A method for recovering nickel-cobalt solution from waste nickel-cobalt-aluminum ternary precursor
Patent Information
- Application Number
- CN202310047036.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-01-31
AI Technical Summary
该现有技术存在的不足是:由于镍钴铝前驱体中的铁铝含量普遍为5000ppm左右,采用上述沉淀法将产生大量的氢氧化铁铝胶体渣,这种渣具有含水量大、过滤困难和镍钴含量高的缺点
[0018] 1. The insulation and aging temperature of the present invention is between 80°C and 90°C, which can reduce the moisture content of iron hydroxide and aluminum hydroxide colloidal slag, thereby improving the slag filtration performance and reducing the entrainment of iron hydroxide and aluminum hydroxide colloidal slag. Nickel cobalt metal.
Smart Images

Figure CN116179872B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new energy battery materials, and in particular to a method for recovering a nickel-cobalt solution from a waste nickel-cobalt-aluminum ternary precursor. Background Art
[0002] Nickel-cobalt-aluminum ternary precursor is one of the key raw materials for nickel-cobalt-aluminum ternary batteries. In the development and production process of nickel-cobalt-aluminum ternary precursors, some waste materials are inevitably generated. Since the nickel and cobalt content in the waste nickel-cobalt-aluminum precursor is high and its value is high, nickel and cobalt need to be separated from aluminum and impure iron and recycled.
[0003] In the prior art, the method for separating nickel and cobalt from iron and aluminum is to dissolve nickel and cobalt and iron and aluminum into a solution, adjust the pH value so that iron and aluminum form hydroxide precipitate slag, and then remove the iron and aluminum by filtering. The disadvantage of the prior art is that since the iron and aluminum content in the nickel-cobalt-aluminum precursor is generally about 5000ppm, the above precipitation method will produce a large amount of iron-aluminum hydroxide colloidal slag, which has the disadvantages of high water content, difficulty in filtering and high nickel and cobalt content.
[0004] Therefore, how to solve the problems of high water content, difficulty in filtration and high nickel-cobalt content in the iron-aluminum slag during the recovery of nickel-cobalt solution from waste nickel-cobalt-aluminum precursors in the prior art has become the subject to be studied and solved by the present invention. Summary of the invention
[0005] The purpose of the present invention is to provide a method for recovering nickel-cobalt solution from waste nickel-cobalt-aluminum ternary precursor.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for recovering nickel-cobalt solution from waste nickel-cobalt-aluminum ternary precursors, comprising:
[0008] Step 1, putting the waste nickel-cobalt-aluminum ternary precursor and acid solution into a reaction kettle;
[0009] Step 2: Adjust the reaction temperature in the reactor to 75-85°C, and add a reducing agent to the reactor until the waste nickel-cobalt-aluminum ternary precursor is completely reacted and dissolved;
[0010] After step 3 and step 2 are completed, the pH value of the slurry is adjusted to between 4 and 5, the temperature of the slurry is adjusted to 80-90° C., a filter aid is added and the mixture is kept warm for 1-3 hours; the amount of the filter aid added is 0.1-5% of the mass of the waste nickel-cobalt-aluminum ternary precursor;
[0011] Step 4: The slurry after aging is coarsely filtered through a filter press to remove most of the ferric aluminum hydroxide colloid and other water-insoluble matter, and then finely filtered through a precision filter to remove the remaining trace ferric aluminum hydroxide colloid and other water-insoluble matter. The two-stage filtration can ensure the filtration efficiency and filtration accuracy at the same time, and the filtered solution is the recovered nickel-cobalt solution.
[0012] According to a further technical solution, in step one, the ratio of the amount of hydrogen ion substance in the acid solution to the sum of 2*the amount of nickel substance + 2*the amount of cobalt substance + 3*the amount of aluminum substance in the nickel-cobalt-aluminum ternary precursor is 1:1.
[0013] A further technical solution also includes step 5, backwashing the slurry from the precision filter and returning it to the filter press for re-filtration, thereby improving the material recovery rate.
[0014] According to a further technical solution, in step 1, the acid solution is one of sulfuric acid, hydrochloric acid and nitric acid.
[0015] According to a further technical solution, in step 2, the reducing agent is one of hydrogen peroxide, sodium sulfite and sulfur dioxide.
[0016] According to a further technical solution, in step three, the filter aid is one of diatomaceous earth, activated carbon, graphite powder, polyacrylamide, and cellulose.
[0017] The working principle and advantages of the present invention are as follows:
[0018] 1. The heat preservation and aging temperature of the present invention is between 80°C and 90°C, which can reduce the water content of the iron hydroxide and aluminum hydroxide colloidal slag, thereby improving the slag filtering performance and reducing the nickel and cobalt metals entrained in the iron hydroxide and aluminum hydroxide colloidal slag.
[0019] 2. The present invention adds a filter aid, which has an adsorption effect on the colloid, can promote the agglomeration of the colloid, reduce the water content of the colloid, thereby improving the filtration performance and reducing the nickel and cobalt metals entrained in the iron hydroxide and aluminum hydroxide colloidal slag.
[0020] 3. The present invention adds a filter aid, which can form a filter layer on the surface of the filter cloth during the filtration process of the filter press, reduce the blockage of the filter cloth pores by the iron hydroxide and aluminum hydroxide colloidal residues, and increase the filtration speed.
[0021] 4. The slurry in the present invention is filtered by a filter press and a precision filter respectively, which can effectively intercept the aluminum hydroxide and iron hydroxide colloidal residues and realize the separation of nickel and cobalt from iron and aluminum.
[0022] 5. In the present invention, the slurry backwashed by the precision filter is returned to the filter press for filtration, which can effectively improve the metal recovery rate.
[0023] Compared with the prior art, the present invention can achieve the recovery of nickel-cobalt solution from waste nickel-cobalt-aluminum precursors, with the water content of aluminum ferric hydroxide colloid lower than 30%, the nickel-cobalt content of slag lower than 20%, the Al content in the nickel-cobalt solution lower than 30 ppm, and the iron content lower than 1 ppm. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Attached Figure 1 The figure is a flow diagram of an embodiment of the present invention. Implementation
[0025] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:
[0026] Embodiment: The present invention will be clearly described below with diagrams and detailed descriptions. After understanding the embodiments of the present invention, any person skilled in the art can make changes and modifications based on the techniques taught by the present invention without departing from the spirit and scope of the present invention.
[0027] The terms used herein are only for describing specific embodiments and are not intended to be limiting of the present invention. Singular forms such as "a", "this", "here", "this", and "the" as used herein also include plural forms. "Including", "including", "having", etc. as used herein are all open terms, that is, they mean including but not limited to.
[0028] The terms used in this document generally have the ordinary meaning of each term used in this field, in the context of the case and in the specific context, unless otherwise noted. Certain terms used to describe the present invention will be discussed below or elsewhere in this specification to provide additional guidance to those skilled in the art in describing the present invention.
[0029] See attached Figure 1 As shown, a method for recovering nickel-cobalt solution from waste nickel-cobalt-aluminum ternary precursor comprises:
[0030] Step 1, putting the waste nickel-cobalt-aluminum ternary precursor and acid solution into a reaction kettle;
[0031] Preferably, the ratio of the amount of hydrogen ion substance in the acid solution to the sum of 2*amount of nickel substance+2*amount of cobalt substance+3*amount of aluminum substance in the nickel-cobalt-aluminum ternary precursor is 1: 1. Preferably, the acid solution is one of sulfuric acid, hydrochloric acid and nitric acid.
[0032] Step 2: Adjust the reaction temperature in the reactor to 75-85°C, and add a reducing agent to the reactor until the waste nickel-cobalt-aluminum ternary precursor is completely reacted and dissolved;
[0033] Preferably, the reducing agent is one of hydrogen peroxide, sodium sulfite and sulfur dioxide.
[0034] After step 3 and step 2 are completed, the pH value of the slurry is adjusted to between 4 and 5, the temperature of the slurry is adjusted to 80-90° C., a filter aid is added and the mixture is kept warm for 1-3 hours; the amount of the filter aid added is 0.1-5% of the mass of the waste nickel-cobalt-aluminum ternary precursor;
[0035] Preferably, the filter aid is one of diatomaceous earth, activated carbon, graphite powder, polyacrylamide, and cellulose.
[0036] Step 4: The slurry after aging is coarsely filtered through a filter press to remove most of the ferric aluminum hydroxide colloid and other water-insoluble matter, and then finely filtered through a precision filter to remove the remaining trace ferric aluminum hydroxide colloid and other water-insoluble matter. The two-stage filtration can ensure the filtration efficiency and filtration accuracy at the same time, and the filtered solution is the recovered nickel-cobalt solution.
[0037] Step 5: The precision filter backwashes the slurry back to the filter press and filters it again, thereby increasing the material recovery rate.
[0038] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for recovering nickel-cobalt solution from waste nickel-cobalt-aluminum ternary precursor, characterized in that: include: Step 1, putting the waste nickel-cobalt-aluminum ternary precursor and the acid solution into a reactor, wherein the ratio of the amount of hydrogen ion substance in the acid solution to the sum of the amount of 2*nickel substance+2*cobalt substance+3*aluminum substance in the nickel-cobalt-aluminum ternary precursor is 1:1; Step 2: Adjust the reaction temperature in the reactor to 75-85°C, and add a reducing agent to the reactor until the waste nickel-cobalt-aluminum ternary precursor is completely reacted and dissolved; After step 3 and step 2 are completed, the pH value of the slurry is adjusted to between 4 and 5, the temperature of the slurry is adjusted to 80-90° C., a filter aid is added and the mixture is kept warm for 1-3 hours; the amount of the filter aid added is 0.1-5% of the mass of the waste nickel-cobalt-aluminum ternary precursor; the filter aid is one of diatomaceous earth, activated carbon, graphite powder, polyacrylamide, and cellulose; Step 4: The slurry after aging is coarsely filtered through a filter press to remove most of the ferric aluminum hydroxide colloid and other water-insoluble matter, and then finely filtered through a precision filter to remove the remaining trace ferric aluminum hydroxide colloid and other water-insoluble matter. The filtered solution is the recovered nickel-cobalt solution; Step 5: The precision filter backwashes the slurry back and returns it to the filter press for further filtration.
2. The method for recovering nickel-cobalt solution according to claim 1, characterized in that: In step 1, the acid solution is one of sulfuric acid, hydrochloric acid and nitric acid.
3. The method for recovering nickel-cobalt solution according to claim 1, characterized in that: In step 2, the reducing agent is one of hydrogen peroxide, sodium sulfite and sulfur dioxide.
Citation Information
Patent Citations
Method for preparing precursor of nickel-cobalt-aluminum ternary positive-electrode material by utilizing high-temperature alloy waste material
CN107585793A
Preparation method of low sodium sulfur nickel cobalt aluminum ternary precursor
CN110808369A
Recovery method of waste lithium batteries and battery-grade nickel-cobalt-manganese mixed crystal recovered and prepared by adopting method
CN111261967A
Method for preparing lithium carbonate and ternary precursor by recycling waste ternary lithium battery
CN112374511A
Preparation method of nickel-cobalt-aluminum ternary positive electrode material precursor
CN113582255A