A method for preparing tetragonal zirconium oxide nano-tubular crystals

By mixing the aqueous solution of zirconium nitrate and sodium benzoate with isopropanol, microwave hydrothermal treatment and calcining, a tetragonal phase zirconia nanotube crystal with a unique one-dimensional tubular structure was prepared, which solved the lack of morphological novelty in the prior art. The problem of this achieves excellent performance and wide application in multiple fields.

CN116199259BActive Publication Date: 2024-11-08LUOYANG INST OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310268887.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-11-08
Estimated Expiration
2043-03-20

AI Technical Summary

Technical Problem

The prior art is difficult to prepare zirconia nanotube crystals with novel morphology, which limits their application in piezoelectric ceramics, aerospace and military industry, fuel cells and other fields.

Method used

By mixing the aqueous solution of zirconium nitrate and sodium benzoate and combining it with isopropanol, microwave hydrothermal treatment and calcining in a high-temperature furnace, tetragonal phase zirconia nanotube crystals with a unique one-dimensional tubular structure were prepared.

Benefits of technology

The preparation of crystallized tetragonal phase zirconia nanotube crystals has been achieved, with wide application prospects, simple equipment, easy operation, and easy industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116199259B_ABST
    Figure CN116199259B_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing tetragonal zirconium oxide nano-tubular crystals, wherein a prepared zirconium nitrate solution and a sodium benzoate solution are mixed to obtain a zirconium benzoate precipitation solution as a reaction precursor, the obtained zirconium benzoate precipitation solution is mixed with isopropanol accounting for 20-40% of the total volume of the mixed solution, and then subjected to microwave hydrothermal, filtration, drying, and calcination to obtain tetragonal zirconium oxide nano-tubular crystals. The method of the invention successfully prepares tetragonal zirconium oxide nano-tubular crystals for the first time and has the advantages of simple operation, controllable crystal morphology, and the like, and is easy to realize industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of inorganic non-metallic technical materials, and in particular to a method for preparing tetragonal zirconium oxide nano-tubular crystals. Background Art

[0002] Zirconia is a very important functional material. Due to its excellent performance, it has a wide range of uses in many fields such as aerospace and military industry, piezoelectric ceramics, fuel cells, optical fibers, microwaves, capacitors, photocatalysis, gas sensors, sensors, and medical treatment. It has been one of the research hotspots in recent years.

[0003] As we all know, nanocrystalline materials with special morphology usually have some particularly excellent properties. Therefore, the preparation of zirconia nanotubular crystals with novel morphology is of great significance in both theoretical basic research and practical applications. Summary of the Invention

[0004] In response to the above technical problems, the main purpose of the present invention is to provide a method for preparing tetragonal zirconia nanotubular crystals. The method is simple in process, and the obtained tetragonal zirconia nanotubular crystals have controllable morphology and a unique one-dimensional tubular structure. They have better performance and broader application prospects in the fields of piezoelectric ceramics, aerospace and military industry, fuel cells, optical fibers, microwaves, capacitors, photocatalysis, gas sensors, sensors, and medical treatment.

[0005] To achieve the above object, the present invention provides the following technical solution: a method for preparing tetragonal zirconium oxide nanotubular crystals, specifically comprising the following steps:

[0006] Step (1) dissolving zirconium nitrate in deionized water to form a zirconium nitrate aqueous solution, and adjusting the concentration of the zirconium nitrate in the solution to 0.02 to 0.8 mol / L;

[0007] Step (2) dissolving sodium benzoate in deionized water to form a sodium benzoate aqueous solution, and adjusting the concentration of sodium benzoate in the solution to 0.08 to 1.6 mol / L;

[0008] Step (3) mixing the zirconium nitrate aqueous solution obtained in step (1) and the sodium benzoate aqueous solution obtained in step (2) to obtain a zirconium benzoate precipitate solution as a reaction precursor; the molar ratio of sodium benzoate to zirconium nitrate during mixing is 4:1;

[0009] Step (4) mixing the zirconium benzoate precipitate solution obtained in step (3) with isopropyl alcohol, wherein the isopropyl alcohol accounts for 20% to 40% of the total volume of the mixed solution to obtain a mixture A;

[0010] Step (5) placing the reaction kettle containing the mixture A into a temperature-controlled microwave hydrothermal apparatus for microwave hydrothermal treatment to obtain B, and filtering and drying B to obtain C;

[0011] Step (6) placing the C obtained in step (5) into a high-temperature furnace for calcination at a temperature of 600 to 1000° C. for 2 to 4 hours to finally obtain tetragonal zirconia nanotubular crystals.

[0012] Furthermore, during the microwave hydrothermal treatment, the microwave power is 500-1500W, the microwave time is 1h-5h, and the temperature of the microwave hydrothermal treatment is 120-220°C.

[0013] Furthermore, the purity of the sodium benzoate, zirconium nitrate and isopropyl alcohol is not lower than chemical purity.

[0014] Furthermore, the length of the obtained tetragonal zirconium oxide nano-tubular crystals is about 1.5 to 2 μm, and the thickness of the nano-tube wall is about 20 to 50 nm.

[0015] Compared with the prior art, the present invention has the following advantages:

[0016] The method of the invention can prepare tetragonal zirconium oxide nano-tubular crystals with good crystallization and high purity, has simple equipment, simple operation, easy control of process conditions, and is easy to realize industrial production.

[0017] The tetragonal zirconia nanotubular crystals prepared by the method of the present invention have a unique one-dimensional tubular structure. The length of the zirconia nanotubular crystals is about 1.5 to 2 μm, and the wall thickness of the nanotubes is about 20 to 50 nm. They have broad application prospects in the fields of piezoelectric ceramics, aerospace and military industry, fuel cells, optical fibers, microwaves, capacitors, photocatalysis, gas sensors, sensors, and medical treatment.

[0018] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the following preferred embodiments are specifically cited and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The XRD pattern of the tetragonal zirconium oxide nano-tubular crystals synthesized by the present invention.

[0020] Figure 2 This is a transmission electron microscope (TEM) image of the tetragonal zirconium oxide nanotubular crystals synthesized in the present invention. DETAILED DESCRIPTION

[0021] To further illustrate the technical means and effects adopted by the present invention to achieve the intended purpose, the following, in conjunction with the accompanying drawings and preferred embodiments, describes in detail a method for preparing tetragonal zirconia nanotubular crystals according to the present invention, including its specific implementation method, structure, characteristics, and effects.

[0022] Example 1

[0023] (1) dissolving zirconium nitrate in deionized water to form a zirconium nitrate aqueous solution, and adjusting the concentration of the zirconium nitrate in the solution to 0.02 mol / L;

[0024] (2) dissolving sodium benzoate in deionized water to form a sodium benzoate aqueous solution, and adjusting the concentration of sodium benzoate in the solution to 0.08 mol / L;

[0025] (3) mixing the zirconium nitrate aqueous solution obtained in step (1) and the sodium benzoate aqueous solution obtained in step (2) to obtain a zirconium benzoate precipitation solution; the molar ratio of sodium benzoate to zirconium nitrate during mixing is 4:1;

[0026] (4) mixing the zirconium benzoate precipitate solution obtained in step (3) with isopropyl alcohol, wherein the isopropyl alcohol accounts for 20% of the total volume of the mixed solution, to obtain a mixture A;

[0027] (5) placing the reaction kettle containing the mixture A into a temperature-controlled microwave hydrothermal apparatus for microwave hydrothermal treatment to obtain B, and filtering and drying B to obtain C (the microwave power during the microwave hydrothermal treatment is 500 W, the microwave time is 5 h, and the microwave hydrothermal treatment temperature is 150°C);

[0028] (6) The C obtained in step (5) is placed in a high-temperature furnace for calcination at a temperature of 800° C. and kept warm for 4 hours to finally obtain tetragonal zirconia nanotubular crystals.

[0029] Figure 1 This is the XRD spectrum of the tetragonal zirconia nanotubular crystals prepared in Example 1. It can be seen from the figure that the prepared product is well-crystallized tetragonal zirconia.

[0030] Figure 2 This is a transmission electron micrograph of the tetragonal zirconia nanotubular crystals prepared in Example 1. The image shows that the resulting product has a distinct nanotubular structure. The resulting tetragonal zirconia nanotubular crystals are approximately 1.5 to 2 μm long, with a nanotube diameter of approximately 200 to 300 nm and a nanotube wall thickness of approximately 20 to 40 nm.

[0031] Example 2

[0032] (1) dissolving zirconium nitrate in deionized water to form a zirconium nitrate aqueous solution, and adjusting the concentration of the zirconium nitrate in the solution to 0.8 mol / L;

[0033] (2) dissolving sodium benzoate in deionized water to form a sodium benzoate aqueous solution, and adjusting the concentration of sodium benzoate in the solution to 1.2 mol / L;

[0034] (3) mixing the zirconium nitrate aqueous solution obtained in step (1) and the sodium benzoate aqueous solution obtained in step (2) to obtain a zirconium benzoate precipitation solution; the molar ratio of sodium benzoate to zirconium nitrate during mixing is 4:1;

[0035] (4) mixing the zirconium benzoate precipitate solution obtained in step (3) with isopropyl alcohol, wherein the isopropyl alcohol accounts for 30% of the total volume of the mixed solution, to obtain a mixture A;

[0036] (5) placing the reaction kettle containing the mixture A into a temperature-controlled microwave hydrothermal apparatus for microwave hydrothermal treatment to obtain B, and filtering and drying B to obtain C (the microwave power during the microwave hydrothermal treatment is 1000 W, the microwave time is 3 h, and the microwave hydrothermal treatment temperature is 200°C);

[0037] (6) The C obtained in step (5) is placed in a high-temperature furnace for calcination at a temperature of 900° C. and kept warm for 3 hours to finally obtain tetragonal zirconia nanotubular crystals.

[0038] Example 3

[0039] (1) dissolving zirconium nitrate in deionized water to form a zirconium nitrate aqueous solution, and adjusting the concentration of the zirconium nitrate in the solution to 0.6 mol / L;

[0040] (2) dissolving sodium benzoate in deionized water to form a sodium benzoate aqueous solution, and adjusting the concentration of sodium benzoate in the solution to 0.6 mol / L;

[0041] (3) mixing the zirconium nitrate aqueous solution obtained in step (1) and the sodium benzoate aqueous solution obtained in step (2) to obtain a zirconium benzoate precipitation solution; the molar ratio of sodium benzoate to zirconium nitrate during mixing is 4:1;

[0042] (4) mixing the zirconium benzoate precipitate solution obtained in step (3) with isopropyl alcohol, wherein the isopropyl alcohol accounts for 40% of the total volume of the mixed solution, to obtain a mixture A;

[0043] (5) placing the reaction kettle containing the mixture A into a temperature-controlled microwave hydrothermal apparatus for microwave hydrothermal treatment to obtain B, and filtering and drying B to obtain C (the microwave power during the microwave hydrothermal treatment is 1500 W, the microwave time is 1 h, and the microwave hydrothermal treatment temperature is 220°C);

[0044] (6) The C obtained in step (5) is placed in a high-temperature furnace for calcination at a temperature of 1000° C. and kept warm for 1 hour to finally obtain tetragonal zirconia nanotubular crystals.

[0045] The above description is merely an embodiment of the present invention and does not constitute any form of limitation to the present invention. The present invention may also have other forms of embodiments based on the above structures and functions, which are not listed here one by one. Therefore, any simple modification, equivalent changes, and modifications made to the above embodiments by any person skilled in the art based on the technical essence of the present invention without departing from the scope of the technical solution of the present invention shall still fall within the scope of the technical solution of the present invention.

Claims

1. A method for preparing tetragonal zirconium oxide nano-tubular crystals, characterized in that: The specific steps include: Step (1) dissolving zirconium nitrate in deionized water to form a zirconium nitrate aqueous solution, and adjusting the concentration of zirconium nitrate in the solution to 0.02-0.8 mol / L; Step (2) dissolving sodium benzoate in deionized water to form a sodium benzoate aqueous solution, and adjusting the concentration of sodium benzoate in the solution to 0.08 to 1.6 mol / L; Step (3) mixing the zirconium nitrate aqueous solution obtained in step (1) and the sodium benzoate aqueous solution obtained in step (2) to obtain a zirconium benzoate precipitate solution as a reaction precursor; the molar ratio of sodium benzoate to zirconium nitrate during mixing is 4:1; Step (4) mixing the zirconium benzoate precipitate solution obtained in step (3) with isopropanol, wherein the isopropanol accounts for 20% to 40% of the total volume of the mixed solution, to obtain a mixture A; Step (5) placing the reaction kettle containing the mixture A into a temperature-controlled microwave hydrothermal apparatus for microwave hydrothermal treatment to obtain B, and filtering and drying B to obtain C; Step (6) placing the C obtained in step (5) into a high temperature furnace for calcination at a temperature of 600 to 1000° C. for 2 to 4 hours, and finally obtaining tetragonal zirconium oxide nano-tubular crystals.

2. The method for preparing tetragonal zirconium oxide nano-tubular crystals according to claim 1, characterized in that: During the microwave hydrothermal treatment, the microwave power is 500-1500W, the microwave time is 1h-5h, and the temperature of the microwave hydrothermal treatment is 120-220°C.

3. The method for preparing tetragonal zirconium oxide nano-tubular crystals according to claim 1, characterized in that: The purity of the sodium benzoate, zirconium nitrate and isopropanol is not lower than chemical purity.

4. The method for preparing tetragonal zirconium oxide nano-tubular crystals according to claim 1, characterized in that: The length of the obtained tetragonal zirconium oxide nano-tube crystals is 1.5-2 μm, and the wall thickness of the nano-tube is 20-50 nm.