A polycyclic unsaturated compound and preparation method thereof, and a stain-resistant covering polymer emulsion and preparation method thereof
Polycyclic unsaturated compounds are prepared by reaction of β-(acryloyloxy)propionic acid and camptothecin, and applied to emulsion polymers, which solve the problem of insufficient stain resistance of the covering polymers in water-based coatings, and achieve significant covering effect and resistance Improved stain performance.
Patent Information
- Application Number
- CN202310007240.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-04
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-01-04
AI Technical Summary
The covering polymers in existing water-based coatings have shortcomings in their stain resistance, which leads to poor stain resistance of the paint film, making it difficult to take into account excellent covering effect and stain resistance.
Polycyclic unsaturated compounds are prepared by reacting β-(acryloyloxy)propionic acid with camptothecin and applied to emulsion polymerization to form a polymer with a polycyclic structure, enhancing the emulsion covering effect and stain resistance of the emulsion .
It significantly improves the covering effect and stain resistance of the emulsion. Through the layered structure formed by the multi-ring-based structure and the extension of the long carbon chain, the internal density of the latex particles is reduced, the cavity structure of the paint film is enhanced, and the stain resistance is effectively resisted. Invasive and also has excellent film formation effect.
Smart Images

Figure CN116199697B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer chemistry and relates to a polycyclic unsaturated compound and a preparation method thereof and a stain-resistant covering polymer emulsion and a preparation method thereof. Background Art
[0002] Emulsion polymerization is generally a process in which unsaturated monomers are polymerized into macromolecules by initiators under the action of water and emulsifiers and with the help of mechanical stirring. The place of emulsion polymerization is inside the latex particles, and the polymer molecular chains formed are entangled with each other to form a dense structure inside the latex particles. Therefore, the polymer itself does not have a certain covering effect.
[0003] In real life, water-based paints prepared from emulsions, pigments, fillers, additives and water are used in the field of architectural decoration, which has high requirements on the covering effect of the paint. Currently, water-based paints mainly provide excellent covering effects through titanium dioxide and covering polymers.
[0004] Patent CN114195944A discloses a method for preparing a seed emulsion of a covering polymer. The preparation method is mainly divided into three steps. First, a highly acidic seed emulsion is prepared as the "core layer" of the covering polymer. Then, 1-2 layers of hard shell emulsion are wrapped around the outside of the highly acidic seed emulsion to form a core-shell structure. Finally, at the softening point temperature of the hard shell polymer, alkali solution is added for neutralization, and the alkali solution enters the polymer.
[0005] The acid core layer reacts with the acid core layer to form a hydrophilic polymer. Due to the difference in ion concentration, a large amount of water enters the polymer and swells to form hollow microspheres. Since there is a large amount of acid inside the polymer, its ability to resist stain invasion is poor, resulting in poor stain resistance of the paint film. As a covering polymer for coatings, one of the key development directions of emulsions is to have both excellent covering effect and stain resistance. Summary of the invention
[0006] In view of this, the present invention first provides a polycyclic unsaturated compound and a preparation method thereof, wherein a polycyclic unsaturated monomer is prepared by reacting β-(acryloyloxy)propionic acid with camptothecin, and the polycyclic unsaturated monomer is applied to emulsion polymerization, which can significantly improve the hiding effect of the emulsion while having excellent stain resistance.
[0007] At the same time, the present invention also provides a polymer emulsion prepared from the above-mentioned polycyclic unsaturated compound, which has the function of improving the covering effect and stain resistance of the coating.
[0008] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0009] In one aspect, the present invention provides a polycyclic unsaturated compound, the structure of which is shown in Formula 1:
[0010]
[0011] In one aspect, the present invention also provides a method for preparing the polycyclic unsaturated compound shown in the above formula 1, which is prepared by reacting camptothecin (the structure of which is shown in the following formula 2) with β-(acryloyloxy) propionic acid under the catalysis of concentrated sulfuric acid;
[0012]
[0013] In a preferred embodiment, the molar ratio of camptothecin to β-(acryloyloxy)propionic acid is 1:1-1.4, preferably 1:1.2-1.4;
[0014] The amount of concentrated sulfuric acid is 1-2% of the mass of β-(acryloyloxy) propionic acid, preferably 1.2-2%;
[0015] The concentration of the concentrated sulfuric acid is 90-98wt%, preferably 96-98wt%;
[0016] The reaction temperature is 70-100°C, preferably 80-90°C, and the reaction time is 5-8h, preferably 6-8h;
[0017] Preferably, the reaction is carried out in the presence of a polymerization inhibitor, and the polymerization inhibitor is selected from one or more of hydroquinone, benzoquinone, and nitrobenzene;
[0018] Preferably, the amount of the polymerization inhibitor is 0.2-0.5% by mass of the β-(acryloyloxy)propionic acid, more preferably 0.3-0.4%.
[0019] The polycyclic unsaturated compound represented by the above formula 1 of the present invention can be used to prepare a polymer emulsion, which is applied in the field of coating adhesives and has an excellent covering effect and excellent stain resistance.
[0020] The present invention provides a stain-resistant covering polymer emulsion, which is prepared by emulsion polymerization from raw material components including the following mass percentages:
[0021] (a) 5-30 wt% of a polycyclic unsaturated compound, preferably 10-25%;
[0022] (b) 0.5-5 wt% of phosphorus-containing monomers, preferably 1-3%,
[0023] (c) 0.5-3 wt% of an ethylenically unsaturated monomer having at least one functional group selected from the group consisting of sulfonic acid group, amide group, carboxyl group, hydroxyl group and urea group, preferably 0.5-2%;
[0024] (d) 62-94 wt% of other ethylenically unsaturated monomers, preferably 65-90%;
[0025] Wherein, the total mass of (a)(b)(c)(d) is 100%;
[0026] The component (a) is a polycyclic unsaturated compound represented by Formula 1.
[0027] In the present invention, all phrases in brackets represent either or both of the two situations of including the content in the brackets or not including the content in the brackets. For example, "(meth) phosphate alkyl acrylate" in the text refers to one of phosphate alkyl acrylate, (meth) phosphate alkyl acrylate or a mixture thereof. In addition, in the present invention, unless otherwise specified, the percentages involved are all percentages by mass.
[0028] In a preferred embodiment, the component (b) is selected from one or two of (meth)acrylic acid phosphate alkoxy esters, preferably acrylic acid phosphate alkoxy esters;
[0029] In a preferred embodiment, the component (c) is selected from one or more of acrylic acid, methacrylic acid, itaconic acid, (meth)acrylamide, sodium vinyl sulfonate, sodium p-styrene sulfonate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and ethylene urea ethoxy methacrylate, preferably methacrylic acid;
[0030] In a preferred embodiment, the component (d) is selected from one or more of styrene, alkyl (meth)acrylates having an alkyl group length of 1 to 8 carbons, allyl esters, vinyl esters, and ethyl acetoacetate (meth)acrylate, preferably one or more of methyl methacrylate, butyl acrylate, isooctyl acrylate, styrene, and ethyl acetoacetate methacrylate;
[0031] The emulsion of the present invention is obtained by emulsion polymerization, which is a polymerization method known in the prior art, and technicians can use any feasible method to prepare it;
[0032] Preferably, the raw materials for preparing the emulsion of the present invention may also optionally include some auxiliary agents, such as emulsifiers, initiators, pH regulators, post-treatment agents, etc., which are conventionally selected in the art and are not particularly required by the present invention.
[0033] In a preferred embodiment, the emulsifier is selected from one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium dodecyl sulfonate, alkyl alcohol ether sulfosuccinate, and alkyl alcohol ether sulfate, preferably alkyl alcohol ether sulfosuccinate;
[0034] Preferably, the total amount of the emulsifier is 0.5-3% of the total mass of components (a)-(d), such as 0.5%, 1%, 1.5%, 2%, 2.5%, preferably 1-2%;
[0035] In a preferred embodiment, the initiator is selected from one or more of sodium persulfate, potassium persulfate, and ammonium persulfate, preferably ammonium persulfate;
[0036] Preferably, the total amount of the initiator is 0.15-0.5% of the total mass of components (a)-(d), such as 0.2%, 0.3%, 0.4%, 0.5%, preferably 0.2-0.4%;
[0037] In a preferred embodiment, the pH adjuster is selected from one or more of sodium bicarbonate, ammonium bicarbonate, sodium hydroxide, potassium hydroxide, ethanolamine, dimethylethanolamine, diethanolamine, and triethanolamine, preferably sodium hydroxide;
[0038] Preferably, the end point of the pH regulator addition is to adjust the system pH to 7-9.
[0039] In a preferred embodiment, the post-treatment agent includes an oxidant and / or a reducing agent; the oxidant is selected from one or more of tert-butyl hydroperoxide, hydrogen peroxide, sodium persulfate, potassium persulfate, and ammonium persulfate, preferably tert-butyl hydroperoxide; the reducing agent is selected from one or more of sodium bisulfite, sodium pyrosulfite, and vitamin C, preferably sodium bisulfite;
[0040] Preferably, the total amount of the post-treatment agent is 0.2-0.6% of the total mass of components (a)-(d), such as 0.2%, 0.3%, 0.4%, 0.5%, preferably 0.2-0.4%; more preferably, the mass ratio of the oxidant to the reductant is 1:0.5-2, preferably 1:1-1.5.
[0041] Another aspect of the present invention provides a method for preparing a stain-resistant covering polymer emulsion, comprising the following steps:
[0042] 1) mixing component (a), component (b), component (c), component (d), part of water, and part of emulsifier to prepare a pre-emulsion;
[0043] 2) dissolving part of the initiator in water to obtain a dropwise initiator; dissolving the remaining initiator in water to obtain a bottom initiator;
[0044] 3) Mix the remaining emulsifier with water and add them into the reactor, stir thoroughly and heat to 80-90°C; add part of the pre-emulsified liquid, stir evenly and add all the initiator at the bottom of the reactor, react for 10-20 minutes to obtain the seed emulsion;
[0045] 4) Control the temperature in the reactor to 80-90°C, continue to add the remaining pre-emulsion to the seed emulsion, the feeding time is 3-4h; at the same time, add the initiator dropwise at a uniform speed throughout the process; then keep warm for 20-40min, such as 20, 30 or 40min;
[0046] 5) Cooling the reactor to 70-80°C, gradually adding the post-treatment agent to the reactor within 20-60 minutes, such as 30, 40 or 50 minutes, and then keeping the temperature for 30-60 minutes, such as 40 or 50 minutes;
[0047] 6) Cooling to below 45° C., adding a pH adjuster to adjust the pH of the system to 7-9, filtering the material to obtain a stain-resistant covering polymer emulsion.
[0048] The specific operating conditions involved in the above preparation process are not particularly required by the present invention, and can be selected conventionally in the art. For example, in a preferred embodiment, the amount of the emulsifier added in step 1) is 80-98% of the total mass of the emulsifier, preferably 85-95%;
[0049] The amount of water added is 25-40% of the total mass of water, preferably 28-38%;
[0050] Step 2) is to mix and dissolve 40-60% of the total mass of the initiator, preferably 45-55%, with 4-10% of the total mass of water, preferably 5-8%, to obtain a dropwise initiator; then the remaining initiator is mixed and dissolved with 1-4% of the total mass of water, preferably 1.5-3.5%, to obtain a bottom initiator;
[0051] In step 3), the amount of the pre-emulsion used to prepare the seed emulsion is 2-8%, preferably 3-6%, of the total mass of the pre-emulsion.
[0052] The present invention also provides an application of the stain-resistant hiding polymer emulsion in the field of coatings.
[0053] The polymer emulsion of the invention has excellent dry and wet hiding effects and excellent stain resistance and solvent resistance, and is particularly suitable for the preparation of coating adhesives and other fields.
[0054] The stain-resistant covering polymer emulsion prepared by the invention has a solid content of 40-55wt%, a pH of 7-9 and an emulsion particle size of 100-200nm.
[0055] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0056] The polycyclic unsaturated compounds are prepared by β-(acryloyloxy) propionic acid and camptothecin, wherein β-(acryloyloxy) propionic acid has a relatively long carbon chain and camptothecin has a large polycyclic structure. The polycyclic unsaturated monomers are prepared by reacting β-(acryloyloxy) propionic acid and camptothecin and applied to emulsion polymerization. By relying on the extensibility of the long carbon chain of β-(acryloyloxy) propionic acid and the rigid steric hindrance effect of the large polycyclic structure of camptothecin, the distance between molecular chains can be greatly increased, a large number of cavities can be introduced into the latex particles and the paint film, and the compactness of the latex particles and the paint film can be reduced, thereby preparing a polymer emulsion with a significant covering effect. The polycyclic unsaturated compounds therein can effectively resist the invasion of stains after film formation by relying on the layered structure formed by the polycyclic structure in the molecular structure, so that it has excellent stain resistance. In addition, the polycyclic unsaturated compound molecules contain a certain amount of amine groups, which can form ionic crosslinks with excess carboxyl groups after polymerization. While the polymer has rigid steric hindrance, it also has an excellent film-forming effect. DETAILED DESCRIPTION
[0057] The present invention is further described below by means of specific examples. The examples described in the present invention are only used to illustrate the present invention and do not limit the scope of the present invention.
[0058] The sources of the raw materials used in the following examples are shown in Table 1. Unless otherwise specified, the other raw materials are common commercially available raw materials:
[0059] Table 1
[0060]
[0061]
[0062] Note: DES-30 has an effective content of 30wt%.
[0063] The following performance testing methods are used in the following embodiments:
[0064] Contrast ratio determination: Determine the hiding ratio of the paint film according to GB / T23981-2009.
[0065] Stain resistance: Test the stain resistance of the paint film according to HG / T 4756-2014.
[0066] H NMR spectrum: instrument model: Bruker AvancedⅢ, 400 MHz, CDCl3 solvent.
[0067] [Example 1]
[0068] The steps of preparing the polycyclic unsaturated compound represented by formula 1 are as follows:
[0069] 350 g (1.01 mol) of camptothecin and 150 g (1.04 mol) of β-(acryloyloxy)propionic acid were mixed, 3 g of hydroquinone and 1.8 g of 92 wt% concentrated sulfuric acid were added, and the mixture was reacted at 75° C. for 6.5 h to obtain a polycyclic unsaturated compound of formula 1.
[0070] By nuclear magnetic hydrogen spectrum analysis: H 1 NMR (400MHz, CDCl3), δ0.9(3H,t), 1.96(2H,m), 2.53(2H,t), 4.22(2H,s), 4.54(2H,t), 4. 74 (2H, s), 5.59 (2H, m), 6.05 (2H, m), 6.74 (1H, s), 7.59 (1H, m), 7.84 (1H, s), 7.99 (1H, s).
[0071] [Example 2]
[0072] The steps of preparing the polycyclic unsaturated compound represented by formula 1 are as follows:
[0073] 350 g (1.01 mol) of camptothecin and 170 g (1.18 mol) of β-(acryloyloxy)propionic acid were mixed, 5.1 g of benzoquinone and 2.55 g of 95 wt% concentrated sulfuric acid were added, and the mixture was reacted at 85° C. for 7.5 h to obtain a polycyclic unsaturated compound of formula 1.
[0074] [Example 3]
[0075] The steps of preparing the polycyclic unsaturated compound represented by formula 1 are as follows:
[0076] 350 g (1.01 mol) of camptothecin and 200 g (1.39 mol) of β-(acryloyloxy)propionic acid were mixed, 8 g of nitrobenzene and 3.6 g of 98 wt % concentrated sulfuric acid were added, and the mixture was reacted at 95° C. for 5.5 h to obtain a polycyclic unsaturated compound of formula 1.
[0077] [Example 4]
[0078] The stain-resistant covering polymer emulsion A was prepared according to the following raw material dosage and method:
[0079] 1) 15 g of emulsifier DES-30, 240 g of deionized water, 280 g of polycyclic unsaturated compound (component a), 25 g of PAM200 (component b), 15 g of MAA (component c), 10 g of AM (component c), 370 g of MMA (component d), and 300 g of EHA (component d) were mixed to obtain a pre-emulsion.
[0080] 2) Mix 2 g of initiator APS and 60 g of water to obtain a dropwise initiator; mix 2 g of APS and 30 g of water to obtain a bottom initiator.
[0081] 3) Add 3 g of emulsifier DES-30 and 600 g of deionized water into the reactor and heat to 85° C. in a nitrogen environment. Then add 30 g of the pre-emulsion and all the bottom initiators of the reactor in sequence and keep warm for 10 min to obtain a seed emulsion.
[0082] 4) Control the temperature at 85°C, and simultaneously add the pre-emulsified liquid and the initiator to the seed emulsion. After all the additions are completed within 3 hours, keep the temperature for 40 minutes.
[0083] 5) Cool down to 75°C, add 2g of oxidant t-BHP and 40g of 5% aqueous solution of reducing agent NaHSO3 to the reactor within 30min, and keep warm for another 30min.
[0084] 6) Cooling to below 45° C., adding 5 wt % sodium hydroxide aqueous solution to adjust the system pH to 8, filtering and discharging the material to obtain a covering polymer emulsion A.
[0085] The prepared covering polymer emulsion A has a solid content of 51.7% and an emulsion particle size of 165 nm.
[0086] [Example 5]
[0087] The stain-resistant covering polymer emulsion B was prepared according to the following raw material dosage and method:
[0088] 1) 20 g of emulsifier DES-30, 300 g of deionized water, 240 g of polycyclic unsaturated compound (component a), 15 g of PAM100 (component b), 15 g of MAA (component c), 5 g of SSS (component c), 350 g of MMA (component d), and 375 g of BA (component d) were mixed to obtain a pre-emulsion.
[0089] 2) Mix 1 g of initiator APS with 80 g of water to obtain a dropwise initiator; mix 1 g of APS with 15 g of water to obtain a bottom initiator.
[0090] 3) Add 3 g of emulsifier DES-30 and 600 g of deionized water into the reactor and heat to 85° C. in a nitrogen environment. Then add 40 g of the pre-emulsion and all the initiators at the bottom of the reactor in sequence and keep warm for 10 min to obtain a seed emulsion.
[0091] 4) Control the temperature at 85°C, and simultaneously add the pre-emulsified liquid and the initiator to the seed emulsion. After all the additions are completed within 3 hours, keep the temperature for 40 minutes.
[0092] 5) Cool down to 75°C, add 1g of oxidant t-BHP and 20g of 5% aqueous solution of reducing agent NaHSO3 to the reactor within 30min, and keep warm for another 30min.
[0093] 6) Cooling to below 45° C., adding 5 wt % sodium hydroxide aqueous solution to adjust the system pH to 7.5, filtering and discharging the material to obtain a covering polymer emulsion B.
[0094] The prepared covering polymer emulsion B has a solid content of 49.9% and an emulsion particle size of 155 nm.
[0095] [Example 6]
[0096] The stain-resistant covering polymer emulsion C was prepared according to the following raw material dosage and method:
[0097] 1) 30 g of emulsifier DES-30, 360 g of deionized water, 160 g of polycyclic unsaturated compound (component a), 10 g of PAM200 (component b), 10 g of MAA (component c), 5 g of HEA (component c), 415 g of St (component d), and 400 g of BA (component d) were mixed to obtain a pre-emulsion.
[0098] 2) Mix 1.8 g of initiator APS and 50 g of water to obtain a dropwise initiator; mix 1.2 g of APS and 30 g of water to obtain a bottom initiator.
[0099] 3) Add 3 g of emulsifier DES-30 and 600 g of deionized water into the reactor and heat to 85° C. in a nitrogen environment. Then add 80 g of the pre-emulsion and all the initiators at the bottom of the reactor in sequence and keep warm for 10 min to obtain a seed emulsion.
[0100] 4) Control the temperature at 85°C, and simultaneously add the pre-emulsified liquid and the initiator to the seed emulsion. After all the additions are completed within 3 hours, keep the temperature for 40 minutes.
[0101] 5) Cool down to 75°C, add 2 g of oxidant t-BHP and 20 g of 5% aqueous solution of reducing agent NaHSO3 to the reactor within 30 min, and keep warm for another 30 min.
[0102] 6) Cooling to below 45° C., adding 5 wt % sodium hydroxide aqueous solution to adjust the system pH to 8.5, filtering and discharging the material to obtain a covering polymer emulsion C.
[0103] The prepared covering polymer emulsion C has a solid content of 48.8% and an emulsion particle size of 170 nm.
[0104] [Example 7]
[0105] The stain-resistant covering polymer emulsion D was prepared according to the following raw material dosage and method:
[0106] 1) 35 g of emulsifier DES-30, 400 g of deionized water, 80 g of polycyclic unsaturated compound (component a), 5 g of PAM100 (component b), 3 g of MAA (component c), 2 g of SSS (component c), 510 g of St (component d), and 400 g of EHA (component d) were mixed to obtain a pre-emulsion.
[0107] 2) Mix 2 g of initiator APS and 60 g of water to obtain a dropwise initiator; mix 3 g of APS and 20 g of water to obtain a bottom initiator.
[0108] 3) Add 3 g of emulsifier DES-30 and 600 g of deionized water into the reactor and heat to 85° C. in a nitrogen environment. Then add 100 g of the pre-emulsion and all the initiators at the bottom of the reactor in sequence and keep warm for 10 min to obtain a seed emulsion.
[0109] 4) Control the temperature at 85°C, and simultaneously add the pre-emulsified liquid and the initiator to the seed emulsion. After all the additions are completed within 3 hours, keep the temperature for 40 minutes.
[0110] 5) Cool down to 75°C, add 1.5g of oxidant t-BHP and 60g of 5% aqueous solution of reducing agent NaHSO3 to the reactor within 30min, and keep warm for another 30min.
[0111] 6) Cooling to below 45° C., adding 5 wt % sodium hydroxide aqueous solution to adjust the pH of the system to 8.2, filtering and discharging the material to obtain a covering polymer emulsion D.
[0112] The prepared covering polymer emulsion D has a solid content of 47.9% and an emulsion particle size of 145 nm.
[0113] [Comparative Example 1]
[0114] Emulsion E was prepared according to the method and raw material dosage in Example 5, except that the polycyclic unsaturated compound (component a) represented by Formula 1 was not added to the system.
[0115] The prepared polymer emulsion E has a solid content of 43.2% and an emulsion particle size of 160 nm.
[0116] [Comparative Example 2]
[0117] The polycyclic unsaturated compound (component a) is prepared by using acrylic acid, and the steps are:
[0118] 350g of camptothecin was mixed with 100g of acrylic acid, and 5.1g of benzoquinone and 2.55g of 95wt% concentrated sulfuric acid were added, and the mixture was reacted at 85°C for 6.5h to obtain a polycyclic unsaturated compound. The polycyclic unsaturated compound was used to prepare emulsion F according to the method and raw material dosage in Example 5, and the prepared polymer emulsion F had a solid content of 49.9% and an emulsion particle size of 165nm.
[0119] [Comparative Example 3]
[0120] Emulsion G was prepared according to the method and raw material dosage in Example 5, except that component a) in the system was replaced with an equal amount of camptothecin.
[0121] The prepared covering polymer emulsion G has a solid content of 49.5% and an emulsion particle size of 200 nm.
[0122] [Comparative Example 4]
[0123] Emulsion H was prepared according to the method and raw material dosage in Example 5, except that component a) in the system was replaced with an equal amount of β-(acryloyloxy)propionic acid.
[0124] The prepared covering polymer emulsion H has a solid content of 49.2% and an emulsion particle size of 185 nm.
[0125] [Comparative Example 5]
[0126] The component (a) in Example 5 was replaced by an equal amount of H400 to obtain polymer emulsion I.
[0127] The emulsion AI prepared in the embodiment and the comparative example was used to prepare coatings according to the formula in Table 2 for evaluation. The performance evaluation results are shown in Table 3:
[0128] Table 2
[0129]
[0130]
[0131] Table 3
[0132] sample Contrast ratio / % Stain resistance performance / point Example 4 98.6 72 Example 5 98.2 70 Example 6 98.0 70 Comparative Example 7 97.6 68 Comparative Example 1 95.6 57 Comparative Example 2 95.8 55 Comparative Example 3 95.4 53 Comparative Example 4 95.5 40 Comparative Example 5 96.6 45
[0133] As shown in Table 3, compared with Examples 4-7, the more polycyclic unsaturated compounds are introduced into the system, the higher the contrast ratio of the system is, the better the hiding effect is, and the paint film exhibits excellent stain resistance.
[0134] Comparison of Example 5 with Comparative Examples 1-4 shows that when both the relatively long carbon chain of β-(acryloyloxy)propionic acid and the large polycyclic structure of camptothecin are present, a relatively high contrast ratio can be achieved by relying on the stretchability of the long carbon chain of β-(acryloyloxy)propionic acid and the rigid steric hindrance effect of the large polycyclic structure of camptothecin, thereby achieving an excellent covering effect.
[0135] Comparing Example 5 with Comparative Example 5, the hiding polymer emulsion prepared by using the polycyclic unsaturated compound has a better hiding effect, and the paint film can achieve an excellent stain resistance effect.
Claims
1. A method for preparing a polycyclic unsaturated compound, characterized in that: It is prepared by the reaction of camptothecin and β-(acryloyloxy) propionic acid under the catalysis of concentrated sulfuric acid; The amount of concentrated sulfuric acid used is 1-2% of the mass of β-(acryloyloxy)propionic acid; The concentration of the concentrated sulfuric acid is 90-98wt%; The reaction temperature is 70-100°C and the reaction time is 5-8h; The polycyclic unsaturated compound has a structure as shown in Formula 1:
2. The preparation method according to claim 1, characterized in that: The amount of concentrated sulfuric acid is 1.2-2%; The concentration of concentrated sulfuric acid is 96-98wt%; The reaction temperature is 80-90°C and the reaction time is 6-8h.
3. The preparation method according to claim 1, characterized in that: The molar ratio of camptothecin to β-(acryloyloxy) propionic acid is 1:1-1.
4.
4. The preparation method according to claim 3, characterized in that: The molar ratio of camptothecin to β-(acryloyloxy) propionic acid is 1:1.2-1.
4.
5. The preparation method according to claim 1, characterized in that: The reaction is carried out in the presence of a polymerization inhibitor, and the polymerization inhibitor is selected from one or more of hydroquinone, benzoquinone, and nitrobenzene.
6. The preparation method according to claim 5, characterized in that: The dosage of the polymerization inhibitor is 0.2-0.5% of the mass of β-(acryloyloxy) propionic acid.
7. The preparation method according to claim 6, characterized in that: The dosage of the polymerization inhibitor is 0.3-0.4% of the mass of β-(acryloyloxy) propionic acid.
8. A stain-resistant hiding polymer emulsion, characterized in that: Prepared by emulsion polymerization from the following raw material components in percentage by weight: (a) 5-30 wt% of a polycyclic unsaturated compound; (b) 0.5-5 wt% of a phosphorus-containing monomer; (c) 0.5-3 wt% of an ethylenically unsaturated monomer having at least one functional group selected from the group consisting of a sulfonic acid group, an amide group, a carboxyl group, a hydroxyl group, and a urea group; (d) 62-94 wt% of other ethylenically unsaturated monomers; Wherein, the total mass of (a)(b)(c)(d) is 100%; The component (a) is the polycyclic unsaturated compound according to claim 1; The component (b) is one or two selected from phosphoalkoxy (meth)acrylates; The component (c) is selected from one or more of acrylic acid, methacrylic acid, itaconic acid, (meth)acrylamide, sodium vinyl sulfonate, sodium p-styrene sulfonate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and ethylene urea ethoxy methacrylate; The component (d) is selected from one or more of styrene, alkyl (meth)acrylates having an alkyl group length of 1 to 8 carbon atoms, allyl esters, vinyl esters, and ethyl acetoacetate (meth)acrylate.
9. The stain-resistant hiding polymer emulsion according to claim 8, characterized in that: The component (b) is alkoxy phosphate acrylic acid; The component (c) is methacrylic acid; The component (d) is one or more of methyl methacrylate, butyl acrylate, isooctyl acrylate, styrene, and ethyl acetoacetate methacrylate.
10. The stain-resistant hiding polymer emulsion according to claim 8, characterized in that: Prepared by emulsion polymerization from the following raw material components in percentage by weight: (a) 10-25% of polycyclic unsaturated compounds; (b) 1-3% phosphorus-containing monomers; (c) 0.5-2 wt% of an ethylenically unsaturated monomer having at least one functional group selected from the group consisting of a sulfonic acid group, an amide group, a carboxyl group, a hydroxyl group, and a urea group; (d) 65-90% of other ethylenically unsaturated monomers; The total mass of (a), (b), (c), and (d) is 100%.
11. The stain-resistant hiding polymer emulsion according to claim 8, characterized in that: The preparation raw materials optionally include emulsifiers, initiators, pH regulators, and post-treatment agents.
12. The stain-resistant hiding polymer emulsion according to claim 8, characterized in that: The emulsifier is selected from one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium dodecyl sulfonate, alkyl alcohol ether sulfosuccinate, and alkyl alcohol ether sulfate; The initiator is selected from one or more of sodium persulfate, potassium persulfate, and ammonium persulfate; The pH regulator is selected from one or more of sodium bicarbonate, ammonium bicarbonate, sodium hydroxide, potassium hydroxide, ethanolamine, dimethylethanolamine, diethanolamine, and triethanolamine; The post-treatment agent includes an oxidant and / or a reducing agent; the oxidant is selected from one or more of tert-butyl hydroperoxide, hydrogen peroxide, sodium persulfate, potassium persulfate, and ammonium persulfate; the reducing agent is selected from one or more of sodium bisulfite, sodium pyrosulfite, and vitamin C.
13. The stain-resistant hiding polymer emulsion according to claim 8, characterized in that: The total amount of the emulsifier is 0.5-3% of the total mass of components (a)-(d); The total amount of the initiator is 0.15-0.5% of the total mass of components (a)-(d); The end point of the pH adjusting agent addition is to adjust the system pH to 7-9; The total amount of the post-treatment agent is 0.2-0.6% of the total mass of components (a)-(d).
14. The stain-resistant hiding polymer emulsion according to claim 13, characterized in that: The total amount of the emulsifier is 1-2% of the total mass of components (a)-(d); The total amount of the initiator is 0.2-0.4% of the total mass of components (a)-(d). The total amount of the post-treatment agent is 0.2-0.6% of the total mass of components (a)-(d); 15. The stain-resistant hiding polymer emulsion according to claim 12, characterized in that: The mass ratio of the oxidant to the reducing agent is 1:0.5-2.
16. The stain-resistant hiding polymer emulsion according to claim 15, characterized in that: The mass ratio of the oxidant to the reductant is 1:1-1.
5.
17. A method for preparing the stain-resistant hiding polymer emulsion according to any one of claims 8 to 16, characterized in that: The following steps are involved: 1) mixing component (a), component (b), component (c), component (d), part of water, and part of emulsifier to prepare a pre-emulsion; 2) dissolving part of the initiator in water to obtain a dropwise initiator; dissolving the remaining initiator in water to obtain a bottom initiator; 3) Mix the remaining emulsifier with water and add them into the reactor, stir thoroughly and heat to 80-90°C; add part of the pre-emulsified liquid, stir evenly and add all the initiator at the bottom of the reactor, react for 10-20 minutes to obtain the seed emulsion; 4) Control the temperature in the reactor to 80-90°C, continue to add the remaining pre-emulsified liquid to the seed emulsion, the feeding time is 3-4h; at the same time, add the initiator dropwise at a uniform speed throughout the process; then keep warm for 20-40min; 5) Cool the reactor to 70-80°C, gradually add the post-treatment agent to the reactor within 20-60 minutes, and then keep warm for 30-60 minutes; 6) Cooling to below 45° C., adding a pH adjuster to adjust the pH of the system to 7-9, filtering the material to obtain a stain-resistant covering polymer emulsion.
18. The preparation method according to claim 17, characterized in that: Step 1) The amount of the emulsifier added is 80-98% of the total mass of the emulsifier; The amount of water added is 25-40% of the total mass of water; Step 2) is to mix and dissolve 40-60% of the total mass of the initiator with 4-10% of the total mass of water to obtain a dropwise initiator; then the remaining initiator is mixed and dissolved with 1-4% of the total mass of water to obtain a bottom initiator; Step 3) The amount of the pre-emulsion used to prepare the seed emulsion is 2-8% of the total mass of the pre-emulsion.
19. The preparation method according to claim 18, characterized in that: In step 1), the amount of the emulsifier added is 85-95% of the total mass of the emulsifier.
20. The preparation method according to claim 18, characterized in that: In step 1), the amount of water added is 28-38% of the total mass of water.
21. The preparation method according to claim 18, characterized in that: Step 2) is to mix and dissolve 45-55% of the total mass of the initiator with 5-8% of the total mass of water to obtain a dropwise initiator; and then mix and dissolve the remaining initiator with 1.5-3.5% of the total mass of water to obtain a bottom initiator.
22. The preparation method according to claim 18, characterized in that: Step 3) The amount of the pre-emulsion used to prepare the seed emulsion is 3-6% of the total mass of the pre-emulsion.
23. Use of the stain-resistant hiding polymer emulsion according to any one of claims 8 to 16 in the field of coatings.