A lithium battery copper foil annealing process

Through the segmented annealing process, the lithium battery copper foil is heated in segments at low temperatures, which solves the problems of increasing the elongation rate and surface oxidation of the lithium battery copper foil, achieving an elongation increase of 1-5%, while maintaining the non-oxidation state of the product. , suitable for the annealing process of ultra-thin lithium battery copper foil.

CN116179978BActive Publication Date: 2024-10-01JIANGXI HUAXIN MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310148615.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-22
Publication Date
2024-10-01
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

The elongation rate of existing chromium-plated lithium battery copper foil cannot be improved, and high-temperature annealing can easily cause oxidation of the copper foil surface, resulting in product scrap.

Method used

Using a segmented annealing process, first raise the room temperature to 100°C and keep it for 0.5h-30h, then raise it to 200°C and keep it for 0.5h-20h in a vacuum or nitrogen protected environment. The heating rate is 10°C/h-100°C/h. , to prevent oxidation and discoloration.

Benefits of technology

It significantly increases the elongation of copper foil by 1-5% and maintains the non-oxidation state of the surface and end faces. The method is simple and low-cost, and is suitable for the annealing process of ultra-thin lithium battery copper foil (3-10 microns).

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116179978B_ABST
    Figure CN116179978B_ABST
Patent Text Reader

Abstract

The invention discloses a lithium battery copper foil annealing process, comprising the following steps: (1) subjecting the copper foil to an anti-oxidation treatment, wherein the anti-oxidation liquid is a chromium liquid; (2) one-stage annealing: subjecting the copper foil subjected to the anti-oxidation treatment to a one-stage annealing, wherein the temperature of the one-stage annealing is raised from room temperature to 100°C, and the temperature is kept for 0.5h-30h; (3) two-stage annealing: subjecting the copper foil subjected to the one-stage annealing to a two-stage annealing directly in a vacuum environment or a nitrogen protection environment, wherein the temperature of the two-stage annealing is raised from 100°C to 200°C, and the temperature is kept for 0.5h-20h. The invention has the beneficial effect that after the annealing process is completed, the elongation of the copper foil is increased by 1-5%, and there is no oxidation discoloration on the surface and end face of the copper foil after annealing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electrolytic copper foil manufacturing methods, and in particular to a lithium battery copper foil annealing process. Background Art

[0002] Copper foil is one of the indispensable materials for the negative electrode current collector of lithium-ion batteries. In recent years, ultra-thin copper foil has been used more and more widely. The thinner the copper foil, the lower the elongation. Low elongation will cause lithium-ion batteries to be subject to alternating stress during the electrochemical cycle, resulting in frequent wrinkling and belt breakage, which not only increases production costs, but also makes battery cell companies face greater quality risks. At present, several of the top ten lithium battery companies in China have clearly put forward the demand for high-elongation electrolytic copper foil to various electrolytic copper foil manufacturers. At the same time, according to the current status of lithium battery technology, lithium battery manufacturers will put forward higher requirements for the elongation of copper foil in order to reduce the risk of pole piece breakage during the pole piece processing process and battery charging and discharging process. High-elongation copper foil will play a key role in improving the high energy density of batteries, so the development of high-elongation lithium battery copper foil production process technology will be an inevitable trend of technological development.

[0003] Lithium battery copper foil is mainly prepared by electrolytic copper sulfate method, with a thickness of 3-10 microns. The process flow is copper wire---add sulfuric acid, prepare copper sulfate solution---prepare additives---mix into copper sulfate electrolyte---foil production machine---surface anti-oxidation treatment---rolling---annealing---slitting---quality inspection---warehousing.

[0004] At present, the main methods for improving the elongation of lithium battery copper foil prepared by electrolysis are additive improvement and low-temperature 50-100℃ stress relief annealing. Among them, annealing is mainly used to improve warpage and eliminate stress. For example, Jia Jintao, Wang Junyi, Zhu Shengxing, etc., in the patent "An electronic copper foil stress elimination device and elimination method" (CN112746164A), involve a device and method for eliminating copper foil stress, which is heated to 40-100℃ and baked for 10-24h, and then cooled to eliminate the internal stress of the copper foil. Nitrogen is provided in the heating mechanism as a protective gas. Liu Chao, Fan Yuanpeng, and Jiang Yang, in their patent "An annealing method for quickly reducing the internal stress of lithium battery copper foil" (CN111733371A), control the temperature of the copper foil during the winding process to achieve the purpose of stress release of the copper foil; directly use the electrolysis time to anneal the unfolded copper foil, which has the advantages of sufficient annealing, time saving and stable product quality. The first annealing system controls the temperature of the copper foil at 80-100°C, and the second annealing system controls the temperature of the copper foil at 60-80°C; Lu Lei, Cheng Zhao, and Jin Shuai, in their patent "A high-elongation electrolytic copper foil and its preparation method" (CN113621999 A), involve a method for preparing high-elongation electrolytic copper foil in the field of copper clad laminates. During the annealing process, the annealing temperature is 300-600°C and the time is 2-200 minutes; argon or nitrogen is used as a protective atmosphere during the annealing process.

[0005] The above patents mainly involve stress relief annealing of copper foil (<100℃) or the preparation of high elongation electrolytic copper foil in the field of copper clad laminates. It does not involve an annealing process for improving the elongation of lithium battery copper foil by medium and low temperature annealing (100℃~300℃). The existing copper foil annealing mainly involves stress relief annealing to improve the surface warping of copper foil; the annealing of copper clad laminates mainly improves the elongation, and the annealing temperature is relatively high, and the anti-oxidation treatment requires special treatment, such as surface galvanizing and nickel plating; the elongation of lithium battery copper foil is mainly improved by additives and stress relief annealing, so that the internal grains grow in the self-annealing process and low-temperature annealing process, and the impurities at the grain boundaries are eliminated; the anti-oxidation treatment of lithium battery copper foil is mostly achieved by surface chrome plating. The chrome plating process has a temperature resistance of no more than 100℃ in an air environment. Excessive annealing temperature can easily cause oxidation of the copper foil surface, resulting in the scrapping of the copper foil. Summary of the invention

[0006] The technical problem to be solved by the present invention is that the elongation of the existing lithium battery copper foil with chromium plating on the surface cannot be improved, and for this purpose, a lithium battery copper foil annealing process is provided.

[0007] After exploration, the present invention mainly designs an annealing process for improving the elongation of lithium battery copper foil in a low-cost surface chrome plating process.

[0008] The technical solution of the present invention is: a lithium battery copper foil annealing process, comprising the following steps: (1) subjecting the copper foil to an anti-oxidation treatment, wherein the anti-oxidation liquid is a chromium liquid; (2) first-stage annealing: subjecting the copper foil subjected to the anti-oxidation treatment to a first-stage annealing, wherein the temperature of the first-stage annealing is increased from room temperature to 100°C, and the temperature is kept for 0.5h-30h; (3) second-stage annealing: subjecting the copper foil subjected to the first-stage annealing to a second-stage annealing directly in a vacuum environment or a nitrogen protection environment, wherein the temperature of the second-stage annealing is increased from 100°C to 200°C, and the temperature is kept for 0.5h-20h.

[0009] The heating rate of the first stage annealing in the above scheme is 10°C / h-100°C / h.

[0010] The heating rate of the second-stage annealing in the above scheme is 10°C / h-100°C / h.

[0011] During the second-stage annealing in the above scheme, the oxygen content in the annealing device is ≤2000ppm.

[0012] In the above solution, the copper foil is wound on the inner sleeve, and through holes are formed on two end surfaces of the inner sleeve.

[0013] The anti-oxidation treatment parameters in the above scheme are: pH value 2-4, CrO3 0.8 g / L -1.2 g / L, COD 2000 mg / L -10000 mg / L, and anti-oxidation liquid temperature 20°C -40°C.

[0014] The anti-oxidation treatment described in the above scheme is double-sided chrome plating, and the total chrome content is ≤150ppm.

[0015] The beneficial effect of the present invention is that after the annealing process is completed, the elongation of the copper foil is increased by 1-5%, and there is no oxidation discoloration on the surface and end face of the copper foil after annealing; the method is simple, the cost is low, and the effect of improving the elongation of the copper foil is obvious, and it is suitable for the annealing of the current ultra-thin lithium battery copper foil (3-10 microns). BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is the EBSD image of the lithium battery copper foil before annealing treatment of the present invention;

[0017] Figure 2 This is the EBSD image of the lithium battery copper foil after annealing treatment of the present invention;

[0018] Figure 3 It is a grain map of the present invention after a stage of annealing;

[0019] Figure 4 This is the grain map of the present invention after the second stage annealing;

[0020] Figure 5 This is a photo of the lithium battery copper foil after annealing of the present invention;

[0021] Figure 6 This is a photo of the lithium battery copper foil of the present invention with an annealing temperature exceeding 100°C;

[0022] Figure 7 It is a schematic diagram of an inner sleeve of the present invention. Implementation

[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments by ordinary technicians in this field without creative work are within the protection scope of the present invention.

[0024] Lithium battery copper foil production process:

[0025] Copper wire---add sulfuric acid to prepare copper sulfate solution---prepare additives---mix into copper sulfate electrolyte---produce foil on foil machine---surface anti-oxidation treatment---rolling---annealing---slitting---quality inspection---warehousing.

[0026] The innovation of the present invention lies in the second stage 100℃-200℃ elongation annealing and segmented continuous annealing. Compared with the ordinary two-stage annealing, there is no intermediate cooling and then heating process. The staged heating method is adopted. The first reason is that the staged heating provides continuous power for the growth of copper foil grains to cross the energy barrier, making the grain growth more uniform. It was found in the experiment that when the ultra-thin lithium battery copper foil (below 6μm) involved in this patent is subjected to a one-stage annealing treatment below 100℃, the average grain size of the copper foil is maintained at 6.49, the median grain size is maintained at 5.6, and the grain size diagram is as follows: Figure 3 As shown in the figure, after the second stage annealing, the average grain size of the copper foil increases to 9.41, and the median grain size increases to 8.84. Figure 4 In addition, the ultra-thin lithium battery copper foil involved in this patent will not be oxidized and discolored when the foil surface and end surface are annealed below 100°C in the case of the existing chrome-plated anti-oxidation layer. Figure 5 As shown; when the annealing temperature is greater than 100°C, the foil surface and end surface will obviously show oxidation discoloration, such as Figure 6 As shown; Based on the above, 100℃ is taken as the critical temperature of the first and second stage annealing.

[0027] 1. Anti-oxidation treatment of copper foil, the anti-oxidation liquid is chromium liquid, the anti-oxidation treatment parameters are: pH value 2-4, CrO3 content 0.8g / L -1.2g / L, COD2000mg / L -10000mg / L, anti-oxidation liquid temperature 20℃-40℃.

[0028] 2. The surface chrome plating process is double-sided chrome plating on the smooth surface and the rough surface, and the total chrome content is ≤150ppm;

[0029] 3. The annealing heating time is 3h-10h, the annealing holding temperature is 50°C-200°C, and the annealing heating time is 0.5h-20h;

[0030] 4. The annealing parameters are a heating rate of 10°C / h -100°C / h;

[0031] 5. The heating is divided into two stages. The first stage is the stress relief annealing stage, the annealing temperature is increased from room temperature to 100°C, and the temperature is kept for 0.5h-30h; the second stage is the elongation improvement annealing stage, the annealing temperature is increased from 100°C to 200°C, and the temperature is kept for 0.5h-20h;

[0032] 6. The annealing environment is vacuum or nitrogen gas protection, wherein the oxygen content in the furnace is ≤2000ppm;

[0033] 7. The inner sleeve used for annealing the copper foil is a hollow steel sleeve with a through hole on the end face;

[0034] Comparative Example 1: 6 micron lithium battery copper foil, roll size 6 micron * 20000 meters, after anti-oxidation chromium plating surface treatment, Cr content 120ppm. Annealing process is 50℃ / 8h, cooled to room temperature and sampled for testing, tensile strength 350Mpa, elongation 7.22%.

[0035] Comparative Example 2: 6 micron lithium battery copper foil, roll size 6 micron * 20000 meters, after anti-oxidation chromium plating surface treatment, Cr content 120ppm. Annealing process is 90℃ / 16h, cooled to room temperature and sampled for testing, tensile strength 342Mpa, elongation 7.78%.

[0036] Example 1: 6 micron lithium battery copper foil, roll specification 6 micron * 20000 meters, after anti-oxidation chromium plating surface treatment, Cr content 120ppm. The annealing process is divided into two stages. The first stage is the stress relief annealing stage. The annealing temperature is increased from room temperature to 100℃, the heating rate is 20℃ / h, and the temperature is kept for 5h; the second stage is the elongation annealing stage. The annealing temperature is increased from 100℃ to 200℃, the heating rate is 20℃ / h, and the temperature is kept for 8h. Vacuum annealing, the oxygen content in the furnace is ≤2000ppm, and the sample is cooled to room temperature to test the tensile strength of 335Mpa and the elongation is 10.40%.

[0037] Example 2: 6 micron lithium battery copper foil, roll specification 6 micron * 20000 meters, after anti-oxidation chromium plating surface treatment, Cr content 120ppm. The annealing process is divided into two stages. The first stage is the stress relief annealing stage. The annealing temperature is increased from room temperature to 100℃, the heating rate is 20℃ / h, and the temperature is kept for 5h; the second stage is the elongation annealing stage. The annealing temperature is increased from 100℃ to 200℃, the heating rate is 20℃ / h, and the temperature is kept for 8h. Nitrogen annealing, the oxygen content in the furnace is ≤2000ppm, and the sample is cooled to room temperature for testing. The tensile strength is 338Mpa and the elongation is 10.23%.

[0038] Example 3: 6 micron lithium battery copper foil, roll specification 6 micron * 20000 meters, after anti-oxidation chromium plating surface treatment, Cr content 120ppm. The annealing process is divided into two stages. The first stage is the stress relief annealing stage. The annealing temperature is increased from room temperature to 100℃, the heating rate is 30℃ / h, and the temperature is kept for 5h; the second stage is the elongation annealing stage. The annealing temperature is increased from 100℃ to 200℃, the heating rate is 30℃ / h, and the temperature is kept for 20h. Nitrogen annealing, the oxygen content in the furnace is ≤2000ppm, and the sample is cooled to room temperature for testing. The tensile strength is 328Mpa and the elongation is 10.91%.

[0039] Comparative Example 3: 6 micron lithium battery copper foil, roll size 6 micron * 20000 meters, after anti-oxidation chromium plating surface treatment, Cr content 120ppm. The annealing process is divided into two stages. The first stage is the stress relief annealing stage. The annealing temperature is increased from room temperature to 100℃, the heating rate is 30℃ / h, and the temperature is kept for 5h; the second stage is the elongation annealing stage. The annealing temperature is increased from 100℃ to 200℃, the heating rate is 30℃ / h, and the temperature is kept for 8h. Annealing in air environment, cooling to room temperature, sampling and testing of tensile strength 332Mpa, elongation 4.56%.

[0040] The data of the above embodiments and comparative examples are shown in the following table:

[0041]

[0042] As can be seen from the above table, the two-stage annealing treatment of the present invention is helpful to improve the elongation of the surface chromium-plated lithium battery copper foil, with an improvement of 1-5%. Taking into account the temperature resistance of chromium in the surface chromium plating anti-oxidation process, the glossiness and hardness did not change significantly when the two-stage heating was performed below 200°C, thus determining the annealing temperature range, that is, below 100°C, the elongation will not be improved, and above 200°C, the foil surface and end surface will be oxidized and discolored.

[0043] According to current experimental data, the electrolytic electrodeposition method produces copper foil with smaller initial grains and the presence of impurity elements (such as carbon C and oxygen O in additives) in the grain boundaries, which makes the mechanical properties of the copper foil just rolled up 680Mpa-730Mpa and the elongation 3%-5%. After baking or storing at a certain temperature for 3-5 days (self-annealing effect), the mechanical properties change. After changing to a stable state, the mechanical properties are 300Mpa-400Mpa, and the elongation is further improved. Current experimental data show that the grain size before and after annealing differs by 3-4 times. Figure 1 and Figure 2 shown.

[0044] like Figure 7 As shown, the opening on the end face of the inner sleeve is beneficial to the heat transfer in the nitrogen environment, so that the copper foil is heated more evenly, and the uniform heating will also make the mechanical properties of the inner and outer copper foils more uniform.

Claims

1. A lithium battery copper foil annealing process, characterized in that: The following steps are involved: (1) The copper foil is subjected to anti-oxidation treatment, and the anti-oxidation liquid is chromium liquid; (2) One-stage annealing: The copper foil that has undergone anti-oxidation treatment is subjected to one-stage annealing, wherein the temperature of the one-stage annealing is increased from room temperature to 100°C and kept warm for 0.5h-30h; (3) Two-stage annealing: The copper foil that has undergone one-stage annealing is directly subjected to two-stage annealing in a vacuum environment or a nitrogen protection environment, wherein the temperature of the two-stage annealing is increased from 100°C to 200°C and kept warm for 0.5h-20h.

2. A lithium battery copper foil annealing process as claimed in claim 1, characterized in that: The heating rate of the first stage annealing is 10°C / h-100°C / h.

3. A lithium battery copper foil annealing process as claimed in claim 1 or 2, characterized in that: The heating rate of the second-stage annealing is 10°C / h-100°C / h.

4. A lithium battery copper foil annealing process as claimed in claim 1, characterized in that: During the second stage annealing, the oxygen content in the annealing device is ≤2000ppm.

5. A lithium battery copper foil annealing process as claimed in claim 1, characterized in that: The copper foil is wound on the inner sleeve, and through holes are formed on two end surfaces of the inner sleeve.

6. A lithium battery copper foil annealing process as claimed in claim 1, characterized in that: The anti-oxidation treatment parameters are: pH value 2-4, CrO3 0.8 g / L-1.2 g / L, COD 2000 mg / L-10000 mg / L, and anti-oxidation liquid temperature 20°C-40°C.

7. A lithium battery copper foil annealing process as claimed in claim 1, characterized in that: The anti-oxidation treatment is double-sided chrome plating, and the total chrome content is ≤150ppm.