A method for coupling carbon dioxide separation and methanation reaction

By using a mixed conductor membrane reactor for carbon dioxide separation and real-time removal of water in the methanation reaction, the problems of carbon dioxide separation efficiency and thermodynamic equilibrium limitations in traditional technology are solved, achieving efficient methanation reaction and carbon dioxide separation, and reducing the cost cost and improve reaction efficiency.

CN116199557BActive Publication Date: 2024-10-11DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202111444095.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-30
Publication Date
2024-10-11
Estimated Expiration
2041-11-30

AI Technical Summary

Technical Problem

It is difficult to simultaneously achieve high permeability and high selectivity of carbon dioxide separation in the methanation reaction with existing technology, and traditional separation membranes cannot meet high-temperature operation requirements, and the thermodynamic process of the methanation reaction is limited by by-product water, which affects the reaction efficiency.

Method used

A mixed conductor membrane reactor is used, and a catalyst-loaded mixed oxygen ion-carbonate ion conductor membrane is used for carbon dioxide separation and methanation reaction coupling. The penetration of carbon dioxide and the reverse removal of water are achieved through the porous skeleton structure and molten carbonate phase. , breaking the thermodynamic equilibrium and improving reaction efficiency.

Benefits of technology

It achieves efficient separation of carbon dioxide and high efficiency of methanation reaction, reduces costs, simplifies the process flow, and improves reaction efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116199557B_ABST
    Figure CN116199557B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of membrane reactors, and specifically relates to a method for coupling carbon dioxide separation, methanation reaction, and timely removal of byproduct water. (1) A mixed gas containing carbon dioxide is introduced into the outer side of a mixed conductor membrane reactor, and hydrogen is introduced into the inner side of the mixed conductor membrane reactor; (2) During the reaction, carbon dioxide permeates from the outer side of the mixed conductor membrane reactor to the inner side and reacts with hydrogen to generate methane and water, and the byproduct water generated is reversely osmotic and discharged. The present invention utilizes a membrane reactor in the methanation reaction process. On the one hand, pure carbon dioxide gas can be directly separated from a low-purity carbon dioxide gas source for methanation reaction. On the other hand, byproduct water can be removed in time to break the chemical equilibrium limitation, thereby achieving the effect of improving the efficiency of the methanation reaction. The present invention couples the three processes of separation, reaction, and byproduct removal in one membrane reactor, and the process is simple, so it has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of membrane reactors, and in particular relates to a method for coupling carbon dioxide separation, methanation reaction and timely removal of by-product water. Background Art

[0002] In recent years, my country's renewable energy power generation technology has developed rapidly, and its share in the energy structure has been increasing. However, due to the seasonal and volatile characteristics of renewable energy, a large number of problems such as wind, water and solar power abandonment have emerged. Power to Gas technology can convert this surplus electricity into synthetic natural gas, which can then be incorporated into existing natural gas pipelines and other infrastructure for storage and large-scale utilization. It is a technology that efficiently connects the power grid and the natural gas grid. It has the characteristics of fast response rate and flexible regulation, and has broad application prospects in improving the efficiency of renewable energy utilization.

[0003] Methanation reaction process ΔH o 298k =-165kJ / mol) is one of the core steps of the power-to-gas technology. It not only solves the problem of hydrogen being difficult to store and transport over long distances, but also realizes the conversion of carbon dioxide, which is conducive to achieving the goal of "carbon neutrality". Hydrogen and carbon dioxide are two raw materials required for the methanation reaction, among which hydrogen is obtained by electrolyzing water from renewable energy. Therefore, how to obtain high-purity and low-cost carbon dioxide is one of the key issues that need to be solved to ensure the economy of the methanation reaction and optimize the power-to-gas process. At present, the separation methods of carbon dioxide mainly include liquid phase absorption method, solid phase adsorption method and membrane separation method. Among them, the liquid phase absorption method and solid phase adsorption method are relatively mature, but the absorbent regeneration process has high energy consumption and high cost. Membrane separation method is an efficient, low-cost and continuously operable separation technology. However, traditional carbon dioxide separation membranes (such as polymer membranes and inorganic membranes) are limited by the "Robinson effect" (a phenomenon in which permeation rate and selectivity are mutually restricted) in terms of permeation rate and selectivity. It is difficult to obtain high permeation rate and high selectivity at the same time, and these separation membranes cannot meet the requirements of high-temperature operation and are difficult to couple with methanation reactions. In addition, since the methanation reaction is an exothermic process, high temperature is favorable to the reaction kinetic process but unfavorable to the thermodynamic process, while low temperature is favorable to the thermodynamic process but the kinetic process is slower. Summary of the invention

[0004] In view of the above problems, the present invention provides a method for coupling carbon dioxide separation and methanation reaction, using a mixed conductor membrane reactor. On the one hand, the membrane reactor can directly separate pure carbon dioxide gas from low-concentration carbon dioxide for methanation reaction, thereby reducing costs; on the other hand, the membrane reactor can break the limitations of thermodynamic equilibrium by timely removing the by-product water of the methanation reaction, thereby improving the reaction efficiency.

[0005] To achieve the above object, the present invention is implemented by the following technical solutions:

[0006] A method for coupling carbon dioxide separation and methanation reaction, the method comprising the following steps:

[0007] (1) Pass a mixed gas containing carbon dioxide into the outside of a mixed conductor membrane reactor, and pass hydrogen into the inside of the mixed conductor membrane reactor;

[0008] (2) During the reaction, carbon dioxide permeates from the outside to the inside of the mixed conductor membrane reactor and reacts with hydrogen to generate methane and water, and at the same time, the by-product water permeates out in the reverse direction.

[0009] In the above technical solution, the operating temperature range of the mixed conductor membrane reactor is 400 - 650 °C.

[0010] In the above technical solution, the catalyst in the mixed conductor membrane reactor is a supported catalyst, and the supported metal components are one or more of Ni, Ca, Fe, Mg, and Co, and the selected carrier is a material the same as or similar to the mixed conductor membrane.

[0011] In the above technical solution, the mass ratio of the metal component to the carrier in the supported catalyst is 0.05 - 1:1.

[0012] In the above technical solution, in the mixed conductor membrane reactor, the mixed conductor membrane is a mixed oxygen ion - carbonate ion conductor membrane, which is prepared from a porous framework structure and a molten carbonate phase impregnated therein; wherein the porous framework structure material is Ce 1-x Sm x O2 or Ce 1-x Gd x O2, where 0 < x ≤ 0.2; the molten carbonate phase is composed of two or three of Li2CO3, Na2CO3, and K2CO3.

[0013] In the above technical solution, the pore diameter of the porous framework structure is 0.1 - 50 microns.

[0014] In the above technical solution, the configuration of the mixed conductor membrane is sheet type or tubular type.

[0015] The beneficial effects of the present invention are as follows:

[0016] The present invention can realize three functions of carbon dioxide separation, methanation reaction, and real-time removal of by-product water in a single mixed conductor membrane reactor. The carbon dioxide separation function enables the methanation reaction to directly utilize low-purity carbon dioxide gas, reducing costs. The real-time removal function of by-product water can break the limitation of chemical equilibrium in thermodynamics and improve the efficiency of the methanation reaction.

[0017] The present invention uses a mixed oxygen ion-carbonate ion conductor membrane as a key component, and utilizes the interaction between oxygen ions and carbonate ions to separate carbon dioxide, thereby obtaining pure carbon dioxide gas. At the same time, it realizes a continuous and controllable supply of carbon dioxide, thereby ensuring that the carbon dioxide concentration in the gas phase is at a relatively low level, thereby preventing the reactor from heating up due to excessive local concentration. The byproduct water of the methanation reaction is removed in a timely manner by utilizing the property of molten carbonate that can conduct hydroxide ions, thereby breaking the limitation of thermodynamic chemical equilibrium, promoting the reaction to move in the direction of generating methane, and improving the reaction efficiency.

[0018] The mixed conductor membrane reactor simultaneously realizes the three processes of gas separation, catalytic reaction and by-product removal, simplifies the production process and improves the efficiency of the reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a structural diagram of the mixed conductor membrane reactor in the present invention;

[0020] Figure 2 The microscopic morphology of the mixed conductor membrane in the present invention, wherein a is a porous skeleton structure, and b is a two-phase dense membrane after being impregnated with molten carbonate. DETAILED DESCRIPTION

[0021] The present invention is further described below in conjunction with embodiments. The described embodiments are only a part of the embodiments of the present invention, but not all of the embodiments.

[0022] The shape of the mixed conductor membrane in the present invention can be designed as a sheet membrane or a tubular membrane according to production requirements.

[0023] In a specific embodiment, the catalyst in the mixed conductor membrane reactor can be but not limited to single metal or combination-based catalysts of Ni, Ca, Fe, Mg, Co. The catalyst can be supported by brushing, impregnation or in-situ precipitation.

[0024] The structure diagram of the mixed conductor membrane reactor used in the following examples is as follows Figure 1 As shown, it includes a quartz tube, a mixed conductor membrane tube, and a heating furnace; the mixed conductor membrane is composed of a porous skeleton structure (such as Figure 2 a) and the molten carbonate two-phase composition immersed therein (as shown in Figure 2 b); a mixed conductor membrane tube is arranged in a quartz tube, and a catalyst is arranged in the mixed conductor membrane tube; the inner side of the mixed conductor membrane tube is connected to a hydrogen pipeline; the top of the quartz tube is connected to a mixed gas pipeline containing carbon dioxide, and a drain port is arranged at the lower end of the quartz tube; a heating furnace is arranged on the outer side of the quartz tube reactor.

[0025] The process of coupling carbon dioxide separation and methanation reaction in the above membrane reactor is as follows:

[0026] A mixed gas containing carbon dioxide is introduced into the outside of the mixed conductor membrane tube, and a mixed gas of hydrogen and helium is introduced into the inside of the mixed conductor membrane tube, and the membrane reactor is heated by a heating furnace. During the reaction, carbon dioxide permeates from the outside to the inside of the mixed conductor membrane and reacts with hydrogen to produce methane and water. At the same time, the by-product water will reversely permeate and be discharged from the drain outlet, thereby improving the efficiency of the methanation reaction.

[0027] Example 1

[0028] Sm 0.2 Ce 0.8 O2(SDC) was used as the porous skeleton material of the mixed conductor membrane reactor to prepare a tubular membrane with an outer diameter of about 9.2 mm, a wall thickness of about 1.0 mm, and a length of about 30 mm. Then, a binary molten carbonate material of 52 mol% Li2CO3-48 mol% Na2CO3 was impregnated to obtain a dense two-phase mixed conductor membrane. A Ni-Ca / SDC catalyst was placed inside the membrane tube. The mixed conductor membrane was sealed to the alumina tube with glass / silver paste. The catalyst was reduced with hydrogen at 700°C, and then the temperature was lowered to 500°C, and 100 mL min was passed through the outside. -1 A mixture of carbon dioxide and nitrogen (50% CO2, 50% N2) was introduced into the inner side at 20 mL / min. -1 A mixture of hydrogen and helium (10% H2, 90% He).

[0029] In Example 1, the carbon dioxide conversion rate was 61.9% and the methane selectivity was 67.3%.

[0030] Example 2

[0031] Sm 0.2 Ce 0.8 O2(SDC) was used as the porous skeleton material of the mixed conductor membrane reactor to prepare a tubular membrane with an outer diameter of about 9.2 mm, a wall thickness of about 1.0 mm, and a length of about 30 mm. Then, a binary molten carbonate material of 52 mol% Li2CO3-48 mol% Na2CO3 was impregnated to obtain a dense two-phase mixed conductor membrane. A Ni-Ca / SDC catalyst was placed inside the membrane tube. The mixed conductor membrane was sealed to the alumina tube with glass / silver paste. The catalyst was reduced with hydrogen at 700°C, and then the temperature was lowered to 500°C, and 100 mL min was passed through the outside. -1 A mixture of carbon dioxide and nitrogen (50% CO2, 50% N2) was introduced into the inner side at 40 mL / min. -1 A mixture of hydrogen and helium (10% H2, 90% He).

[0032] In Example 2, the carbon dioxide conversion rate is 58.7% and the methane selectivity is 41.4%.

[0033] Example 3

[0034] Sm 0.2 Ce 0.8 O2(SDC) was used as the porous skeleton material of the mixed conductor membrane reactor to prepare a tubular membrane with an outer diameter of about 9.2 mm, a wall thickness of about 1.0 mm, and a length of about 30 mm. Then, a binary molten carbonate material of 52 mol% Li2CO3-48 mol% Na2CO3 was impregnated to obtain a dense two-phase mixed conductor membrane. A Ni-Ca / SDC catalyst was placed inside the membrane tube. The mixed conductor membrane was sealed to the alumina tube with glass / silver paste. The catalyst was reduced with hydrogen at 700°C, and then the temperature was lowered to 500°C, and 100 mL min was passed through the outside. -1 A mixture of carbon dioxide and nitrogen (50% CO2, 50% N2) was introduced into the inner side at 20 mL / min. -1 A mixture of hydrogen and helium (25% H2, 75% He).

[0035] In Example 3, the carbon dioxide conversion rate is 89.8% and the methane selectivity is 95.2%.

[0036] Example 4

[0037] Sm 0.2 Ce 0.8 O2(SDC) was used as the porous skeleton material of the mixed conductor membrane reactor to prepare a tubular membrane with an outer diameter of about 9.2 mm, a wall thickness of about 1.0 mm, and a length of about 30 mm. Then, a binary molten carbonate material of 52 mol% Li2CO3-48 mol% Na2CO3 was impregnated to obtain a dense two-phase mixed conductor membrane. A Ni-Ca / SDC catalyst was placed inside the membrane tube. The mixed conductor membrane was sealed to the alumina tube with glass / silver paste. The catalyst was reduced with hydrogen at 700°C, and then the temperature was lowered to 500°C, and 100 mL min was passed through the outside. -1 A mixture of carbon dioxide and nitrogen (50% CO2, 50% N2) was introduced into the inner side at 40 mL / min. -1 A mixture of hydrogen and helium (25% H2, 75% He).

[0038] In Example 4, the carbon dioxide conversion rate is 90.1% and the methane selectivity is 86.2%.

[0039] Comparative Example 1

[0040] Fixed bed reaction process: In the fixed bed reaction process, the amount of catalyst used and the gas flow rate and composition are the same as those of the membrane reactor in Examples 1-4, except that carbon dioxide gas and hydrogen are simultaneously introduced into the quartz tube reactor, the reaction quartz tube is placed in a high-temperature furnace, the temperature is raised to a reaction temperature of 500°C, and a mixture of carbon dioxide, hydrogen and helium is introduced into the reaction tube for reaction. The pressure in the reaction tube is atmospheric pressure. The performance in the fixed bed reactor is compared with that of the membrane reactor. As shown in Table 1, it can be seen that the carbon dioxide conversion rate and methane selectivity in the membrane reactor are significantly higher than those in the fixed bed reactor.

[0041] Table 1

[0042]

Claims

1. A method for coupling carbon dioxide separation and methanation reaction, characterized in that: The method comprises the following steps: (1) A mixed gas containing carbon dioxide is introduced into the outer side of a mixed conductor membrane reactor, and hydrogen is introduced into the inner side of the mixed conductor membrane reactor; (2) During the reaction, carbon dioxide permeates from the outside of the mixed conductor membrane reactor to the inside and reacts with hydrogen to produce methane and water. At the same time, the by-product water is discharged through reverse osmosis. The operating temperature range of the mixed conductor membrane reactor is 400-650°C; The catalyst in the mixed conductor membrane reactor is a supported catalyst, the supported metal component is one or more of Ni, Ca, Fe, Mg, and Co, and the selected carrier is the same or similar material as the mixed conductor membrane; In the mixed conductor membrane reactor, the mixed conductor membrane is a mixed oxygen ion-carbonate ion conductor membrane, which is prepared from a porous framework structure and a molten carbonate phase impregnated therein; wherein the porous framework structure material is Ce 1-x Sm x O2, where 0 < x ≤ 0.2; the molten carbonate phase is composed of two or three of Li2CO3, Na2CO3, and K2CO3; The pore diameter of the porous skeleton structure is 0.1 to 50 microns.

2. The method according to claim 1, characterized in that The mass ratio of the metal component to the carrier in the supported catalyst is 0.05-1:

1.

3. The method according to claim 1, characterized in that: The mixed conductor membrane is in a sheet or tube configuration.

Citation Information

Patent Citations

  • Anti-CO2 mixed conductor oxygen permeable membrane, preparation method and application thereof

    CN102775134A

  • Preparation method of in-situ synthesis carbonate ion-electron mixed conductor dual-phase membrane and prepared product

    CN107008159A

  • Methane anaerobic aromatization method based on molecular sieve membrane reactor

    CN111087279A

  • Method for preparing synthesis gas using carbon dioxide as oxygen resource and its reaction apparatus

    CN1623890A

  • Combined co2 capture and conversion method and system

    US20150047989A1