Anti-cracking concrete for shield segment and preparation method thereof

By using calcium alginate, concave and convex rod soil and modified silica in shield pipe sheet concrete, the cracking and leakage problems of shield pipe sheet concrete are solved, and the cracking and seepage resistance are improved. Reduces cost and process complexity.

CN116199470BActive Publication Date: 2024-11-08XIA MEN SAN HANG HUN NING TU YOU XIAN GONG SI
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211626529.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-17
Publication Date
2024-11-08
Estimated Expiration
2042-12-17

AI Technical Summary

Technical Problem

After the service life of shield pipe sheets increases, concrete cracking, water leakage and bolt reinforcement corrosion are prone to problems such as reduction in the bearing capacity of tunnel lining structures. The application of existing steel fiber concrete has problems such as high cost and poor durability.

Method used

Calcium alginate and concave and concave stick soil as composite wall material and modified silica as core material to prepare sustained release capsules. These sustained release capsules are added to the concrete to improve crack resistance, and hexadecyl trimethoxy Silane hydrophobically modifys the surface of silica and slowly releases the hydrophobically modified silica to repair concrete cracks.

Benefits of technology

Effectively inhibit concrete cracking, improve crack resistance and seepage resistance, extend the service life of the tunnel structure, and reduce the cost and complex process requirements of steel fiber concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004004589170000071
    Figure BDA0004004589170000071
  • Figure BDA0004004589170000081
    Figure BDA0004004589170000081
  • Figure BDA0004004589170000091
    Figure BDA0004004589170000091
Patent Text Reader

Abstract

The present application relates to the technical field of concrete, and specifically discloses a crack-resistant concrete for shield segments and a preparation method thereof, wherein the crack-resistant concrete for shield segments comprises 280-320 parts of cement; 30-45 parts of fly ash; 400-520 parts of sand; 410-470 parts of crushed stone; 60-80 parts of water; 5-10 parts of water reducer; and 3-18 parts of sustained-release capsules, wherein the sustained-release capsules are prepared by using calcium alginate and attapulgite as composite wall materials and modified silica as core materials. The crack-resistant concrete for shield segments of the present application has the advantage of improving the crack resistance of concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete, and in particular to a crack-resistant concrete for shield segments and a preparation method thereof. Background Art

[0002] The shield segment is the main assembly component of the shield construction. The finished segment mold is sealed and poured with concrete to form the shield segment. The shield segment is the innermost barrier of the tunnel, and is responsible for resisting soil pressure, groundwater pressure and some special loads. The quality of the shield segment is directly related to the overall quality and safety of the tunnel.

[0003] Due to the complex rock and soil conditions in which shield tunnels are located, as the service life increases, cracks in the segment concrete gradually appear, leading to water leakage, rust on bolts and steel bars, and shrinkage and deformation of the pipe diameter. The damage and cracks in the segments reduce the bearing capacity of the entire tunnel lining structure, which is a great challenge to controlling the safety and quality indicators of the project.

[0004] At present, the mechanical properties of ordinary reinforced concrete segments are mostly improved by adding steel fibers. As a new type of building material, steel fibers can be added to concrete to effectively hinder the expansion of micro cracks inside the concrete and the formation of macro cracks, significantly improve the strength of the concrete, and have good ductility.

[0005] In the above-mentioned related technologies, although the addition of steel fibers into concrete greatly improves the crack resistance of concrete, the price of steel fibers is relatively expensive, the segment preparation process is complicated, and there are problems such as poor durability due to the rust expansion of exposed steel fibers and waste caused by the failure to fully exert the mechanical properties of steel fibers, which restricts the application of steel fiber concrete in actual projects. Summary of the invention

[0006] In order to improve the crack resistance of concrete, the present application provides a crack-resistant concrete for shield segments and a preparation method thereof.

[0007] The present application provides a crack-resistant concrete for shield segments, which adopts the following technical solution:

[0008] A crack-resistant concrete for shield segments, comprising the following raw materials in parts by weight:

[0009] 280-320 parts of cement;

[0010] 30-45 parts of fly ash;

[0011] Sand 400-520 parts;

[0012] 410-470 parts of crushed stone;

[0013] 60-80 parts of water;

[0014] Water reducing agent 5-10 parts;

[0015] 3-18 sustained-release capsules;

[0016] The sustained-release capsule is prepared by using calcium alginate and attapulgite as composite wall materials and modified silicon dioxide as core material.

[0017] By adopting the above technical scheme, sustained-release capsules are prepared with hydrophobically modified silica as the core material and calcium alginate and attapulgite as the wall materials. Attapulgite is fibrous, contains more adsorbed water, has the characteristics of large specific surface area, good chemical stability, strong adsorption capacity, etc. By adding attapulgite to the wall material, a relatively uniform random support system can be formed inside the concrete, the cohesion of the concrete is improved, the cracks in the concrete are effectively reduced, and the crack resistance of the concrete is improved. The prepared sustained-release capsules can slowly release the hydrophobically modified silica and continuously fill the cracks in the concrete. At the same time, the hydrophobicity of the silica surface can improve the anti-seepage performance of the concrete.

[0018] Optionally, the specific preparation steps of the hydrophobically modified silica are as follows:

[0019] The silica was mixed with deionized water, emulsified for 10-20 minutes, ultrasonicated, and then the hexadecyltrimethoxysilane solution and ammonia water were added, the pH was adjusted to 7-8 with ammonia water, the temperature was raised to 40-60°C, the temperature was kept constant for 1.5-3 hours, filtered, and dried to obtain hydrophobically modified silica.

[0020] By adopting the above technical solution, the surface of silica is hydrophobically modified with hexadecyltrimethoxysilane, and the hydrophobic silica can be used as the core material and encapsulated in a capsule with calcium alginate and attapulgite as the wall material, so as to effectively repair concrete cracks by slowly releasing the hydrophobic silica.

[0021] Optionally, the weight ratio of silicon dioxide to hexadecyltrimethoxysilane is (8-11):1.

[0022] By adopting the above technical solution and adjusting the ratio of silicon dioxide and hexadecyltrimethoxysilane, the grafting rate of hexadecyltrimethoxysilane on the surface of silicon dioxide is increased, thereby effectively improving the hydrophobicity of the surface of silicon dioxide.

[0023] Optionally, the preparation of the sustained-release capsule comprises the following steps:

[0024] S1: Add sodium alginate into water, stir evenly, let stand, add attapulgite, shear, and form a suspension;

[0025] S2: Add hydrophobically modified silica and surfactant to the suspension, shear to form an emulsion, drip CaCl2 solution into the emulsion drop by drop, react, rinse, and dry to obtain sustained-release capsules.

[0026] By adopting the above technical scheme, a cross-linked mixture is formed by the reaction of sodium alginate, attapulgite and CaCl2, calcium alginate and attapulgite are used as capsule wall materials, and hydrophobically modified silica is used as core material. The prepared sustained-release capsule wall material has a certain strength to ensure the stability of the capsule. The attapulgite is dispersed in concrete to improve the crack resistance of the concrete. The hydrophobically modified silica in the core material can repair the cracks in the concrete after being slowly released.

[0027] Optionally, the mass concentration of sodium alginate in the sodium alginate aqueous solution is 1.8-2.5wt%.

[0028] By adopting the above technical solution, when the concentration of the sodium alginate solution is low, the coating rate of the modified silicon dioxide is low. Therefore, by adjusting the concentration of the sodium alginate, the coating rate of the sustained-release capsule is increased.

[0029] Optionally, the weight ratio of attapulgite to sodium alginate is 5:(4-7).

[0030] By adopting the above-mentioned technical scheme, as the amount of attapulgite increases, the attapulgite, as a reinforcing material, is dispersed in the calcium alginate wall material, playing a role in particle reinforcement. At the same time, the magnesium ions and aluminum ions in the attapulgite are replaced with the calcium ions, further increasing the calcification degree of the sustained-release capsules. Therefore, the addition of attapulgite improves the crack resistance of concrete on the one hand, and improves the strength of the sustained-release capsules on the other hand.

[0031] Optionally, the weight ratio of the suspension to the modified silica is (9-11):1.

[0032] By adopting the above technical scheme, due to the hydrophobicity of the surface of modified silica, under the action of surfactant, sodium alginate, attapulgite and CaCl2 react in the emulsion to form a cross-linked mixture, which is cross-linked on the surface of the hydrophobic silica to form a wall material, thereby preparing a sustained-release capsule.

[0033] In a second aspect, the present application provides a method for preparing crack-resistant concrete for shield segments, which adopts the following technical solution:

[0034] A method for preparing crack-resistant concrete for shield segments comprises the following steps:

[0035] Mix cement, fly ash, sand and gravel for 30-45 minutes, add water reducer and water, stir for 5-10 minutes, add sustained-release capsules, stir evenly, and obtain concrete slurry.

[0036] By adopting the above technical solution and adding slow-release capsules that can improve the crack resistance of concrete, cracks that appear in the late stage of concrete shrinkage can be slowed down, thereby greatly improving the crack resistance of concrete.

[0037] In summary, this application has the following beneficial effects:

[0038] 1. Since the present application adopts attapulgite, the fibrous attapulgite can form a relatively uniform random support system inside the concrete, improve the cohesiveness of the concrete, effectively inhibit the arbitrariness of the cracking direction of the concrete, and improve the crack resistance of the concrete.

[0039] 2. This application adopts the method of adding sustained-release capsules into concrete, hydrophobically modifying the surface of silica with hexadecyltrimethoxysilane, introducing long alkyl chains into the surface of silica, and then using modified silica as the core material, and calcium alginate and attapulgite as the wall materials to prepare sustained-release capsules. By adding sustained-release capsules into concrete, the crack resistance of concrete is improved. DETAILED DESCRIPTION

[0040] The present application is further described in detail below in conjunction with embodiments.

[0041] The sources of raw materials for the following embodiments and comparative examples are provided: the raw materials for the embodiments and comparative examples can all be purchased commercially.

[0042] 1.8 kg of sodium alginate was mixed with water to prepare a sodium alginate solution with a mass concentration of 1.8 wt%, and attapulgite was added. The shear time was 20 min to form a suspension. The mass ratio of attapulgite to sodium alginate was 5:4.

[0043] S2: Add 0.1 kg of modified silica to 0.9 kg of suspension....

[0044] Preparation Example of Sustained Release Capsules

[0045] Preparation Example 1

[0046] Mix 0.5 kg of silica with 1.2 kg of deionized water, add 0.2 kg of emulsifier O-100, emulsify for 15 minutes, and ultrasonicate for 25 minutes. Then add 0.3 kg of anhydrous ethanol solution of hexadecyltrimethoxysilane, 0.05 kg of hexadecyltrimethoxysilane, 0.25 kg of anhydrous ethanol, and a weight ratio of anhydrous ethanol to hexadecyltrimethoxysilane of 5:1. Adjust the pH to 8 with 25 wt % ammonia water, heat to 55 ° C, react at constant temperature for 2 hours, filter, and dry at 40 ° C for 4 hours to obtain hydrophobically modified silica.

[0047] S1: 0.02 kg of sodium alginate was mixed with water to prepare a sodium alginate solution with a mass concentration of 2.0 wt%, and after being stirred evenly, the mixture was allowed to stand for 40 min, and 0.02 kg of attapulgite was added, and the shearing time was 20 min to form a suspension;

[0048] S2: Add 0.05 kg of hydrophobically modified silica and 0.0025 kg of surfactant Tween80 to 0.5 kg of suspension, and the shear time is 15 min to form an emulsion. The emulsion is dripped dropwise into 0.9 kg of 2 wt% CaCl2 aqueous solution, and reacted for 10 h. Rinse with clean water and dry to obtain sustained-release capsules.

[0049] Preparation Example 2

[0050] 0.5 kg of silica was mixed with 1.2 kg of deionized water, and 0.2 kg of emulsifier O-100 was added. The mixture was emulsified for 10 min and subjected to ultrasound for 25 min. Then, 0.375 kg of anhydrous ethanol solution of hexadecyltrimethoxysilane was added, wherein the amount of hexadecyltrimethoxysilane was 0.0625 kg, the amount of anhydrous ethanol was 0.3125 kg, and the weight ratio of anhydrous ethanol to hexadecyltrimethoxysilane was 5:1. The pH value was adjusted to 7 with 25 wt % ammonia water, the temperature was raised to 40° C., the mixture was reacted at a constant temperature for 1.5 h, filtered, and dried at 40° C. for 4 h to obtain hydrophobically modified silica.

[0051] S1: 0.018 kg of sodium alginate was mixed with water to prepare a sodium alginate solution with a mass concentration of 1.8 wt%, and after being stirred evenly, the mixture was allowed to stand for 40 min, and 0.0144 kg of attapulgite was added, and the shearing time was 20 min to form a suspension;

[0052] S2: Add 0.056 kg of hydrophobically modified silica and 0.0025 kg of surfactant to 0.504 kg of suspension, and the shear time is 15 min to form an emulsion. Add the emulsion dropwise into 0.9 kg of 2 wt% CaCl2 aqueous solution, react for 10 h, rinse with clean water, and dry to obtain sustained-release capsules.

[0053] Preparation Example 3

[0054] 0.66 kg of silicon dioxide was mixed with 1.2 kg of deionized water, 0.2 kg of emulsifier O-100 was added, emulsification was performed for 20 min, ultrasonication was performed for 25 min, and then 0.36 kg of anhydrous ethanol solution of hexadecyltrimethoxysilane was added, the hexadecyltrimethoxysilane was 0.06 kg, the anhydrous ethanol was 0.3 kg, the weight ratio of anhydrous ethanol to hexadecyltrimethoxysilane was 5:1, the pH was adjusted to 8 with 25 wt % ammonia water, the temperature was raised to 60 ° C, the reaction was carried out at a constant temperature for 3 h, filtered, and dried at 40 ° C to obtain hydrophobically modified silicon dioxide; S1: 0.0252 kg of sodium alginate was mixed with water to prepare a sodium alginate solution with a mass concentration of 2.5 wt %, after stirring evenly, it was allowed to stand for 40 min, 0.018 kg of attapulgite was added, the shear time was 20 min, and a suspension was formed;

[0055] S2: Add 0.045 kg of modified silicon dioxide and 0.0025 kg of surfactant to 0.495 kg of suspension, and the shear time is 15 min to form an emulsion. Add the emulsion dropwise into 0.9 kg of 2 wt% CaCl2 aqueous solution, react for 10 h, rinse with clean water, and dry to obtain sustained-release capsules.

[0056] Preparation Example 4

[0057] 0.504 kg of silica was mixed with 1.2 kg of deionized water, and 0.2 kg of emulsifier O-100 was added. The mixture was emulsified for 15 min and subjected to ultrasound for 25 min. Then, 0.432 kg of anhydrous ethanol solution of hexadecyltrimethoxysilane was added. The amount of hexadecyltrimethoxysilane was 0.072 kg, the amount of anhydrous ethanol was 0.36 kg, and the weight ratio of anhydrous ethanol to hexadecyltrimethoxysilane was 5:1. The pH value was adjusted to 8 with 25 wt % ammonia water, the temperature was raised to 55° C., the mixture was reacted at a constant temperature for 2 h, filtered, and dried at 40° C. for 4 h to obtain hydrophobically modified silica.

[0058] S1: 0.02 kg of sodium alginate was mixed with water to prepare a sodium alginate solution with a mass concentration of 2.0 wt%, and after being stirred evenly, the mixture was allowed to stand for 40 min, and 0.02 kg of attapulgite was added, and the shearing time was 20 min to form a suspension;

[0059] S2: Add 0.05 kg of hydrophobically modified silica and 0.0025 kg of surfactant Tween80 to 0.5 kg of suspension, and the shear time is 15 min to form an emulsion. The emulsion is dripped dropwise into 0.9 kg of 2 wt% CaCl2 aqueous solution, and reacted for 10 h. Rinse with clean water and dry to obtain sustained-release capsules.

[0060] Preparation Example 5

[0061] Mix 0.6 kg of silica with 1.2 kg of deionized water, add 0.2 kg of emulsifier O-100, emulsify for 15 minutes, and ultrasonicate for 25 minutes. Then add 0.3 kg of anhydrous ethanol solution of hexadecyltrimethoxysilane, 0.05 kg of hexadecyltrimethoxysilane, 0.25 kg of anhydrous ethanol, and a weight ratio of anhydrous ethanol to hexadecyltrimethoxysilane of 5:1. Adjust the pH to 8 with 25 wt % ammonia water, heat to 55 ° C, react at constant temperature for 2 hours, filter, and dry at 40 ° C for 4 hours to obtain hydrophobically modified silica.

[0062] S1: 0.02 kg of sodium alginate was mixed with water to prepare a sodium alginate solution with a mass concentration of 2.0 wt%, and after being stirred evenly, the mixture was allowed to stand for 40 min, and 0.02 kg of attapulgite was added, and the shearing time was 20 min to form a suspension;

[0063] S2: Add 0.05 kg of hydrophobically modified silica and 0.0025 kg of surfactant Tween80 to 0.5 kg of suspension, and the shear time is 15 min to form an emulsion. The emulsion is dripped dropwise into 0.9 kg of 2 wt% CaCl2 aqueous solution, and reacted for 10 h. Rinse with clean water and dry to obtain sustained-release capsules.

[0064] Preparation Example 6

[0065] 0.5 kg of silica was mixed with 1.2 kg of deionized water, and 0.2 kg of emulsifier O-100 was added. The mixture was emulsified for 15 min and ultrasonicated for 25 min. Then, 0.3 kg of anhydrous ethanol solution of hexadecyltrimethoxysilane was added, wherein the amount of hexadecyltrimethoxysilane was 0.05 kg, the amount of anhydrous ethanol was 0.25 kg, and the weight ratio of anhydrous ethanol to hexadecyltrimethoxysilane was 5:1. The pH value was adjusted to 8 with 25 wt % ammonia water, the temperature was raised to 55° C., the mixture was reacted at a constant temperature for 2 h, filtered, and dried at 40° C. for 4 h to obtain hydrophobically modified silica.

[0066] S1: 0.05 kg of sodium alginate was mixed with water to prepare a sodium alginate solution with a mass concentration of 2.0 wt%, and after being stirred evenly, the mixture was allowed to stand for 40 min, and 0.03 kg of attapulgite was added, and the shearing time was 20 min to form a suspension;

[0067] S2: Add 0.05 kg of hydrophobically modified silica and 0.0025 kg of surfactant Tween80 to 0.5 kg of suspension, and the shear time is 15 min to form an emulsion. The emulsion is dripped dropwise into 0.9 kg of 2 wt% CaCl2 aqueous solution, and reacted for 10 h. Rinse with clean water and dry to obtain sustained-release capsules.

[0068] Preparation Example 7

[0069] 0.5 kg of silica was mixed with 1.2 kg of deionized water, and 0.2 kg of emulsifier O-100 was added. The mixture was emulsified for 15 min and ultrasonicated for 25 min. Then, 0.3 kg of anhydrous ethanol solution of hexadecyltrimethoxysilane was added, wherein the amount of hexadecyltrimethoxysilane was 0.05 kg, the amount of anhydrous ethanol was 0.25 kg, and the weight ratio of anhydrous ethanol to hexadecyltrimethoxysilane was 5:1. The pH value was adjusted to 8 with 25 wt % ammonia water, the temperature was raised to 55° C., the mixture was reacted at a constant temperature for 2 h, filtered, and dried at 40° C. for 4 h to obtain hydrophobically modified silica.

[0070] S1: 0.048 kg of sodium alginate was mixed with water to prepare a sodium alginate solution with a mass concentration of 2.0 wt%, and after being stirred evenly, the mixture was allowed to stand for 40 min, and 0.03 kg of attapulgite was added, and the shearing time was 20 min to form a suspension;

[0071] S2: Add 0.05 kg of modified silicon dioxide and 0.0025 kg of surfactant Tween80 to 0.5 kg of suspension, and the shear time is 15 min to form an emulsion. Add the emulsion dropwise into 0.9 kg of 2 wt% CaCl2 aqueous solution, react for 10 h, rinse with clean water, and dry to obtain sustained-release capsules.

[0072] Preparation Example 8

[0073] Mix 0.5 kg of silica with 1.2 kg of deionized water, add 0.2 kg of emulsifier O-100, emulsify for 15 minutes, and ultrasonicate for 25 minutes. Then add 0.3 kg of anhydrous ethanol solution of hexadecyltrimethoxysilane, 0.05 kg of hexadecyltrimethoxysilane, 0.25 kg of anhydrous ethanol, and a weight ratio of anhydrous ethanol to hexadecyltrimethoxysilane of 5:1. Adjust the pH to 8 with 25 wt % ammonia water, heat to 55 ° C, react at constant temperature for 2 hours, filter, and dry at 40 ° C for 4 hours to obtain hydrophobically modified silica.

[0074] S1: 0.02 kg of sodium alginate was mixed with water to prepare a sodium alginate solution with a mass concentration of 2.0 wt%, and after being stirred evenly, the mixture was allowed to stand for 40 min, and 0.02 kg of attapulgite was added, and the shearing time was 20 min to form a suspension;

[0075] S2: Add 0.0625 kg of hydrophobically modified silica and 0.0025 kg of surfactant Tween80 to 0.5 kg of the suspension, and the shear time is 15 min to form an emulsion. The emulsion is dripped dropwise into 0.9 kg of a 2 wt% CaCl2 aqueous solution, and reacted for 10 h. The capsule is then rinsed with clean water and dried to obtain sustained-release capsules.

[0076] Preparation Example 9

[0077] Mix 0.5 kg of silica with 1.2 kg of deionized water, add 0.2 kg of emulsifier O-100, emulsify for 15 minutes, and ultrasonicate for 25 minutes. Then add 0.3 kg of anhydrous ethanol solution of hexadecyltrimethoxysilane, 0.05 kg of hexadecyltrimethoxysilane, 0.25 kg of anhydrous ethanol, and a weight ratio of anhydrous ethanol to hexadecyltrimethoxysilane of 5:1. Adjust the pH to 8 with 25 wt % ammonia water, heat to 55 ° C, react at constant temperature for 2 hours, filter, and dry at 40 ° C for 4 hours to obtain hydrophobically modified silica.

[0078] S1: 0.02 kg of sodium alginate was mixed with water to prepare a sodium alginate solution with a mass concentration of 2.0 wt%, and after being stirred evenly, the mixture was allowed to stand for 40 min, and 0.02 kg of attapulgite was added, and the shearing time was 20 min to form a suspension;

[0079] S2: Add 0.05 kg of hydrophobically modified silica and 0.0025 kg of surfactant Tween80 to 0.6 kg of the suspension, and the shear time is 15 min to form an emulsion. The emulsion is dripped dropwise into 0.9 kg of a 2 wt% CaCl2 aqueous solution, and reacted for 10 h. The capsule is then rinsed with clean water and dried to obtain sustained-release capsules.

[0080] Example

[0081] Example 1

[0082] A crack-resistant concrete for shield segments, the raw material dosage of which is shown in Table 1. The preparation method of the crack-resistant concrete for shield segments comprises the following steps:

[0083] Cement, fly ash, sand and crushed stone are mixed and stirred for 40 minutes. The water reducing agent calcium lignin sulfonate and water are added and stirred for 8 minutes. The sustained-release capsules prepared in Preparation Example 1 are added and stirred for 5 minutes to obtain concrete slurry. The cement is ordinary Portland cement with a grade of 52.5, the crushed stone particle size is 23 mm, the fly ash is first-grade fly ash, and the fineness modulus of the sand is 2.2.

[0084] Example 2

[0085] The difference from Example 1 is that a crack-resistant concrete for shield segments, the raw material dosage of which is shown in Table 1, a method for preparing crack-resistant concrete for shield segments, the sustained-release capsules are prepared by Preparation Example 2, comprising the following steps: mixing cement, fly ash, sand and gravel, stirring for 30 minutes, adding water reducer calcium lignin sulfonate and water, stirring for 5 minutes, adding the sustained-release capsules prepared in Preparation Example 2, stirring for 5 minutes, and obtaining concrete slurry.

[0086] Example 3

[0087] The difference from Example 1 is that a crack-resistant concrete for shield segments, the raw material dosage of which is shown in Table 1, a method for preparing crack-resistant concrete for shield segments, the sustained-release capsules are prepared by Preparation Example 3, comprising the following steps: mixing cement, fly ash, sand and gravel, stirring for 45 minutes, adding water reducer calcium lignin sulfonate and water, stirring for 10 minutes, adding the sustained-release capsules prepared in Preparation Example 3, stirring for 5 minutes, and obtaining concrete slurry.

[0088] The components of the raw materials of Examples 1-3 and their corresponding weight parts are shown in Table 1.

[0089] Table 1 Raw materials and their weights in Examples 1-3 (kg)

[0090]

[0091]

[0092] Example 4

[0093] A method for preparing crack-resistant concrete for shield segments, which is different from Example 1 in that the sustained-release capsule is prepared by Preparation Example 4.

[0094] Example 5

[0095] A method for preparing crack-resistant concrete for shield segments, which is different from Example 1 in that the sustained-release capsule is prepared by Preparation Example 5.

[0096] Example 6

[0097] A method for preparing crack-resistant concrete for shield segments, which is different from Example 1 in that the sustained-release capsule is prepared by Preparation Example 6.

[0098] Example 7

[0099] A method for preparing crack-resistant concrete for shield segments, which is different from Example 1 in that the sustained-release capsule is prepared by Preparation Example 7.

[0100] Example 8

[0101] A method for preparing crack-resistant concrete for shield segments, which is different from Example 1 in that the sustained-release capsule is prepared by Preparation Example 8.

[0102] Example 9

[0103] A method for preparing crack-resistant concrete for shield segments, which is different from Example 1 in that the sustained-release capsule is prepared by Preparation Example 9.

[0104] Comparative Example

[0105] Comparative Example 1

[0106] A method for preparing crack-resistant concrete for shield segments, which is different from Example 1 in that the raw materials do not include sustained-release capsules, comprises the following steps:

[0107] 300 kg of cement, 40 kg of fly ash, 450 kg of sand and 430 kg of crushed stone were mixed and stirred for 40 minutes, and 8 kg of water reducing agent calcium lignin sulfonate and 70 kg of water were added and stirred for 8 minutes to obtain concrete slurry.

[0108] Comparative Example 2

[0109] A method for preparing crack-resistant concrete for shield segments, which differs from Example 1 in that the sustained-release capsules are replaced with silicon dioxide, comprises the following steps:

[0110] 300 kg of cement, 40 kg of fly ash, 450 kg of sand and 430 kg of crushed stone were mixed and stirred for 40 minutes, 8 kg of water reducing agent calcium lignin sulfonate and 70 kg of water were added and stirred for 8 minutes, 12 kg of silicon dioxide was added and stirred for 5 minutes to obtain concrete slurry.

[0111] Comparative Example 3

[0112] A method for preparing crack-resistant concrete for shield segments, which is different from Example 1 in that the sustained-release capsule is replaced with attapulgite, comprises the following steps:

[0113] 300 kg of cement, 40 kg of fly ash, 450 kg of sand and 430 kg of crushed stone were mixed and stirred for 40 minutes. 8 kg of water reducing agent calcium lignin sulfonate and 70 kg of water were added and stirred for 8 minutes. 12 kg of attapulgite was added and stirred for 5 minutes to obtain concrete slurry.

[0114] Performance testing

[0115] Test methods

[0116] 1. The concrete slurries prepared in Examples 1-9 and Comparative Examples 1-3 were used as samples to perform the following performance tests:

[0117] 2. Crack resistance test: The prepared concrete was cast into standard cubic specimens of 180mm*180mm*180mm. After curing for 28 days, the surface of the concrete samples was observed for cracks and the crack width was recorded. If the crack width was less than 0.5mm, it was considered to be within the allowable range of cracks. If the crack width was greater than 0.5mm, the concrete was considered to have weak crack resistance.

[0118] Compressive strength test: According to the test standard of GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the 28d compressive strength (MPa) of the sample was tested. The specific results are shown in Table 2.

[0119] Table 2 Performance test results

[0120]

[0121]

[0122] It can be seen from Example 1 and Examples 4-5 and Table 2 that by adjusting the appropriate ratio of silicon dioxide and hexadecyltrimethoxysilane, a sustained-release capsule with good anti-cracking performance can be prepared.

[0123] From Example 1 and Example 6-7 and Table 2, it can be seen that when the amount of attapulgite added is low, the reinforcement effect on the wall material is weakened and the crack repair effect cannot be played. When the amount added is high, the viscosity is too high and the cross-linking reaction is hindered, and the repair performance of the prepared sustained-release capsule on concrete is reduced.

[0124] Combining Example 1 and Examples 8-9 with Table 2, it can be seen that by adjusting the addition ratio of hydrophobically modified silica in the suspension, the hydrophobically modified silica is used as the core material to prepare sustained-release capsules, and the modified silica effectively fills the cracks in the concrete.

[0125] It can be seen from Example 1 and Comparative Examples 1-3 and Table 2 that the prepared sustained-release capsules greatly improve the anti-cracking performance of concrete, the addition of attapulgite inhibits the cracking of concrete, and the modified silica effectively repairs the cracks in concrete.

[0126] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A crack-resistant concrete for shield segments, characterized in that: It is made of the following raw materials in parts by weight: 280-320 parts of cement; 30-45 parts of fly ash; 400-520 parts of sand; 410-470 parts of crushed stone; 60-80 parts of water; 5-10 parts of water reducing agent; 3-18 sustained-release capsules; The sustained-release capsule is prepared by using calcium alginate and attapulgite as composite wall materials and hydrophobically modified silica as core material; The specific preparation steps of the hydrophobically modified silica are as follows: mixing silica with deionized water, emulsifying for 10-20 minutes, ultrasonicating, then adding hexadecyltrimethoxysilane solution and ammonia water, adjusting the pH to 7-8 with ammonia water, heating to 40-60° C., keeping the temperature constant for 1.5-3 hours, filtering, and drying to obtain hydrophobically modified silica; The weight ratio of silicon dioxide to hexadecyltrimethoxysilane is (8-11):1; The preparation of the sustained-release capsule comprises the following steps: S1: adding sodium alginate into water, stirring evenly, and standing to obtain a sodium alginate aqueous solution, and then adding attapulgite, shearing, and forming a suspension; S2: adding hydrophobically modified silica and a surfactant to the suspension, shearing to form an emulsion, dripping the emulsion dropwise into a CaCl2 solution, reacting, washing, and drying to obtain a sustained-release capsule; The mass concentration of sodium alginate in the sodium alginate aqueous solution is 1.8-2.5wt%; the weight ratio of attapulgite to sodium alginate is 5:(4-7); and the weight ratio of the suspension to hydrophobically modified silica is (9-11):

1.

2. The method for preparing crack-resistant concrete for shield segments according to claim 1, characterized in that: The steps include: Mix cement, fly ash, sand and gravel for 30-45 minutes, add water reducer and water, stir for 5-10 minutes, add sustained-release capsules, stir evenly, and obtain concrete slurry.

Citation Information

Patent Citations

  • Method for preparing attapulgite / calcium alginate composite wall material asphalt self-healing capsules

    CN110511435A

  • Self-repairing polymer cement waterproof paint and preparation method thereof

    CN111574126A

  • Anti-crack self-repairing concrete and preparation method thereof

    CN115010440A

  • Super-long-structure high-crack-resistance shrinkage-compensating concrete and preparation method thereof

    CN115073075A

  • Long-life concrete and preparation method thereof

    CN115368069A