Halogen-free flame-retardant material reinforced composite polyethylene and preparation method thereof
By modifying the crosslinking of polyethylene and polyvinyl alcohol and the surface modification of inorganic particles, composite polyethylene with high flame retardant performance is prepared, which solves the problems of poor flame retardant performance and degraded mechanical properties of polyethylene, and achieves good Mechanical properties and environmental protection.
Patent Information
- Application Number
- CN202411020118.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-08
AI Technical Summary
Polyethylene has poor performance in flame retardant performance. Traditional halogen flame retardants will produce toxic gases and smoke, and the inorganic flame retardant fillers have poor compatibility with polyethylene, resulting in a decrease in the mechanical properties of composite materials.
By modifying the crosslinking of low-density polyethylene and polyvinyl alcohol and KH-560, an epoxy-modified polyethylene elastomer is formed, and surface modification and amino modification are carried out using a combination of parallol, magnesium oxide and zinc oxide. Prepare flame retardant enhancers, combined with stearic acid, to improve the crosslinking degree and interface compatibility of polyethylene.
It significantly improves the tensile properties, impact resistance, bending properties and flame retardant properties of composite polyethylene, forming a tight interface combination to inhibit flame spread, and is suitable for environmental protection requirements.
Smart Images

Figure BDA0004966968080000041 
Figure BDA0004966968080000042 
Figure BDA0004966968080000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame-retardant polyethylene processing, and in particular to a composite polyethylene reinforced with a halogen-free flame-retardant material and a preparation method thereof. Background Art
[0002] Polyethylene is a thermoplastic resin obtained by polymerization of ethylene monomers. It has excellent low-temperature resistance and chemical stability. Because the polymer molecules are connected by carbon-carbon single bonds, it can withstand the corrosion of most acids and alkalis. With the increasing attention paid to environmental protection and safety in modern society, polymer materials, especially polyethylene and its composite materials, are increasingly used in daily life, industrial production and special fields. However, polyethylene itself has poor performance in flame retardancy and is flammable and difficult to self-extinguish. Therefore, polyethylene needs to be modified to improve its flame retardancy. Composite materials are a way to obtain excellent performance by combining different types of materials.
[0003] The traditional method of polyethylene flame retardant is mainly achieved by adding halogen flame retardants. Although this type of flame retardant has high flame retardant efficiency, it will produce a large amount of toxic gases and smoke during the combustion process, causing secondary pollution to the environment. It does not meet the environmental protection requirements of modern society. In recent years, the research on halogen-free flame retardants has gradually received attention.
[0004] In the process of enhancing the flame retardant properties of polyethylene in the prior art, the composite material can enhance the flame retardant properties of the material by introducing various flame retardant fillers. At present, commonly used flame retardant fillers include inorganic fillers such as alumina, silicates, and phosphorus-containing compounds. However, polyethylene is a non-polar material, and its molecular chain is mainly composed of CH bonds, showing a low surface energy, and inorganic flame retardant fillers, such as metal oxides, silicates, etc., often have strong polarity. Due to the difference in surface polarity between the two, the affinity and compatibility between the filler and the polyethylene matrix are poor, the inorganic filler is easy to agglomerate in the polyethylene material, and the composite polyethylene material has a weak interface, which leads to a decrease in the mechanical properties of the composite polyethylene. In addition, when a single flame retardant inorganic filler improves the flame retardant properties of polyethylene, the improvement of the flame retardant properties of the polyethylene material is limited.
[0005] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention
[0006] The object of the present invention is to provide a halogen-free flame retardant material reinforced composite polyethylene and a preparation method thereof, so as to solve the technical defects proposed by the background technology.
[0007] The object of the present invention can be achieved by the following technical scheme: A composite polyethylene reinforced with a halogen-free flame retardant material, comprising the following components in parts by weight: 85-100 parts of a polyethylene elastomer, 10-20 parts of a flame retardant reinforcing agent, and 3-5 parts of an auxiliary additive;
[0008] The preparation method of the polyethylene elastomer is as follows: adding modified low-density polyethylene, modified polyvinyl alcohol and N,N-dimethylformamide into a reactor and stirring, raising the temperature of the reactor to 85-95° C., stirring and keeping warm until the system is dissolved, adding KH-560 into the reactor and stirring for 15-20 minutes, adding sodium hydroxide solution into the reactor, keeping warm for reaction for 3-5 hours, and post-treating to obtain the polyethylene elastomer.
[0009] The synthetic reaction principle of polyethylene elastomer is:
[0010] The siloxane bonds on the modified low-density polyethylene, modified polyvinyl alcohol and KH-560 are broken and reorganized in an alkaline high-temperature environment to form a polysiloxane structure, which promotes the cross-linking of polyethylene and polyvinyl alcohol molecular chains and introduces epoxy groups into the molecular chains to prepare a polyethylene elastomer cross-linked with highly cross-linked epoxy-modified polyethylene and polyvinyl alcohol molecular chains.
[0011] Furthermore, the auxiliary additives are composed of a plasticizer, an antioxidant, a lubricant and a light stabilizer in a weight ratio of 2:1:1:1, the plasticizer is a phthalate, the antioxidant is one or more of antioxidant 1010, antioxidant 1076, and antioxidant 168, the lubricant is a higher fatty acid metal salt, the light stabilizer is an ultraviolet absorber, and the modified low-density polyethylene, modified polyvinyl alcohol, N,N-dimethylformamide, KH-560 and sodium hydroxide solution are The dosage ratio is 8-10g:4-5g:80-90mL:2-3g:10-20mL, the concentration of the sodium hydroxide solution is 2-3mol / L, and the post-treatment includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, and purified water is first added to the reactor under stirring, stirred for 20-30min, filtered, the filter cake is washed with purified water 3 times and then dried, and the filter cake is transferred to a drying oven at a temperature of 70-80°C, and dried to constant weight to obtain a polyethylene elastomer.
[0012] Furthermore, the preparation method of the modified low-density polyethylene is: low-density polyethylene, vinyl triethoxysilane and an initiator are uniformly mixed and then added into a twin-screw extruder, melt-extruded, and air-cooled to solidify to obtain the modified low-density polyethylene.
[0013] The synthetic reaction principle of modified polyethylene is:
[0014] Under the conditions of initiator and high temperature, the vinyl group in alkenyltriethoxysilane chemically reacts with the low-density polyethylene molecular chain and is connected together by covalent bonds to form a three-dimensional network structure to prepare modified low-density polyethylene.
[0015] Furthermore, the weight ratio of the low-density polyethylene, vinyl triethoxysilane and initiator is 20:3-4:0.2-0.3, the initiator is dicumyl peroxide, and the temperatures of the six temperature zones of the twin-screw extruder from the feed end toward the head are 280°C, 290°C, 290°C, 290°C, 290°C and 300°C, respectively, and the spindle speed is 15-25r / min.
[0016] Furthermore, the modified polyvinyl alcohol is obtained by processing the following steps:
[0017] A1. Add polyvinyl alcohol and deionized water into a reactor and stir until the system is dissolved. The temperature of the reactor is raised to 90-95° C., phosphoric acid solution is added dropwise into the reactor, and the reaction is carried out by heat preservation for 2-3 hours. Urea solution is added into the reactor, and the reaction is carried out by heat preservation for 2-3 hours. Post-treatment is performed to obtain a modified polyvinyl alcohol precursor.
[0018] The synthetic reaction formula of modified polyvinyl alcohol precursor is:
[0019]
[0020] The synthetic reaction principle of modified polyvinyl alcohol precursor is:
[0021] The hydrogen ions of phosphoric acid in the phosphoric acid solution react with the hydroxyl groups of polyvinyl alcohol to form ester bonds, thereby modifying the phosphoric acid groups on the polyvinyl alcohol molecular chains. The phosphoric acid groups on the molecular chains then react with urea to generate ammonium phosphate salts, thereby obtaining modified polyvinyl alcohol precursors.
[0022] A2. Add modified polyvinyl alcohol precursor and tetrahydrofuran into a nitrogen-protected reactor and stir. Raise the temperature of the reactor to 50-60° C., add isocyanatepropyltriethoxysilane into the reactor, keep the reaction temperature for 4-6 hours, and perform post-treatment to obtain modified polyvinyl alcohol.
[0023] The synthetic reaction formula of modified polyvinyl alcohol is:
[0024]
[0025] The synthetic reaction principle of modified polyvinyl alcohol is:
[0026] The modified polyvinyl alcohol precursor contains a large number of active hydroxyl groups. Under high temperature conditions, the isocyanate groups on isocyanatepropyltriethoxysilane can undergo condensation reaction with the active oxygen-containing functional groups on the modified polyvinyl alcohol precursor chain segments, forming triethoxysilane modifications on the molecular chain segments of the modified polyvinyl alcohol precursor to prepare modified polyvinyl alcohol.
[0027] Furthermore, in step A1, the amount ratio of the polyvinyl alcohol, deionized water, phosphoric acid solution and urea solution is 5g:50mL:10mL:5mL, the mass fraction of the phosphoric acid is 20-25%, and the urea solution is composed of urea and deionized water in an amount ratio of 2g:5mL. The post-treatment operation includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, the film is cast, placed in a saturated sodium sulfate solution, solidified, washed with deionized water 5-8 times and then drained, transferred to a drying oven at a temperature of 60-70°C, and dried to constant weight to obtain a modified polyvinyl alcohol precursor; in step A2, the amount ratio of the modified polyvinyl alcohol precursor, tetrahydrofuran and isocyanatepropyltriethoxysilane is 3g:20mL:1g, and the post-treatment operation includes: after the reaction is completed, the reactor is kept warm at 50-60°C, and tetrahydrofuran is evaporated under reduced pressure to obtain modified polyvinyl alcohol.
[0028] Furthermore, the flame retardant reinforcing agent is obtained by processing the following steps:
[0029] B1, palygorskite, magnesium oxide and zinc oxide are mixed, crushed by a pulverizer, and passed through a 100-mesh sieve to obtain a mixed powder;
[0030] B2, adding the mixed powder, anhydrous ethanol and KH-550 into a reactor and stirring, raising the temperature of the reactor to 50-60°C, adding sodium hydroxide solution into the reactor, keeping the temperature for 3-5h, and post-treating to obtain an activated mixed powder;
[0031] The synthetic reaction formula of activated mixed powder is:
[0032]
[0033] Where: It is palygorskite, magnesium oxide or zinc oxide particles.
[0034] The synthetic reaction principle of activated mixed powder is:
[0035] In an alkaline environment, the siloxane bonds on the KH-550 molecules are broken, forming silanol groups that react with the surface of the mixed powder particles, forming an amino-modified polysiloxane coating on the outside of the particles, thereby increasing the reactivity of the inorganic particles.
[0036] B3, adding 6-chloro-2,4-amino-1,3,5-triazine, N-methylpyrrolidone solution and activated mixed powder into a reactor and stirring, raising the temperature of the reactor to 100-110°C, keeping the temperature for reaction for 10-12h, and post-treating to obtain a modified mixed powder;
[0037] The synthetic reaction formula of the modified mixed powder is:
[0038]
[0039] The synthetic reaction principle of modified mixed powder is:
[0040] Under high temperature, the halogen on 6-chloro-2,4-amino-1,3,5-triazine undergoes a substitution reaction with the amino group modified on the outside of the activated powder particles, forming a large amount of nitrogen and amino group modifications on the outside of the particles to prepare a modified mixed powder.
[0041] B4. Evenly mix the modified mixed powder and stearic acid to obtain a flame retardant enhancer.
[0042] Further, in step B1, the weight ratio of palygorskite, magnesium oxide and zinc oxide is 3:1:1; in step B2, the amount ratio of the mixed powder, anhydrous ethanol, KH-550 and sodium hydroxide solution is 2g:15mL:1g:3mL, and the concentration of the sodium hydroxide solution is 1-2mol / L, and the post-treatment includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, the filter cake is washed with 65wt% ethanol aqueous solution until neutral and then dried, and the filter cake is transferred to a drying oven at a temperature of 65-75°C and dried to constant weight to obtain an activated mixed powder; in step B3, the 6- The dosage ratio of chloro-2,4-amino-1,3,5-triazine, N-methylpyrrolidone solution and activated mixed powder is 2g:20mL:5g, the N-methylpyrrolidone solution is composed of N-methylpyrrolidone and 15-20wt% sodium bicarbonate solution in a volume ratio of 3:2, and the post-treatment comprises: after the reaction is completed, the temperature of the reactor is lowered to room temperature, suction filtration is performed, the filter cake is washed with purified water until it is neutral and then dried, the filter cake is transferred to a drying oven at a temperature of 65-75°C, and dried to constant weight to obtain a modified mixed powder; in step B4, the weight ratio of the modified mixed powder to stearic acid is 5:1-2.
[0043] A method for preparing composite polyethylene reinforced by a halogen-free flame retardant material comprises the following steps: uniformly mixing a polyethylene elastomer, a flame retardant reinforcing agent and auxiliary additives, adding the mixture to a twin-screw extruder, melt-extruding the mixture into a molding die, cooling and solidifying the mixture, and preparing the composite polyethylene.
[0044] Furthermore, the temperatures of the six temperature zones of the twin-screw extruder from the feed end toward the die are 290°C, 300°C, 300°C, 300°C, 300°C and 310°C respectively, and the main shaft speed is 10-16r / min.
[0045] The present invention has the following beneficial effects:
[0046] 1. The composite polyethylene of the present invention is prepared by using low-density polyethylene and polyvinyl alcohol as raw materials, modifying the low-density polyethylene and polyvinyl alcohol respectively, and then coordinating with KH-560 to prepare a polyethylene elastomer containing epoxy-modified highly cross-linked polyethylene and polyvinyl alcohol cross-linked polyethylene, combining palygorskite, magnesium oxide and zinc oxide to form a mixed powder, then surface modifying the mixed powder to prepare a modified mixed powder, and then mixing the modified mixed powder with stearic acid to prepare a flame retardant enhancer; the flame retardant enhancer and the polyethylene elastomer are melt-blended, and the flame retardant enhancer is used to enhance the flame retardancy of the polyethylene elastomer, while improving the cross-linking degree of the composite polyethylene, so that the composite polyethylene has good tensile properties, impact resistance, bending properties and excellent flame retardant properties.
[0047] 2. The composite polyethylene of the present invention is prepared by modifying polyethylene and polyvinyl alcohol respectively, and then compounding the modified polyethylene, modified polyvinyl alcohol and KH-560 to form a polyethylene elastomer bonded with polysiloxane and cross-linked polyethylene with modified polyvinyl alcohol molecular chains, and a highly cross-linked polyethylene elastomer, so that the polyethylene material has good performance, impact resistance and bending properties; the ammonium phosphate salt modified on the molecular chain segment of the modified polyvinyl alcohol decomposes at high temperature to produce phosphoric acid and other phosphorus-containing compounds, which absorb heat during combustion, reduce the material temperature, delay combustion, and improve the flame retardant properties of the material. Appropriate ammonium phosphate modification may increase the rigidity and strength of the polyvinyl alcohol molecular chain and enhance the interaction between the polyvinyl alcohol molecular chains, thereby enhancing the tensile properties of the polyethylene elastomer, and helping the composite polyethylene to disperse and absorb energy when impacted, thereby improving the impact resistance.
[0048] 3. The composite polyethylene of the present invention is prepared by selecting palygorskite, magnesium oxide and zinc oxide as inorganic materials, crushing them, coating and modifying them, modifying the amino groups on their surfaces, and then reacting with 6-chloro-2,4-amino-1,3,5-triazine under high temperature to form a large amount of nitrogen and amino groups on the outside of the particles to prepare a modified mixed powder, and combining stearic acid with the modified mixed powder to prepare a flame retardant enhancer; by coating and modifying the inorganic particles, the inorganic particles can form a tighter interface when composited with the polyethylene elastomer, thereby improving the tensile strength of the material, and under the action of high temperature, the amino groups on the outside of the particles can be used as active groups to condense with the epoxy groups on the modified polyethylene elastomer, and the palygorskite, magnesium oxide and zinc oxide can form a flame retardant enhancer, thereby improving the tensile strength of the material, and under the action of high temperature, the amino groups on the outside of the particles can be used as active groups to condense with the epoxy groups on the modified polyethylene elastomer, and the palygorskite, magnesium oxide and zinc oxide can form a flame retardant enhancer, thereby improving the tensile strength of the material, and Magnesium chloride and zinc oxide themselves have certain toughness and strength. When these inorganic particles are evenly dispersed in the polyethylene matrix, they can enhance the toughness and strength of the matrix. When impacted, the inorganic particles can serve as stress concentration points to disperse and absorb impact energy, thereby improving the impact resistance of the material. The modified mixed powder, stearic acid and ammonium phosphate in the polyethylene elastomer cooperate with each other to form a synergistic flame retardant mechanism in the composite polyethylene, inhibiting the spread of flames and the burning rate, and significantly improving the flame retardant properties of the composite polyethylene. In addition to cooperating with the modified mixed powder to improve the flame retardant properties of the material, stearic acid can also improve the flowability and dispersibility of polyethylene, making polyethylene easier to process and form, and using it as a crystal nucleus to promote polyethylene crystallization, further improving the mechanical properties of the composite polyethylene. DETAILED DESCRIPTION
[0049] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0050] Example 1
[0051] This embodiment provides a method for preparing a composite polyethylene reinforced with a halogen-free flame retardant material, comprising the following steps:
[0052] S1. Preparation of modified polyethylene
[0053] Weigh: 2kg of low-density polyethylene, 300g of vinyltriethoxysilane, and 20g of diisopropylbenzene peroxide, mix well, and add to a twin-screw extruder. The temperatures of the six temperature zones of the twin-screw extruder from the feed end to the die are 280°C, 290°C, 290°C, 290°C, 290°C and 300°C, respectively. The spindle speed is 15r / min. After melt extrusion through the twin-screw extruder, the product is air-cooled and solidified to obtain modified low-density polyethylene.
[0054] S2. Preparation of modified polyvinyl alcohol
[0055] Urea and deionized water were mixed evenly at a ratio of 2 g:5 mL to obtain a urea solution for later use;
[0056] Weigh: 500g of polyvinyl alcohol and 5L of deionized water are added to a reactor and stirred until the system is dissolved. The temperature of the reactor is raised to 90°C. 1L of 20wt% phosphoric acid solution is added dropwise to the reactor and the reaction is kept warm for 2h. 500mL of urea solution is added to the reactor and the reaction is kept warm for 2h. After the reaction is completed, the temperature of the reactor is lowered to room temperature, and a film is cast and placed in a saturated sodium sulfate solution for solidification. The film is washed 5 times with deionized water and then drained. The film is transferred to a drying oven at 60°C and dried to constant weight to obtain a modified polyvinyl alcohol precursor.
[0057] Weigh: 600 g of modified polyvinyl alcohol precursor and 4 L of tetrahydrofuran are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 50°C. 200 g of isocyanatepropyltriethoxysilane is added to the reactor and the reaction is kept warm for 4 hours. After the reaction is completed, the reactor is kept warm at 50°C, and tetrahydrofuran is evaporated under reduced pressure to obtain modified polyvinyl alcohol.
[0058] S3. Preparation of polyethylene elastomer
[0059] Weigh: 800g of modified low-density polyethylene, 400g of modified polyvinyl alcohol and 8L of N,N-dimethylformamide, add to the reactor and stir, raise the temperature of the reactor to 85°C, keep warm and stir until the system is dissolved, add 200g of KH-560 to the reactor, stir for 15min, add 1L of 2mol / L sodium hydroxide solution to the reactor, keep warm and react for 3h, after the reaction is completed, lower the temperature of the reactor to room temperature, add 20L of purified water to the reactor while stirring, stir for 20min, filter, wash the filter cake with purified water 3 times and then dry, transfer the filter cake to a drying oven at 70°C, dry to constant weight, and obtain a polyethylene elastomer.
[0060] S4. Preparation of flame retardant reinforcing agent
[0061] The palygorskite, magnesium oxide and zinc oxide were mixed in a weight ratio of 3:1:1, crushed by a pulverizer, and passed through a 100-mesh sieve to obtain a mixed powder;
[0062] Weigh: 200g of mixed powder, 1.5L of anhydrous ethanol and 100g of KH-550, add them into a reactor and stir, raise the temperature of the reactor to 50°C, add 300mL of 1mol / L sodium hydroxide solution into the reactor, and keep warm for 3h. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, wash the filter cake with 65wt% ethanol aqueous solution until it is neutral and then dry, transfer the filter cake to a drying oven at a temperature of 65°C, and dry it to constant weight to obtain an activated mixed powder;
[0063] N-methylpyrrolidone and 15 wt % sodium bicarbonate solution were mixed uniformly in a volume ratio of 3:2 to obtain an N-methylpyrrolidone solution for later use;
[0064] Weigh: 200 g of 6-chloro-2,4-amino-1,3,5-triazine, 2 L of N-methylpyrrolidone solution and 500 g of activated mixed powder are added to a reactor and stirred. The temperature of the reactor is raised to 100° C. and the reaction is kept warm for 10 hours. After the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, and the filter cake is washed with purified water until it is neutral and then dried. The filter cake is transferred to a drying oven at a temperature of 65° C. and dried to constant weight to obtain a modified mixed powder;
[0065] The modified mixed powder and stearic acid are uniformly mixed in a weight ratio of 5:1 to obtain a flame retardant enhancer.
[0066] S5. Preparation of composite polyethylene
[0067] Dibutyl phthalate, antioxidant 1010, sodium stearate and ultraviolet absorber UV-0 are uniformly mixed in a weight ratio of 2:1:1:1 to obtain an auxiliary additive for standby use;
[0068] Weigh by weight: 85 parts of polyethylene elastomer, 10 parts of flame retardant reinforcing agent and 3 parts of auxiliary additives, mix them evenly, and add them into a twin-screw extruder. The temperatures of the 6 temperature sections of the twin-screw extruder from the feed end to the head are 290°C, 300°C, 300°C, 300°C, 300°C and 310°C respectively, the main shaft speed is 10r / min, melt extruded into a molding mold, cooled and solidified, to prepare a composite polyethylene.
[0069] Example 2
[0070] This embodiment provides a method for preparing a composite polyethylene reinforced with a halogen-free flame retardant material, comprising the following steps:
[0071] S1. Preparation of modified polyethylene
[0072] Weigh: 2kg of low-density polyethylene, 350g of vinyltriethoxysilane, and 25g of diisopropylbenzene peroxide, mix well, and add to a twin-screw extruder. The temperatures of the six temperature zones of the twin-screw extruder from the feed end to the die are 280°C, 290°C, 290°C, 290°C, 290°C and 300°C, respectively. The spindle speed is 20r / min. After melt extrusion through the twin-screw extruder, the product is air-cooled and solidified to obtain modified low-density polyethylene.
[0073] S2. Preparation of modified polyvinyl alcohol
[0074] Urea and deionized water were mixed evenly at a ratio of 2 g:5 mL to obtain a urea solution for later use;
[0075] Weigh: 500g of polyvinyl alcohol and 5L of deionized water are added to a reactor and stirred until the system is dissolved. The temperature of the reactor is raised to 93°C. 1L of 23wt% phosphoric acid solution is added dropwise to the reactor and the reaction is kept warm for 2.5h. 500mL of urea solution is added to the reactor and the reaction is kept warm for 2.5h. After the reaction is completed, the temperature of the reactor is lowered to room temperature, and a film is cast and placed in a saturated sodium sulfate solution for solidification. The film is washed 6 times with deionized water and then drained. The film is transferred to a drying oven at a temperature of 65°C and dried to constant weight to obtain a modified polyvinyl alcohol precursor.
[0076] Weigh: 600 g of modified polyvinyl alcohol precursor and 4 L of tetrahydrofuran are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 55°C. 200 g of isocyanatepropyltriethoxysilane is added to the reactor and the reaction is kept warm for 5 hours. After the reaction is completed, the reactor is kept warm at 55°C, and tetrahydrofuran is evaporated under reduced pressure to obtain modified polyvinyl alcohol.
[0077] S3. Preparation of polyethylene elastomer
[0078] Weigh: 900g of modified low-density polyethylene, 450g of modified polyvinyl alcohol and 8.5L of N,N-dimethylformamide, add to the reactor and stir, raise the temperature of the reactor to 90°C, keep warm and stir until the system is dissolved, add 250g of KH-560 to the reactor, stir for 17min, add 1.5L of 2.5mol / L sodium hydroxide solution to the reactor, keep warm and react for 4h, after the reaction is completed, lower the temperature of the reactor to room temperature, add 20L of purified water to the reactor while stirring, stir for 25min, filter, wash the filter cake with purified water 3 times and then dry, transfer the filter cake to a drying oven at 75°C, dry to constant weight, and obtain a polyethylene elastomer.
[0079] S4. Preparation of flame retardant reinforcing agent
[0080] The palygorskite, magnesium oxide and zinc oxide were mixed in a weight ratio of 3:1:1, crushed by a pulverizer, and passed through a 100-mesh sieve to obtain a mixed powder;
[0081] Weigh: 200g of mixed powder, 1.5L of anhydrous ethanol and 100g of KH-550, add them into a reactor and stir, raise the temperature of the reactor to 55°C, add 300mL of 1.5mol / L sodium hydroxide solution into the reactor, and keep the reaction for 4h. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, wash the filter cake with 65wt% ethanol aqueous solution until it is neutral and then dry, transfer the filter cake to a drying oven at 70°C, and dry it to constant weight to obtain an activated mixed powder;
[0082] N-methylpyrrolidone and 17 wt % sodium bicarbonate solution were mixed uniformly in a volume ratio of 3:2 to obtain an N-methylpyrrolidone solution for later use;
[0083] Weigh: 200 g of 6-chloro-2,4-amino-1,3,5-triazine, 2 L of N-methylpyrrolidone solution and 500 g of activated mixed powder, add them into a reactor and stir, raise the temperature of the reactor to 105°C, and keep the reaction for 11 hours. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, wash the filter cake with purified water until it is neutral, and then drain, transfer the filter cake to a drying oven at a temperature of 70°C, and dry to constant weight to obtain a modified mixed powder;
[0084] The modified mixed powder and stearic acid are uniformly mixed in a weight ratio of 5:1.5 to obtain a flame retardant enhancer.
[0085] S5. Preparation of composite polyethylene
[0086] Diethyl phthalate, antioxidant 1076, barium stearate and ultraviolet absorber UV-9 are uniformly mixed in a weight ratio of 2:1:1:1 to obtain an auxiliary additive for standby use;
[0087] Weigh by weight: 93 parts of polyethylene elastomer, 15 parts of flame retardant reinforcing agent and 4 parts of auxiliary additives, mix them evenly, and add them into a twin-screw extruder. The temperatures of the six temperature sections of the twin-screw extruder from the feed end to the head are 290°C, 300°C, 300°C, 300°C, 300°C and 310°C, respectively. The main shaft speed is 13r / min. Melt extrude into a molding mold, cool and solidify, and prepare composite polyethylene.
[0088] Example 3
[0089] This embodiment provides a method for preparing a composite polyethylene reinforced with a halogen-free flame retardant material, comprising the following steps:
[0090] S1. Preparation of modified polyethylene
[0091] Weigh: 2kg of low-density polyethylene, 400g of vinyltriethoxysilane, and 30g of diisopropylbenzene peroxide, mix well, and add to a twin-screw extruder. The temperatures of the six temperature zones of the twin-screw extruder from the feed end to the die are 280°C, 290°C, 290°C, 290°C, 290°C and 300°C, respectively. The spindle speed is 25r / min. After melt extrusion through the twin-screw extruder, the product is air-cooled and solidified to obtain modified low-density polyethylene.
[0092] S2. Preparation of modified polyvinyl alcohol
[0093] Urea and deionized water were mixed evenly at a ratio of 2 g:5 mL to obtain a urea solution for later use;
[0094] Weigh: 500g of polyvinyl alcohol and 5L of deionized water are added to a reactor and stirred until the system is dissolved. The temperature of the reactor is raised to 95°C. 1L of 25wt% phosphoric acid solution is added dropwise to the reactor and the reaction is kept warm for 3h. 500mL of urea solution is added to the reactor and the reaction is kept warm for 3h. After the reaction is completed, the temperature of the reactor is lowered to room temperature, cast into a film, placed in a saturated sodium sulfate solution, solidified, washed 8 times with deionized water and drained, transferred to a drying oven at a temperature of 70°C, and dried to constant weight to obtain a modified polyvinyl alcohol precursor;
[0095] Weigh: 600 g of modified polyvinyl alcohol precursor and 4 L of tetrahydrofuran are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 60°C. 200 g of isocyanatepropyltriethoxysilane is added to the reactor and the reaction is kept warm for 6 hours. After the reaction is completed, the reactor is kept warm at 60°C, and tetrahydrofuran is evaporated under reduced pressure to obtain modified polyvinyl alcohol.
[0096] S3. Preparation of polyethylene elastomer
[0097] Weigh: 1000g of modified low-density polyethylene, 500g of modified polyvinyl alcohol and 9L of N,N-dimethylformamide, add to the reactor and stir, raise the temperature of the reactor to 95°C, keep warm and stir until the system is dissolved, add 300g of KH-560 to the reactor, stir for 20min, add 2L of 3mol / L sodium hydroxide solution to the reactor, keep warm and react for 5h, after the reaction is completed, lower the temperature of the reactor to room temperature, add 20L of purified water to the reactor while stirring, stir for 30min, filter, wash the filter cake with purified water 3 times and then dry, transfer the filter cake to a drying oven at 80°C, dry to constant weight, and obtain a polyethylene elastomer.
[0098] S4. Preparation of flame retardant reinforcing agent
[0099] The palygorskite, magnesium oxide and zinc oxide were mixed in a weight ratio of 3:1:1, crushed by a pulverizer, and passed through a 100-mesh sieve to obtain a mixed powder;
[0100] Weigh: 200g of mixed powder, 1.5L of anhydrous ethanol and 100g of KH-550, add them into a reactor and stir, raise the temperature of the reactor to 60°C, add 300mL of 2mol / L sodium hydroxide solution into the reactor, and keep the reaction for 5h. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, wash the filter cake with 65wt% ethanol aqueous solution until it is neutral and then dry it, transfer the filter cake to a drying oven at 75°C, and dry it to constant weight to obtain an activated mixed powder;
[0101] N-methylpyrrolidone and 20 wt % sodium bicarbonate solution were mixed uniformly in a volume ratio of 3:2 to obtain an N-methylpyrrolidone solution for later use;
[0102] Weigh: 200 g of 6-chloro-2,4-amino-1,3,5-triazine, 2 L of N-methylpyrrolidone solution and 500 g of activated mixed powder, add them into a reactor and stir, raise the temperature of the reactor to 110°C, and keep the reaction for 12 hours. After the reaction is completed, lower the temperature of the reactor to room temperature, filter, wash the filter cake with purified water until it is neutral, and then drain, transfer the filter cake to a drying oven at a temperature of 75°C, and dry to constant weight to obtain a modified mixed powder;
[0103] The modified mixed powder and stearic acid are uniformly mixed in a weight ratio of 5:2 to obtain a flame retardant enhancer.
[0104] S5. Preparation of composite polyethylene
[0105] Dipropyl phthalate, antioxidant 168, calcium stearate and ultraviolet absorber UV-1084 are uniformly mixed in a weight ratio of 2:1:1:1 to obtain an auxiliary additive for standby use;
[0106] Weigh by weight: 100 parts of polyethylene elastomer, 20 parts of flame retardant reinforcing agent and 5 parts of auxiliary additives, mix them evenly, and add them into a twin-screw extruder. The temperatures of the six temperature sections of the twin-screw extruder from the feed end to the die are 290°C, 300°C, 300°C, 300°C, 300°C and 310°C, respectively. The spindle speed is 16 r / min. The mixture is melt-extruded into a molding die, cooled and solidified, and a composite polyethylene is prepared.
[0107] Comparative Example 1
[0108] The difference between this comparative example and Example 3 is that step S1 is omitted, and the low-density polyethylene and the modified polyvinyl alcohol precursor in step S1 are blended to prepare a polyethylene elastomer.
[0109] Comparative Example 2
[0110] The difference between this comparative example and Example 3 is that in step S2, polyvinyl alcohol is used instead of modified polyvinyl alcohol precursor to prepare modified polyethylene.
[0111] Comparative Example 3
[0112] The difference between this comparative example and Example 3 is that in step S3, KH-560 is not added.
[0113] Comparative Example 4
[0114] The difference between this comparative example and Example 3 is that in step S4, the modified mixed powder is replaced by mixed powder to participate in the preparation of the flame retardant mixed powder.
[0115] Comparative Example 5
[0116] The difference between this comparative example and Example 3 is that in step S4, the modified mixed powder is used as a flame retardant reinforcing agent.
[0117] Performance Test:
[0118] The impact resistance, tensile properties and flame retardant properties of the composite polyethylene prepared in Examples 1-3 and Comparative Examples 1-5 were tested. The tensile strength of the sample was determined according to the standard GB / T 1040.1-2018 "Determination of Tensile Properties of Plastics Part 1: General Principles" for tensile properties; the impact resistance was determined according to the standard GB / T1043.2-2018 "Determination of Impact Properties of Simply Supported Beams of Plastics Part 2: Instrumented Impact Test" for simply supported beam notched impact strength of the sample; the bending performance was determined according to the standard GB / T9341-2008 "Determination of Bending Properties of Plastics" for fracture bending stress and fracture bending strain of the sample; the flame retardant performance was determined according to the standard GB / T2408-2021 "Determination of Combustion Performance of Plastics - Horizontal and Vertical Methods" for vertical combustion performance grade of the sample. The specific test results are shown in Table 1 below.
[0119] Table 1-Performance test data of the sample
[0120]
[0121] Data Analysis:
[0122] Comparative analysis of the data in Table 1 shows that the tensile strength of the composite polyethylene sample prepared by the present invention reaches 22.8 MPa, and the simply supported beam notched impact strength reaches 9.1 kJ / m 2The bending modulus reaches 1195MPa, the bending strain at break reaches 36.2%, the vertical combustion performance grade reaches V-0, and the performance test data are all better than the control example, indicating that the present invention prepares a flame retardant enhancer to enhance the flame retardant modification of the highly cross-linked polyethylene modified with epoxy group and the polyethylene elastomer cross-linked with polyvinyl alcohol, which not only effectively improves the tensile properties, impact resistance and bending properties of the composite polyethylene, but also improves the flame retardant properties of the composite polyethylene.
[0123] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
[0124] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0125] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A composite polyethylene reinforced with a halogen-free flame retardant material, characterized in that: The invention comprises the following components in parts by weight: 85-100 parts of polyethylene elastomer, 10-20 parts of flame retardant reinforcing agent and 3-5 parts of auxiliary additives; The preparation method of the polyethylene elastomer is as follows: adding modified low-density polyethylene, modified polyvinyl alcohol and N,N-dimethylformamide into a reactor and stirring, raising the temperature of the reactor to 85-95° C., stirring and keeping warm until the system is dissolved, adding KH-560 into the reactor and stirring for 15-20 minutes, adding sodium hydroxide solution into the reactor, keeping warm for reaction for 3-5 hours, and post-treating to obtain the polyethylene elastomer.
2. The halogen-free flame retardant material reinforced composite polyethylene according to claim 1, characterized in that: The auxiliary additives are composed of a plasticizer, an antioxidant, a lubricant and a light stabilizer in a weight ratio of 2:1:1:1, the plasticizer is a phthalate, the antioxidant is one or more of antioxidant 1010, antioxidant 1076, and antioxidant 168, the lubricant is a higher fatty acid metal salt, the light stabilizer is an ultraviolet absorber, and the amount of the modified low-density polyethylene, modified polyvinyl alcohol, N,N-dimethylformamide, KH-560 and sodium hydroxide solution is The ratio is 8-10g:4-5g:80-90mL:2-3g:10-20mL, the concentration of the sodium hydroxide solution is 2-3mol / L, and the post-treatment includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, and purified water is first added to the reactor under stirring, stirred for 20-30min, filtered, the filter cake is washed with purified water 3 times and then dried, and the filter cake is transferred to a drying oven with a temperature of 70-80°C, and dried to constant weight to obtain a polyethylene elastomer.
3. The halogen-free flame retardant material reinforced composite polyethylene according to claim 1, characterized in that: The preparation method of the modified low-density polyethylene is as follows: low-density polyethylene, vinyl triethoxysilane and an initiator are uniformly mixed and then added into a twin-screw extruder, melt-extruded, and air-cooled and solidified to obtain the modified low-density polyethylene.
4. The halogen-free flame retardant material reinforced composite polyethylene according to claim 3, characterized in that: The weight ratio of the low-density polyethylene, vinyl triethoxysilane and initiator is 20:3-4:0.2-0.3, the initiator is dicumyl peroxide, the temperatures of the six temperature zones of the twin-screw extruder from the feed end toward the die are 280°C, 290°C, 290°C, 290°C, 290°C and 300°C respectively, and the spindle speed is 15-25r / min.
5. The halogen-free flame retardant material reinforced composite polyethylene according to claim 1, characterized in that: The modified polyvinyl alcohol is obtained by processing the following steps: A1. Add polyvinyl alcohol and deionized water into a reactor and stir until the system is dissolved. The temperature of the reactor is raised to 90-95° C., phosphoric acid solution is added dropwise into the reactor, and the reaction is carried out by heat preservation for 2-3 hours. Urea solution is added into the reactor, and the reaction is carried out by heat preservation for 2-3 hours. Post-treatment is performed to obtain a modified polyvinyl alcohol precursor. A2. Add modified polyvinyl alcohol precursor and tetrahydrofuran into a nitrogen-protected reactor and stir. Raise the temperature of the reactor to 50-60° C., add isocyanatepropyltriethoxysilane into the reactor, keep the reaction temperature for 4-6 hours, and perform post-treatment to obtain modified polyvinyl alcohol.
6. The halogen-free flame retardant material reinforced composite polyethylene according to claim 5, characterized in that: In step A1, the amount ratio of the polyvinyl alcohol, deionized water, phosphoric acid solution and urea solution is 5g:50mL:10mL:5mL, the mass fraction of the phosphoric acid is 20-25%, and the urea solution is composed of urea and deionized water in an amount ratio of 2g:5mL. The post-treatment operation includes: after the reaction is completed, the temperature of the reactor is reduced to room temperature, the film is cast, placed in a saturated sodium sulfate solution, solidified, washed with deionized water 5-8 times and then drained, transferred to a drying oven at a temperature of 60-70°C, and dried to constant weight to obtain a modified polyvinyl alcohol precursor; in step A2, the amount ratio of the modified polyvinyl alcohol precursor, tetrahydrofuran and isocyanatepropyltriethoxysilane is 3g:20mL:1g, and the post-treatment operation includes: after the reaction is completed, the reactor is kept at 50-60°C, and tetrahydrofuran is evaporated under reduced pressure to obtain modified polyvinyl alcohol.
7. The halogen-free flame retardant material reinforced composite polyethylene according to claim 1, characterized in that: The flame retardant reinforcing agent is obtained by processing the following steps: B1, palygorskite, magnesium oxide and zinc oxide are mixed, crushed by a pulverizer, and passed through a 100-mesh sieve to obtain a mixed powder; B2, adding the mixed powder, anhydrous ethanol and KH-550 into a reactor and stirring, raising the temperature of the reactor to 50-60°C, adding sodium hydroxide solution into the reactor, keeping the temperature for 3-5h, and post-treating to obtain an activated mixed powder; B3, adding 6-chloro-2,4-amino-1,3,5-triazine, N-methylpyrrolidone solution and activated mixed powder into a reactor and stirring, raising the temperature of the reactor to 100-110°C, keeping the temperature for reaction for 10-12h, and post-treating to obtain a modified mixed powder; B4. Evenly mix the modified mixed powder and stearic acid to obtain a flame retardant enhancer.
8. The halogen-free flame retardant material reinforced composite polyethylene according to claim 7, characterized in that: In step B1, the weight ratio of palygorskite, magnesium oxide and zinc oxide is 3:1:1; in step B2, the amount ratio of the mixed powder, anhydrous ethanol, KH-550 and sodium hydroxide solution is 2g:15mL:1g:3mL, the concentration of the sodium hydroxide solution is 1-2mol / L, and the post-treatment comprises: after the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, the filter cake is washed with 65wt% ethanol aqueous solution until neutral and then dried, the filter cake is transferred to a drying oven at a temperature of 65-75°C, and dried to constant weight to obtain an activated mixed powder; in step B3, the 6-chloro-2 , the dosage ratio of 4-amino-1,3,5-triazine, N-methylpyrrolidone solution and activated mixed powder is 2g:20mL:5g, the N-methylpyrrolidone solution is composed of N-methylpyrrolidone and 15-20wt% sodium bicarbonate solution in a volume ratio of 3:2, and the post-treatment includes: after the reaction is completed, the temperature of the reactor is lowered to room temperature, filtered, the filter cake is washed with purified water until neutral and then dried, the filter cake is transferred to a drying oven at a temperature of 65-75°C, and dried to constant weight to obtain a modified mixed powder; in step B4, the weight ratio of the modified mixed powder to stearic acid is 5:1-2.
9. The method for preparing a halogen-free flame retardant material reinforced composite polyethylene according to any one of claims 1 to 8, characterized in that: The preparation method of the halogen-free flame retardant material reinforced composite polyethylene is as follows: polyethylene elastomer, flame retardant reinforcing agent and auxiliary additives are uniformly mixed and added into a twin-screw extruder, melt-extruded into a molding die, cooled and solidified, and the composite polyethylene is prepared.
10. The method for preparing a halogen-free flame retardant material reinforced composite polyethylene according to claim 9, characterized in that: The temperatures of the six temperature sections of the twin-screw extruder from the feed end toward the die are 290° C., 300° C., 300° C., 300° C., 300° C. and 310° C., respectively, and the main shaft speed is 10-16 r / min.
Citation Information
Cited By
Flame-retardant high-toughness modified PP (polypropylene) material as well as preparation method and application thereof
CN120484380A