized and analyzed below.
[0074] <Opening Rate>
[0075] The non-foam skin of the foam material is removed to expose the porous structure for N2 penetration. The test was carried out in accordance with ASTM-D6226, and the applied N2 pressure was 0.07MPa. The low N2 pressure can minimize the collapse of the open-cell structure, and the measurement results were recorded after 20 minutes to ensure equilibrium.
[0076] <Cell Size>
[0077] The test was performed according to ASTM D3576-1977.
[0078] <Foaming ratio>
[0079] The expansion ratio is the density of the unfoamed sample (ρ o ) and the density of the foamed sample (ρ f ) ratio.
[0080] <Cell Density>
[0081] The surface morphology of the foam material was observed using a FEI QuantaFEG250 scanning electron microscope, and the cell density was counted. The selected SEM images contained at least 100 cells. 2 The number of internal pores was counted by selecting three SEM images from different positions and taking the average value.
[0082] <Oil Absorption Ratio>
[0083] The foam material was weighed after removing the non-foam skin, and then completely immersed in the test oil (VG32-Mobil), and weighed again after standing for 24 hours. The oil absorption ratio is the ratio of the re-weighed foam weight to the initial foam weight.
[0084] The analysis results of the structure, performance, etc. of the foam materials prepared in the above examples and comparative examples are as follows.
[0085] Comparative Example 2 (1 # ), Comparative Example 3 (2 #) The PET foam material prepared by the method has too little PMDA content and the PET melt strength is too low to support the foaming cell structure, resulting in collapse. Figure 1 For comparative example 2 (1 # ) Foam morphology of PET foam material prepared at a foaming temperature of 216°C. Figure 2 For comparative example 3 (2 # ) is a foam morphology diagram of a PET foam material prepared at a foaming temperature of 216°C. # ) The PET foam material prepared by the method has a too high PMDA content, which results in a PET melt strength that is too high and can only produce closed-cell foam, but no open-cell foam. Figure 3 For comparative example 6 (5 # ) Foam morphology of PET foam material prepared at a foaming temperature of 216°C.
[0086] Figure 4 For comparative example 4 (3 # )、Comparative Example 5(4 # ) Foam morphology of PET open-cell foam materials prepared at different foaming temperatures (216°C, 218°C) with different PMDA addition amounts. Figure 4 It can be seen that when the addition amount of PMDA is 0.45 parts and 0.6 parts, the cell wall strength and pressure drop are adapted to each other, and open-cell foam is successfully produced. However, only at a foaming temperature of 216°C, a mesh open-cell structure is formed in which there is no cell wall between adjacent cells and only a skeleton is used as support. This is because at 216°C, the foaming ratio of PET / PMDA (0.6) (Comparative Example 5) is 35 to 40 times, while at 218°C, the foaming ratio of PET / PMDA (0.45) (Comparative Example 4) is only 30 times. Since the thickness of the cell wall is affected by the foaming ratio, the greater the foaming ratio, the thinner the cell wall, so the degree of openness of PET / PMDA (0.6) is higher than that of PET / PMDA (0.45).
[0087] Figure 5 For comparative example 4 (3 # )、Comparative Example 5(4 # ) The cell size distribution diagram of PET open-cell foam materials prepared at different foaming temperatures (216°C, 218°C) with different PMDA addition amounts. Figure 5 It can be seen that the comparative example 4 (3 # )、Comparative Example 5(4 # The pore diameter of the PET open-cell foam material is between 20 μm and 250 μm, and the pore size is relatively large. The open-cell foam with a smaller pore size can better exert its adsorption characteristics.
[0088] Figure 6 For comparative example 7 (6# ), Comparative Example 8 (7 # ), Comparative Example 9 (8 # ) Foam morphology of PET foam materials prepared at different foaming temperatures (214°C, 216°C, 218°C) with different MMT addition amounts. Figure 6 It can be seen that after adding MMT to the branched PET foam, at a foaming temperature of 214°C, the cell size of PET / PMDA (0.75) / MMT (0.05) (Comparative Example 7) is smaller and the cell wall is thicker, while PET / PMDA (0.75) / MMT (0.1) (Comparative Example 8) and PET / PMDA (0.75) / MMT (0.15) (Comparative Example 9) successfully obtain a network open-cell structure. This shows that the lower foaming temperature allows the PET / PMDA / MMT blend to form crystals faster, and the open-cell structure cannot be generated when the crystals are stable. Compared with the composite material with an MMT addition of 0.05 parts, when the MMT addition is 0.1 parts and 0.15 parts, the melt viscosity of the PET / PMDA / MMT blend is lower, the time to form crystals is longer, and more time is given to the bubbles to grow, resulting in the formation of an open-cell foam structure. When the foaming temperature is 216℃, the melt strength of the PET / PMDA / MMT blend with 0.05 parts of MMT added is lower than that at 214℃, while the melts of the PET / PMDA / MMT blends with 0.1 and 0.15 parts of MMT added collapse due to insufficient melt strength and fail to successfully obtain an open-cell structure. When the foaming temperature is 218℃, the PET / PMDA / MMT blend melts with 0.05 and 0.1 parts of MMT added successfully produce open-cell foams. This is because at this temperature, the foaming ratio of the foam increases from 25 times to 30 times, and the cell walls between the cells become thinner, reducing the difficulty of opening the cells.
[0089] Compared with PMDA branched modified PET foam, the addition of MMT plays the role of bubble heterogeneous nucleating agent, which increases the bubble nucleation sites and plays a positive role in the formation of open-cell foam. Although open-cell foam was successfully prepared in a wider foaming temperature window (214℃-218℃), the problem of too large pore size was not significantly improved. The open-cell pore size was 10-130μm, and there was still an open-cell foam with a size of more than 100μm. The foaming ratio could only reach 30 times, and the foaming was uneven. Figure 7a , Figure 7b and Figure 7c Comparative Example 7 (6 # ), Comparative Example 8 (7 # ), Comparative Example 9 (8 #) Cell size distribution diagram of PET foam materials prepared with different MMT addition amounts at different foaming temperatures (214°C, 216°C, 218°C).
[0090] Figure 8 This is the foam morphology diagram of the PET open-cell foam material prepared by CNCs at different foaming temperatures (224°C, 226°C) in Comparative Example 10. Fig. 9 The cell size distribution diagram of the PET open-cell foam material prepared by CNCs at different foaming temperatures (224°C, 226°C) in Comparative Example 10. Comparative Example 10 uses PMDA for branching modification and further uses CNCs to prepare a PET open-cell foam material with a foaming ratio of about 35 times, an open porosity of 93-94%, and a cell size of 10-150μm. Figure 8 and Fig. 9 It can be seen that the cell size distribution of the PET open-cell foam material of Comparative Example 10 is uneven, which may be caused by the fracture of the skeleton. Since the open-cell foam was successfully prepared using cellulose nanocrystals, the inventors of this case speculate that the formation of rod-shaped crystal nuclei or fiber networks during the melt blending process promotes the stability of the cell structure and the formation of the open-cell structure during the foaming process.
[0091] Fig.10 The foam morphology diagrams of PET foam materials prepared by using SiO2 and carbon nanotubes at different foaming temperatures (216°C and 218°C) in Comparative Examples 11 and 12 respectively. Comparative Examples 11 and 12 can only produce closed-cell foam materials with a foaming ratio of about 25 times at foaming temperatures of 214°C, 216°C, and 218°C, and cannot produce open-cell foam materials. This is because the nucleating agents SiO2 and carbon nanotubes used in Comparative Examples 11 and 12 enhance the strength of the melt and increase the difficulty of breaking the cell wall.
[0092] Fig.11 For Example 1 (9 # )、Example 2(10 # )、Example 3 (11 # ), Comparative Example 1 (12 # ) Foam morphology of PET foam materials prepared at different foaming temperatures (222°C, 224°C, 226°C, 228°C) with different PTFE addition amounts. Fig.11 It can be seen that in Examples 1 to 3, with the addition of polytetrafluoroethylene, the cell diameters of the open-cell foams are reduced to 10 μm to 100 μm.
[0093] Fig.12This is a diagram of the cell density of PET foam materials prepared in the examples and comparative examples at different PMDA addition amounts, different PTFE addition amounts, and different foaming temperatures. Among them, it includes the PET foam material prepared at a foaming temperature of 218°C in Comparative Example 6 (PET / PMDA (0.75)), the PET foam material prepared at a foaming temperature of 218°C in Comparative Example 5 (PET / PMDA (0.6)), the PET foam material prepared at a foaming temperature of 218°C in Comparative Example 4 (PET / PMDA (0.45)), the PET foam material prepared at a foaming temperature of 216°C in Comparative Example 1 (PET / PMDA (0.45) / PTFE (0.7)), the PET foam material prepared at a foaming temperature of 228°C in Example 1 (PET / PMDA (0.45) / PTFE (0.1)), the PET foam material prepared at a foaming temperature of 222°C in Example 2 (PET / PMDA (0.45) / PTFE (0.3)), and the PET foam material prepared at a foaming temperature of 224°C in Example 3 (PET / PMDA (0.45) / PTFE (0.5)).
[0094] Depend on Fig.12 It can be seen that with the addition of polytetrafluoroethylene, the cell density of Examples 1 to 3 is greatly increased compared with the PET foam modified by PMDA branching. This is due to the unique CO2 affinity of polytetrafluoroethylene, which increases the nucleation sites, resulting in thinning of the cell wall and reducing the difficulty of forming an open-cell structure. The fiber network formed by polytetrafluoroethylene can improve the melt strength and viscosity of PET, and effectively prevent collapse caused by insufficient melt strength during the foaming process. In addition, PTFE fiber has a significant promoting effect on the crystallization performance of PET. It promotes the nucleation of cells during the foaming process, maintains the stability of the cell structure during the cooling process, reduces the size of the cells, and increases the cell density. In addition, the foaming ratio of the open-cell foam prepared by Examples 1 to 3 at different foaming temperatures is stable at about 35 to 40 times, which is significantly higher than the PMDA branched modified foam (Comparative Examples 3 to 6) and the foam added with MMT, CNCs, SiO2 or carbon nanotubes (Comparative Examples 7 to 12). Therefore. The technical solution of the present invention adopts PTFE, which increases the foaming ratio of the foam and reduces the difficulty of opening the foam cells.
[0095] When the addition amount of PTFE is 0.1 part (Example 1), the improved melt strength of PET is adapted to the thinned cell wall, and an open-cell structure is successfully obtained at a foaming temperature of 222°C to 228°C. When the addition amount of PTFE is increased to 0.3 part (Example 2) and 0.5 part (Example 3), at a foaming temperature of 222°C and 224°C, it is difficult to obtain the same open-cell structure as when the addition amount of PTFE is 0.1 part, because the effect of more PTFE on melt reinforcement is greatly improved, and is greater than the effect on the thinning of the cell wall, so it is impossible to form an open-cell structure with a high open-cell rate (more than 95%). Specifically, when the addition amount of PTFE is 0.3 part (Example 2), at a foaming temperature of 222°C, the open-cell rate of the obtained foam material is about 91%, the cell size is 10 to 70 μm, and the foaming ratio is 35 to 37 times. When the addition amount of PTFE is 0.3 parts (Example 2), at a foaming temperature of 224°C, the open porosity of the obtained foam material is about 92.5%, the pore size is 10-50 μm, and the foaming ratio is 35-38 times. When the addition amount of PTFE is 0.5 parts (Example 3), at a foaming temperature of 222°C, the open porosity of the obtained foam material is about 91%, the pore size is 10-70 μm, and the foaming ratio is 35-37 times. When the addition amount of PTFE is 0.5 parts (Example 3), at a foaming temperature of 224°C, the open porosity of the obtained foam material is about 93%, the pore size is 10-50 μm, and the foaming ratio is 36-38 times. Fig.13a , Fig.13b , Fig.13c and Fig.13d Embodiment 1 (9 # )、Example 2(10 # )、Example 3 (11 # ), Comparative Example 1 (12 # ) Cell size distribution diagram of PET foam materials prepared with different PTFE addition amounts at different foaming temperatures (222℃, 224℃, 226℃, 228℃).
[0096] However, at the foaming temperature of 226°C and 228°C, when the addition amount of PTFE is 0.3 parts (Example 2) and 0.5 parts (Example 3), the crystallized part of the PET / PMDA / PTFE blend is less than that at 222°C and 224°C, so the melt strength is also lower, and an open-cell structure can be successfully formed and the material has a high open-cell ratio (more than 95%). When the addition amount of PTFE is 0.7 parts (Comparative Example 1), the strength of the PET / PMDA / PTFE blend is too large, and an open-cell structure cannot be obtained at the foaming temperature of 222°C to 228°C.
[0097] Fig.14 The foaming temperature window diagram of the foam materials of Comparative Example 5, Comparative Example 4 and Examples 1 to 3. Fig.14 As shown, compared with the PMDA branched modified PET foam, the addition of PTFE effectively broadened the foaming temperature window of the prepared open-cell foam. The open-cell temperature window was increased from 216°C to 218°C (Comparative Example 4 (3 # )、Comparative Example 5(4 # )) successfully expanded to 222℃~228℃ (Example 1 (9 # )、Example 2(10 # )、Example 3 (11 # )).
[0098] The structure of the open-cell foam prepared in the embodiment of the present invention is a three-dimensional network structure, the open porosity is 90-96%, the cell size is 10-100 μm, the foaming ratio is 35-40 times, and the cell density is 50-200 / mm 2 The thinning of the cell walls due to the reduction in cell size and the increase in cell density can better adapt to the increased melt strength and is conducive to adjusting the cell structure in a wider foaming temperature window.
[0099] Fig.15 The oil absorption ratio and open porosity of the PET foam materials prepared in Comparative Example 4, Comparative Example 5, Comparative Example 7, Example 1, and Example 2 are shown. Fig.15 It can be seen that the oil absorption capacity is basically proportional to the open porosity. The larger the open porosity, the stronger the oil absorption capacity. The cell size of the foams in Comparative Examples 4 and 5 is between 10 μm and 250 μm. The smaller the cell size, the stronger the oil absorption capacity. In the PET / PMDA (0.75) / MMT (0.05) open-cell foam of the same formula in Comparative Example 7, the open porosity is different due to the difference in foaming temperature; when the foaming temperature is 216°C, the open porosity is 94.4% and the oil absorption ratio is 12.5 g / g; when the foaming temperature is 218°C, the open porosity is 89.3% and the oil absorption ratio is 8.5 g / g. The oil absorption ratio of the open-cell foam made of PMDA branched modified PET with an open porosity of 96.3% is also greater than that of the PET / PMDA foam sample with an open porosity of 91.5%. In addition, the oil absorption capacity of the open-cell foam samples prepared from branched PET (i.e., PET / PMDA) and PET / PMDA / MMT blends is not ideal because their cell sizes are not much different, and both have more cells larger than 100 μm.
[0100] Compared with branched PET (i.e., PET / PMDA) and PET / PMDA / MMT, the PET open-cell foam obtained by adding PTFE in Examples 1-3 of the present invention has a wider foaming temperature window. In the range of 222°C to 228°C, the PET / PMDA / PTFE composite materials of Examples 1-3 can all be foamed to obtain open-cell foams. When the amount of polytetrafluoroethylene added is 0.1 parts, the foam open-cell rate obtained at a foaming temperature of 228°C can reach 95.4%, and the oil absorption ratio is 28.4g / g. When the amount of polytetrafluoroethylene added is 0.3 parts, the foam open-cell rate obtained at a foaming temperature of 226°C can reach 95.9%, and the oil absorption ratio is 26.3g / g. Compared with the foams obtained in Comparative Example 7 (PET / PMDA (0.75) / MMT (0.05)) and Comparative Example 5 (PET / PMDA (0.6)) at a foaming temperature of 216°C, the oil absorption capacity of the open-cell foams prepared from the PET / PMDA / MMT blends in the examples of the present invention is significantly higher than that of the former when the open-cell ratios are similar. It can be seen that the reduction in the cell size of the open-cell foams in the examples greatly improves the oil absorption capacity of the open-cell foams.
[0101] Fig.16 This is a comparison chart of the oil absorption ratios of the PET open-cell foam materials prepared in Example 1 and Example 2 under normal temperature and high temperature conditions. The open-cell foam prepared from the PET / PMDA (0.45) / PTFE (0.1) blend of Example 1 at a foaming temperature of 226°C has an oil absorption ratio of 27.8 g / g at normal temperature, and an oil absorption ratio of 29.1 g / g when the oil absorption test temperature is 230°C. The open-cell foam prepared from the PET / PMDA (0.45) / PTFE (0.3) blend of Example 2 at a foaming temperature of 228°C has an oil absorption ratio of 26.9 g / g at normal temperature, and an oil absorption ratio of 27.9 g / g when the oil absorption test temperature is 230°C. Fig.16 It can be seen that the open-cell foam prepared in the embodiment of the present invention successfully inherits the excellent high temperature resistance of the PET material. Under the same open porosity, when the test temperature is 230°C, the measured oil absorption ratio is higher than that when the test temperature is room temperature. This is because high temperature promotes the movement and diffusion of molecules.
[0102] The inventors of this case have for the first time developed a strategy for preparing PET open-cell foam with high open porosity and small-sized pores. First, regarding the melt strength of the matrix resin; if the melt strength is too weak, the pore structure cannot be formed; if the melt strength is too strong, during the pressure relief process, the instantaneous change in pressure drop is not enough to provide enough power to break through the pore walls between adjacent pores, and only a closed-cell structure can be formed. The present invention introduces PMDA into the PET resin, enhances the PET melt strength through chain extension and branching, and controls the strength of the PET melt to adapt to the pressure drop by adjusting different contents of PMDA. Secondly, the thickness and strength of the pore wall largely determine the difficulty of preparing the open-cell foam. Adding a nucleating agent to the PET matrix can not only increase the nucleation sites to reduce the pore size and make the pore wall thinner, reducing the difficulty of forming an open-cell foam, but also induce faster crystallization to broaden the foaming temperature window, so that the foaming process can be better adjusted during the foaming process. At least through the above-mentioned embodiments and comparative examples of the present invention, it can be seen that not all nucleating agents can make the prepared foam material have satisfactory open porosity, expansion ratio and pore size, and thus have better oil absorption ratio. The present invention uses PTFE as a nucleating agent. Due to the unique CO2 affinity of PTFE, the adsorption of carbon dioxide is increased, the amorphous region of the polymer system is locally plasticized, and the formation of an open-cell structure is promoted. Pillar breakage and excessive melt strength are the main obstacles to achieving open-cell foam. Due to the introduction of PTFE, the present invention can induce PET to crystallize along the original fibers and improve the strength of the skeleton. Therefore, the present invention finally successfully prepared a PET open-cell foam material with a small pore size (10 to 100 μm) and uniform pore distribution, an open porosity of 90 to 96%, and a foaming ratio of up to 35 to 40 times in a wider foaming temperature window range (222°C to 228°C). According to the preferred technical solution of the present invention, the PET open-cell foam material of the present invention has an oil absorption ratio of 20 to 30 g / g, has excellent oil absorption performance, and can be widely used in the fields of filtration, adsorption, and tissue engineering. Moreover, the PET open-cell foam material of the present invention has excellent high temperature resistance, and still has excellent oil absorption performance in a high temperature (above 180° C.) environment.
Claims
1. A PET open-cell foam material, whose raw material composition comprises, by weight: 100 parts of polyethylene terephthalate, 0.45-0.6 parts of pyromellitic dianhydride and 0.1-0.5 parts of polytetrafluoroethylene; The PET open-cell foam material is a reticulated foam; The PET open-cell foam material has an open-cell rate of 90% to 96%, a cell size of 10 μm to 100 μm, and a foaming ratio of 35 to 40 times; The PET open-cell foam material is prepared by the following steps: polyethylene terephthalate, pyromellitic anhydride and polytetrafluoroethylene are melt-blended according to the weight of the raw materials, and then molded and foamed to obtain the PET open-cell foam material; The foaming specifically includes: using a supercritical fluid to perform foaming in an autoclave, wherein the supercritical fluid is supercritical CO2, maintaining the pressure in the autoclave at 18MPa-23MPa, first raising the temperature to 265°C-267°C, and keeping it warm for 1min-5min to fully melt the formed blend, then reducing the temperature to 222°C-228°C, keeping it warm for 1min-5min, and then reducing the pressure in the autoclave to normal pressure.
2. The PET open-cell foam material according to claim 1, wherein: The raw material composition of the PET open-cell foam material includes, by weight: 100 parts of polyethylene terephthalate, 0.45 parts of pyromellitic dianhydride and 0.1-0.5 parts of polytetrafluoroethylene.
3. The PET open-cell foam material according to claim 1, wherein: The oil absorption ratio of the PET open-cell foam material is 12 g / g to 30 g / g.
4. The method for preparing the PET open-cell foam material according to any one of claims 1 to 3, comprising the following steps: According to the weight of the raw materials, polyethylene terephthalate, pyromellitic anhydride and polytetrafluoroethylene are melt-blended, molded and then foamed to obtain the PET open-cell foam material; Among them, the foaming specifically includes: using a supercritical fluid to foam in an autoclave, the supercritical fluid is supercritical CO2, the pressure in the autoclave is maintained at 18MPa~23MPa, the temperature is first raised to 265℃~267℃, and kept warm for 1min~5min to allow the molded blend to fully melt, and then the temperature is reduced to 222℃~228℃, and after keeping warm for 1min~5min, the pressure in the autoclave is relieved to normal pressure.
5. The preparation method according to claim 4, wherein The preparation method further comprises the following steps before melt blending: drying polyethylene terephthalate, pyromellitic anhydride and polytetrafluoroethylene.
6. The preparation method according to claim 5, wherein: The drying temperature of the polyethylene terephthalate is 150° C. to 160° C., and the drying time is 5 hours to 7 hours.
7. The preparation method according to claim 5, wherein: The drying temperature of the pyromellitic dianhydride and the polytetrafluoroethylene is 70° C. to 80° C., and the drying time is 5 h to 7 h.
8. The preparation method according to claim 4, wherein The temperature of the melt blending is 270°C to 280°C.
9. The preparation method according to claim 8, wherein: A torque rheometer is used for melt blending; the rotation speed of the torque rheometer is 60 rpm to 70 rpm, and the melt blending time is 10 min to 15 min.
10. The preparation method according to claim 4, wherein: The tablet press is used for molding.
11. The preparation method according to claim 10, wherein: The blend was compressed into square flakes by tabletting machine.
Citation Information
Patent Citations
Oriented PBT micro-nano hole foam material and preparation method thereof
CN113789035A
Modified polyethylene glycol terephthalate foam material and preparation method thereof
CN115160745A
Low density foamed polymers
US20070059511A1