Low-temperature-resistant stiffening and toughening type polypropylene random copolymer pipe and preparation method thereof
By adopting multi-layer blending structure and online hot water treatment process in random copolymer polypropylene pipes, the problems of low-temperature brittle cracking and welding flange peeling of PP-R pipes are solved, and the low-temperature impact resistance and Voltage resistance and reduce production costs and energy consumption.
Patent Information
- Application Number
- CN202411378226.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-26
AI Technical Summary
The existing random copolymer polypropylene (PP-R) pipes are severely brittle and cracked under low temperature conditions. Although the heat treatment process improves the low-temperature impact resistance, it has long manufacturing time, high cost, unstable equipment, high energy consumption and welding flips The problem of skinning.
The structural design of β-PPR blending inner layer, low-temperature rigid-reinforced toughening intermediate layer and α-PPR blending outer layer is adopted. Through the blending of ethylene propylene tereum rubber, nano CaCO3, compatibility agent and PP-R, Combined with the online hot water treatment process, the crystallization rate and crystallization ability of the pipe are improved, and a polycrystalline structure is formed to enhance rigidity and toughness.
It significantly improves the low-temperature impact resistance and pressure resistance of the pipe, reduces production costs and energy consumption, reduces welding peeling phenomenon, and improves the convenience and safety of construction.
Smart Images

Figure CN119022137A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of pipes, and in particular relates to a low-temperature resistant, rigidity-enhanced and toughened random copolymer polypropylene pipe and a preparation method thereof. Background Art
[0002] Random copolymer polypropylene (PP-R) is a new type of resin developed in the late 1980s and early 1990s. It has excellent mechanical properties, good molding and processing properties, and relatively low production costs. It is widely used in various industries of national production (such as hot and cold water pipes, auto parts, furniture, etc.). As a new type of green material, the use of PP-R can not only reduce the damage to the ecological environment, but also meet people's needs in the field of production and life; however, the material is very prone to brittle cracking under low temperature conditions and has poor toughness, which limits the further development of PP-R.
[0003] In order to solve the low-temperature brittle cracking problem of existing PP-R pipes, a common way is to add a heat treatment process after the pipes are off the production line. The heat treatment increases the crystallization rate and crystallization ability of PP-R, improves the activity of the molecular chain and the regularity of the lattice stacking, and promotes the perfection of crystallization, so as to improve the low-temperature impact resistance of PP-R pipes.
[0004] The use of offline oven heat treatment process to improve the low-temperature impact performance of PP-R pipes requires that the pipes be heat treated at 85℃-125℃ for 2-2.5h after they are offline. This can increase the low-temperature drop hammer impact integrity rate of random copolymer polypropylene pipes by more than five times. However, it was found during the actual construction process that when the temperature in winter was below -5℃, the pipes still frequently broke. At the same time, it would consume a lot of time and energy for factory production, and would require investment in heat treatment equipment and sites.
[0005] Moreover, oven heat treatment is an important factor causing the flakes on the welded flanges of pipes. The purpose of heat treatment is to improve the low-temperature brittleness of PP-R pipes to a certain extent, but under high temperature conditions, annealing treatment introduces oxygen-containing functional groups into the polymer surface, with a thickness of up to 4-9nm. A small amount of oxygen-containing groups increases the surface tension. During welding, the surface and the inner layer cannot be well fused due to their different structures, causing irregular sliding of the welded flanges and resulting in flakes; the phenomenon of flakes on the welded flanges of pipes frequently occurs during the construction process, which is not conducive to the safety of the installation system.
[0006] Therefore, the use of oven heat treatment to improve the low-temperature impact resistance of pipes, although the performance will be improved, but there are many problems such as high manufacturing time and investment cost, low equipment stability, high energy consumption cost, hot-melt welding flange peeling of pipes and fittings causing installation system safety. Invention content
[0007] In view of this, the present invention aims to provide a low-temperature resistant, rigidified and toughened random copolymer polypropylene pipe and a preparation method thereof, so as to solve at least one technical problem in the background technology.
[0008] To achieve the above object, the technical solution created by the present invention is implemented as follows:
[0009] A low-temperature resistant, rigidity-enhanced and toughened random copolymer polypropylene pipe, comprising a β-PPR blended inner layer, a low-temperature resistant, rigidity-enhanced and toughened middle layer, and an α-PPR blended outer layer;
[0010] The β-PPR blended inner layer, the low temperature resistant stiffening and toughening middle layer, and the α-PPR blended outer layer are arranged in sequence from the inside to the outside;
[0011] And / or, the β-PPR blend inner layer includes a β nucleating agent and PP-R;
[0012] And / or, the low temperature resistant stiffening and toughening middle layer comprises ethylene propylene diene monomer rubber (EPDM), nano-CaCO3, a compatibilizer, a masterbatch and PP-R;
[0013] And / or, the α-PPR blend outer layer includes an α nucleating agent and PP-R.
[0014] Further, the β-PPR blended inner layer comprises 0.4-0.6 β nucleating agent and 99.4-99.6 parts of PP-R in parts by weight;
[0015] And / or, the low temperature resistant stiffening and toughening middle layer comprises, by weight, 10-20 parts of EPDM rubber, 4-6 parts of nano-CaCO3, 8-12 parts of compatibilizer, 3-5 parts of masterbatch and 100 parts of PP-R;
[0016] And / or, the α-PPR blended outer layer comprises 0.01-0.2 parts of α nucleating agent and 99.8-99.99 parts of PP-R by weight.
[0017] Further, the wall thickness of the β-PPR blended inner layer accounts for 45.5%-49.5%;
[0018] And / or, the wall thickness of the low temperature resistant stiffening and toughening intermediate layer accounts for 1%-9%;
[0019] And / or, the wall thickness of the α-PPR blended outer layer accounts for 45.5%-49.5%.
[0020] A method for preparing a low-temperature resistant, rigidity-enhanced and toughened random copolymer polypropylene pipe comprises the following steps:
[0021] S1: EPDM, nano-CaCO3, compatibilizer, masterbatch and PP-R are granulated to obtain the PP-R rigidity and toughness enhancing masterbatch for the middle layer of the pipe;
[0022] S2: Mixing the α nucleating agent and PP-R to obtain an outer layer mixture, and adding the outer layer mixture to an outer layer extruder; mixing the β nucleating agent and PP-R to obtain an inner layer mixture, and adding the inner layer mixture to an inner layer extruder; adding the PP-R rigidity-enhancing and toughening masterbatch for the pipe middle layer obtained in step S1 to the middle layer extruder, and extruding through a three-layer co-extrusion die head to obtain a preliminarily formed low-temperature resistant rigidity-enhanced and toughened random copolymer polypropylene pipe;
[0023] S3: The initially formed low-temperature resistant, stiffened and toughened random copolymer polypropylene pipe is cooled and sized in a vacuum box; it is sequentially subjected to the first online heat treatment and the second online heat treatment, and then subjected to other treatments to be judged as qualified, thereby obtaining the low-temperature resistant, stiffened and toughened random copolymer polypropylene pipe.
[0024] Furthermore, the extrusion temperature of the outer layer mixture in step S1 is 200-210°C, the extrusion temperature of the PP-R stiffening and toughening masterbatch of the middle layer of the pipe is 170-185°C, and the extrusion temperature of the inner layer mixture is 225-235°C.
[0025] Furthermore, the extrusion temperature of the inner layer mixture is 230°C.
[0026] Furthermore, the thickness of the middle layer is 0.03 mm to 0.25 mm.
[0027] Furthermore, the first online heat treatment in step S2 is performed by an online hot water treatment thermostat;
[0028] Preferably, the length of the online heat treatment thermostat is 5.8 meters to 6.2 meters, and the water temperature is 65°C to 75°C;
[0029] Preferably, the second online heat treatment is performed by a normal temperature cooling water tank.
[0030] Furthermore, the other qualified processing judgments in step S3 include spraying characters on the low-temperature resistant stiffening and toughening random copolymer polypropylene pipe with a printer, then towing it with a traction machine, cutting the low-temperature resistant stiffening and toughening random copolymer polypropylene pipe as required with a cutting machine to obtain the product, measuring and testing it, packaging and warehousing it if qualified, and scrapping and crushing it if unqualified.
[0031] Compared with the prior art, the low-temperature resistant, rigidity-enhanced and toughened random copolymer polypropylene pipe and its preparation method created by the present invention have the following advantages:
[0032] 1. The outer layer of the present invention adopts the technical solution of blending α nucleating agent and PP-R. By adding an appropriate amount of α nucleating agent, the crystallinity and crystallization rate of PP-R are improved, α spherulites are generated, and the grains are refined so that the molecules have a microcrystalline structure, so that the PP-R material maintains good processing performance while enhancing the thermal stability of the material and also has excellent mechanical properties. The use of this technical solution can effectively improve the rigidity and tensile strength of the pipe. The pipe has high rigidity and is not easy to sag due to its own weight. It is horizontal and vertical, more beautiful when exposed, has good tensile properties, and is convenient and safe to install and use, thereby reducing the difficulty of construction and increasing the service life of the pipe.
[0033] 2. The intermediate layer of the present invention adopts the technical solution of blending EPDM, nano-CaCO3, compatibilizer, masterbatch and PP-R. As the main low-temperature resistant toughening layer, a dual toughening method of elastomer toughening and inorganic rigid particle toughening is adopted at the same time. By introducing EPDM, the PP-R / EPDM composite material is prepared by melt blending. This method can reduce the grain size of PP-R and refine the grains, so it will consume more energy under the action of external force, thereby greatly improving the low-temperature impact resistance.
[0034] At the same time, by adding nano-CaCO3 to toughen PP-R, the nano-CaCO3 particles will play the role of sandbags. When external force is applied, the agglomerated nano-CaCO3 particles will slide relative to each other, absorb energy, and improve the toughness of the pipe. Under appropriate proportions, not only will the tensile properties of PP-R not be sacrificed, but the rigidity of the pipe will also be greatly improved while its low-temperature impact toughness will be greatly improved.
[0035] The compatibilizer promotes the dispersion of phases, increases the adhesion between phases, improves thermal stability, increases stress transfer efficiency, and provides uniform and stable performance for the material. By means of the bonding force between molecules, it promotes the polymers to be combined together, thereby obtaining a stable blend.
[0036] 3. The inner layer of the present invention adopts the technical scheme of blending β-nucleating agent and PP-R, and promotes the transformation of α-spherulites in PP-R into β-spherulites by adding an appropriate amount of β-nucleating agent, thereby generating a large number of β-spherulites, thereby improving the notched impact strength of the pipe, and essentially improving the low-temperature impact resistance of the PP-R pipe. At the same time, as the proportion of β-spherulites increases, the pressure and heat resistance of the PP-R pipe is also improved, thereby improving the stability and safety of the pipe in long-term use.
[0037] 4. The present invention places the heat treatment process in front of the vacuum sizing cooling box of the PP-R pipe production line, and uses a 65℃-75℃ constant temperature water tank for soaking. After the pipe is cooled once in the vacuum box, it enters the constant temperature box for secondary heating. The rapid heating solves the problems of fast cooling rate and incomplete crystal development during the PP-R processing and molding process, effectively improves the crystallization process of the polymer, reduces the residual stress in the matrix, thereby improving the comprehensive mechanical properties of the material, and improving the crystallization rate and crystallization ability of the PP-R pipe on the production line, achieving the effect of increasing rigidity and toughness, and further improving the low-temperature impact resistance of the PP-R pipe (improved by about 10%) and pressure resistance (improved by about 5%). At the same time, the use of the online hot water treatment process reduces production costs and production energy consumption, and also solves the problem of welding peeling, making construction convenient, fast and simple. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments and descriptions of the present invention are used to explain the present invention and do not constitute an improper limitation on the present invention. In the drawings:
[0039] Figure 1 A schematic diagram of a method for preparing a low-temperature resistant, rigidity-enhanced and toughened random copolymer polypropylene pipe according to an embodiment of the present invention (the outer layer formula, the middle layer formula and the inner layer formula are respectively recorded as formula 1, 2 and 3);
[0040] Figure 2 The cross-sectional schematic diagram is a low-temperature resistant, rigidified and toughened random copolymer polypropylene pipe described in an embodiment of the present invention. DETAILED DESCRIPTION
[0041] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0042] The present invention will be described in detail below with reference to the accompanying drawings and in combination with embodiments.
[0043] Embodiment 1, as Figure 1 to Figure 2 Shown
[0044] The key of the present invention is to introduce a novel online hot water treatment method: after the heat treatment process is pre-placed in the vacuum sizing cooling box of the PP-R pipe production line, a 65℃-75℃ constant temperature water tank is used for soaking. After the pipe is cooled once in the vacuum sizing box, it enters the constant temperature box for secondary heating. The rapid heating solves the problems of fast cooling rate and incomplete crystal development in the PP-R processing and molding process, effectively improves the crystallization process of the polymer, reduces the residual stress in the matrix, thereby improving the comprehensive mechanical properties of the material, and improves the crystallization rate and crystallization ability of the PP-R pipe on the production line, achieving the effect of increasing rigidity and toughness, and further improving the low-temperature impact resistance of the PP-R pipe (increased by about 10%) and pressure resistance (increased by about 5%). At the same time, the use of the online hot water treatment process reduces production costs and production energy consumption, solves the problem of welding peeling, and makes construction convenient, fast and simple.
[0045] Step 1: Granulation. Select EPDM, nano-CaCO3, compatibilizer, masterbatch and PP-R pellets according to the formula requirements. Weigh 15 parts by mass of EPDM, 5 parts by mass of nano-CaCO3, 10 parts by mass of compatibilizer, 4 parts by mass of masterbatch and 100 parts by mass of PP-R resin (Daqing PA14D) respectively, place the weighed materials in a mixer and stir (12min-15min), stir them well and granulate them through a twin-screw extruder, extrude them at a step process temperature of 225°C, 220°C, 205°C and 195°C, then enter the drawing strip for cooling and cutting into plastic particles to obtain the PP-R stiffening and toughening masterbatch for the middle layer of the pipe.
[0046] In the specific implementation, this application uses PP-R resin (PA14D from Daqing Petrochemical), β nucleating agent (WBG-II from Guangdong Weilinna), α nucleating agent (NA-98G from Chenghe Technology), EPDM (Dow 3722P from the United States), nano-CaCO3 (CC-1 from Guangxi Warner), and compatibilizer (J700 from Mitsui, Japan);
[0047] Step 2: stir and mix, and extrude through a Battenfeld-Cincinnati extruder. The equipment uses a three-layer co-extrusion die head. The outer layer of the pipe is added with a formula of 0.1 parts by mass of α-nucleating agent and 99.9 parts by mass of PP-R resin; the middle layer of the pipe uses the granulated material of "step 1"; the inner layer of the pipe is added with a formula of 0.5 parts by mass of β-nucleating agent and 99.5 parts by mass of PP-R resin.
[0048] Step three, traction cooling, after the extruded pipe is cooled for the first time in the vacuum box, it immediately enters the first online heat treatment constant temperature box, the length of the constant temperature box is 5.8 meters to 6.2 meters, the temperature is controlled at 65℃~75℃ to promote crystallization, and then enters the second online heat treatment (normal temperature cooling water tank) in turn.
[0049] Extrusion process parameter requirements: outer layer processing temperature 200-210℃, middle layer 170-185℃, inner layer 225-235℃, cooling water temperature 15-25℃, online heat treatment heating box water temperature 65℃-75℃. The thickness of the middle layer is 0.03mm-0.25mm (taking dn20x2.8 as an example). The inner layer temperature is recommended to be set at 230℃; the higher inner layer temperature is mainly due to the addition of β nucleating agent, in order to promote the rapid crystallization of PP-R, the formation of more and more perfect β crystals is adjusted. With the increase of temperature, the low-temperature impact resistance of the β-PPR system shows a trend of first rising and then falling. The impact strength reaches its highest point at about 233℃, so it is recommended to set 230℃ to ensure the stability of the impact strength.
[0050] Table 1. Processing temperature
[0051]
[0052] Table 2. Comparison of pipes under drop hammer impact at 0℃
[0053]
[0054] Table 3. Comparison of static pressure and tensile data of pipes
[0055]
[0056] The present invention selects to add ethylene propylene diene monomer (EPDM) when configuring the middle layer, mainly because the presence of the elastomer just acts as the center of stress concentration when subjected to external force impact. If ethylene propylene diene monomer (EPDM) is not added, the toughness of the middle layer of the pipe will be greatly reduced, and the function of effectively absorbing impact energy will be lost; if nano-CaCO3 is not added, the elastic modulus and tensile strength of the composite material will be reduced due to the addition of the elastomer in the blending system. In summary, ethylene propylene diene monomer (EPDM) and nano-CaCO3 in the formula show complementary performance, and the content has strict requirements. The different contents of each component will greatly affect the low-temperature impact resistance and tensile properties of the pipe, so the present invention selects the best formula ratio for production through experiments. By using the above three technical solutions, compared with the PP-R pipes treated by offline oven heat treatment, when the pipes are subjected to a 0°C drop hammer test under the same conditions, the intact rates of the pipes (taking dn20x2.8 as an example) are: 0% (ordinary PP-R pipes), 20% (PP-R pipes treated by offline heat treatment), and 80% (PP-R pipes manufactured by the above technical solutions). Compared with the traditional offline annealing method, the low-temperature impact resistance of the pipes of the present invention is improved by more than 400%. It also effectively improves the rigidity and tensile strength of the pipes. It makes the pipes safer during installation and use, and has higher added value.
[0057] 1. Single formula layer test;
[0058] 1. When formula 1 is used alone to produce pipes, the finished pipes have good rigidity and thermal stability, and also have excellent mechanical properties. Compared with ordinary PP-R pipes, the pipes produced using formula 1 can effectively improve the rigidity and tensile strength of the pipes. The pipes have high rigidity and are not easy to sag due to their own weight. They are horizontal and vertical, more beautiful when exposed, and have good tensile properties, but there is no obvious improvement in the low-temperature brittleness of the pipes.
[0059] 2. When formula 3 is used alone to produce pipes, the finished pipes have a majority of crystals of β-spherulites, so the low-temperature brittleness resistance of the pipes is significantly improved. At the same time, as the proportion of β-spherulites increases, the pressure resistance and heat resistance of the PP-R pipes also increase. However, it is still impossible to obtain pipes with excellent low-temperature resistance and external force impact resistance, which is still far from the purpose of the invention.
[0060] 2. The inner and outer structural layers of the pipe are interchanged;
[0061] 1. After exchanging the inner and outer layers of the pipe, extrude the pipe according to the corresponding process and place it in the test room for 24 hours. After eliminating the internal stress inside the pipe, carry out a 0℃ drop hammer impact test. The test samples (taking dn20x2.8 as an example) are grouped into 20 pieces, each piece is 20cm, and a total of two groups of tests are carried out.
[0062] The test found that after the pipe was subjected to a low-temperature (0°C) drop hammer impact, the number of pipe damages increased compared to the pipe of the present invention, and the cracks were all located on the inner surface of the pipe. The fracture form analysis was conducted: when the pipe was impacted by an external force, the external force penetrated the inside of the pipe, and after the middle functional layer absorbed the energy, the residual impact force formed a stress concentration at one point inside the pipe. The inner layer used a technical solution of blending α nucleating agent and PP-R. Although this solution can improve the overall rigidity and tensile strength of the pipe, it cannot effectively improve the toughness of the pipe, so cracks appeared inside the pipe. The specific data is shown in Table 4, so the overall structure of the pipe must be implemented according to the design of the present invention.
[0063] Table 4. Comparison of 0℃ drop hammer impact
[0064]
[0065] Middle layer proportion verification;
[0066] When the proportion of the middle layer is less than 1%, the overall low-temperature impact resistance of the pipe is not significantly improved compared with ordinary PP-R pipes, and the purpose of the present invention cannot be achieved.
[0067] When the proportion of the middle layer is greater than 9%, the pipe will have the following established problems:
[0068] Since the middle layer accounts for too large a proportion, the material rheological properties are prone to be unstable during the pipe processing, affecting production stability;
[0069] If the proportion of the middle layer is too large, it will affect the tensile strength, elastic modulus and high-temperature creep performance of the pipe;
[0070] Due to the high cost of the middle layer formula, if the middle layer accounts for too much, the production cost will be greatly increased.
[0071] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A low temperature resistant, rigid and toughened random copolymer polypropylene pipe, characterized by: It includes a β-PPR blended inner layer, a low-temperature resistant stiffening and toughening middle layer, and an α-PPR blended outer layer; The β-PPR blended inner layer, the low temperature resistant stiffening and toughening middle layer, and the α-PPR blended outer layer are arranged in sequence from the inside to the outside; And / or, the β-PPR blend inner layer includes a β nucleating agent and PP-R; And / or, the low temperature resistant stiffening and toughening middle layer comprises EPDM rubber, nano-CaCO3, compatibilizer, masterbatch and PP-R; And / or, the α-PPR blend outer layer includes an α nucleating agent and PP-R.
2. The low temperature resistant, rigidity and toughness enhanced random copolymer polypropylene pipe according to claim 1, characterized in that: The β-PPR blended inner layer comprises 0.4-0.6 β nucleating agent and 99.4-99.6 parts of PP-R by weight; And / or, the low temperature resistant stiffening and toughening intermediate layer comprises, by weight, 10-20 parts of EPDM rubber, 4-6 parts of nano-CaCO3, 8-12 parts of compatibilizer, 3-5 parts of masterbatch and 100 parts of PP-R.
3. The low temperature resistant, rigidity and toughness enhanced random copolymer polypropylene pipe according to claim 1, characterized in that: The α-PPR blended outer layer comprises 0.01-0.2 parts of α nucleating agent and 99.8-99.99 parts of PP-R by weight.
4. The low temperature resistant, rigidity-enhanced and toughened random copolymer polypropylene pipe according to claim 1, characterized in that: The wall thickness of the β-PPR blended inner layer accounts for 45.5%-49.5%; And / or, the wall thickness of the low temperature resistant stiffening and toughening intermediate layer accounts for 1%-9%; And / or, the wall thickness of the α-PPR blended outer layer accounts for 45.5%-49.5%.
5. The method for preparing a low temperature resistant, rigidity-enhanced and toughened random copolymer polypropylene pipe according to any one of claims 1 to 4, characterized in that: The steps include: S1: EPDM, nano-CaCO3, compatibilizer, masterbatch and PP-R are granulated to obtain the PP-R rigidity and toughness enhancing masterbatch for the middle layer of the pipe; S2: Mixing the α nucleating agent and PP-R to obtain an outer layer mixture, and adding the outer layer mixture to an outer layer extruder; mixing the β nucleating agent and PP-R to obtain an inner layer mixture, and adding the inner layer mixture to an inner layer extruder; adding the PP-R rigidity-enhancing and toughening masterbatch for the pipe middle layer obtained in step S1 to the middle layer extruder, and extruding through a three-layer co-extrusion die head to obtain a preliminarily formed low-temperature resistant rigidity-enhanced and toughened random copolymer polypropylene pipe; S3: The initially formed low-temperature resistant, stiffened and toughened random copolymer polypropylene pipe is cooled and sized in a vacuum box; it undergoes a first online heat treatment, a second online heat treatment, and other treatments to obtain a low-temperature resistant, stiffened and toughened random copolymer polypropylene pipe after being judged as qualified.
6. The method for preparing a low-temperature resistant, rigidity-enhanced and toughened random copolymer polypropylene pipe according to claim 5, characterized in that: The extrusion temperature of the outer layer mixture in step S1 is 200-210°C, the extrusion temperature of the PP-R stiffening and toughening masterbatch of the middle layer of the pipe is 170-185°C, and the extrusion temperature of the inner layer mixture is 225-235°C.
7. The method for preparing a low-temperature resistant, rigidity-enhanced and toughened random copolymer polypropylene pipe according to claim 5, characterized in that: The extrusion temperature of the inner layer mixture is 230°C.
8. The method for preparing a low-temperature resistant, rigidity-enhanced and toughened random copolymer polypropylene pipe according to claim 5, characterized in that: The thickness of the middle layer is 0.03 mm to 0.25 mm.
9. The low temperature resistant, rigidity and toughness enhanced random copolymer polypropylene pipe and its preparation method according to claim 5, characterized in that: The first online heat treatment in step S2 is performed by using an online hot water treatment thermostat; Preferably, the length of the online heat treatment thermostat is 5.8 meters to 6.2 meters, and the water temperature is 65°C to 75°C; Preferably, the second online heat treatment is performed by a normal temperature cooling water tank.
10. The low temperature resistant, rigidity enhanced and toughened random copolymer polypropylene pipe and its preparation method according to claim 5, characterized in that: The other processing judgments in step S3 include spraying characters on the low-temperature resistant stiffening and toughening random copolymer polypropylene pipe with a printer, then towing it with a traction machine, cutting the low-temperature resistant stiffening and toughening random copolymer polypropylene pipe as required with a cutting machine, obtaining the product, measuring and testing it, packaging and warehousing it if it is qualified, and scrapping and crushing it if it is unqualified.
Citation Information
Cited By
Multilayer composite polypropylene color master batch and preparation method thereof
CN121362406A