A kind of anti-skid and anti-scouring asphalt pavement fine solid seal layer and its construction method

By using a three-layer sandwich structure of nano-alumina, polydimethylsiloxane-modified epoxy resin, fast-cracking asphalt emulsifier and other materials on the asphalt pavement, combined with improved construction methods, the attenuation of the anti-skid performance of the asphalt pavement is solved. It solves the problem of excessive floating sand and achieves efficient and low-cost road maintenance effect.

CN116200170BActive Publication Date: 2024-10-29GUANGDONG NENGDA HIGHER LEVEL HIGHWAY MAINTENANCE CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310055778.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-19
Publication Date
2024-10-29
Estimated Expiration
2043-01-19

AI Technical Summary

Technical Problem

The anti-skid performance of existing asphalt pavements decays rapidly after it is opened to traffic. The traditional overlay technology is costly, complex in construction, and affects road drainage and driving safety. The fine anti-skid protective layer technology has problems such as slow maintenance, excessive floating sand, and poor durability.

Method used

It adopts a three-layer sandwich asphalt pavement precise sealing layer structure, including a stabilizing layer, a bonding layer and a wear-resistant gravel layer. The bonding layer uses nano-alumina and polydimethylsiloxane to synergistically modify epoxy resin to ensure stability. The layer uses quick-crack asphalt emulsifier, and the wear-resistant gravel layer contains basalt, white corundum, zirconia and gabbro. The anti-skid and waterproof erosion properties are improved through improved construction methods.

Benefits of technology

It has achieved improved anti-skid performance, significant waterproof and scouring effect, low cost, fast maintenance, less floating sand, high bonding strength, good durability, uniform and beautiful surface, low driving noise, and reduced maintenance and repair costs for roads with insufficient anti-skid performance. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure BDA0004060528770000021
    Figure BDA0004060528770000021
Patent Text Reader

Abstract

The present application provides a skid-resistant and scour-resistant asphalt pavement fine sealing layer and a construction method thereof, which adopts a three-layer sandwich structure and places a wear-resistant crushed stone layer in the middle, so as to give full play to the skid-resistant performance of the wear-resistant crushed stone layer and the bonding performance of the bonding layer and the original pavement. The toughness of the resin is increased by adding polydimethylsiloxane, so that the resin is not prone to cracks under the action of cyclic shearing. The addition of nano-alumina improves the bearing capacity of the resin. As a bonding layer, it has excellent bonding strength and can be blended with the wear-resistant crushed stone layer, thereby increasing the service life of the pavement. The bonding layer material and the stabilizing layer material used are both emulsified asphalt materials, which greatly reduce the production cost compared with solvent asphalt. At the same time, it is low-carbon, environmentally friendly, and safe to use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pavement construction, in particular to an anti-skid and anti-scouring asphalt pavement fine solid sealing layer and a construction method thereof. Background Art

[0002] With the continuous increase in the mileage of asphalt pavement on my country's highways, the anti-skid problem of asphalt pavement has become more and more prominent. The main reason is that the anti-skid performance of asphalt pavement will gradually decay as the traffic time increases after it is opened to traffic. The tires of vehicles will wear the asphalt surface during driving, especially in heavy traffic, long downhill sections, sections with heavy rain, tunnels and other sections. The wear will be more serious, resulting in rapid attenuation of asphalt pavement anti-skid index, affecting driving safety. Some newly built asphalt pavements have insufficient anti-skid indicators within 2-3 years after opening to traffic, and the driving lanes are generally more serious than the overtaking lanes. The traditional hot-laid ultra-thin wear layer can improve the anti-skid performance of the road surface, but this process can only lay 1.2cm at the thinnest, and requires mixing at an asphalt mixing station. The construction is complicated, energy-consuming, and the cost is too high. The implementation of a single lane will affect road drainage and driving safety. Although traditional micro-surfacing technology can use a slurry seal paver to mix and spread at room temperature, the thickness must be 1 cm. Single-lane implementation still has the potential to affect road drainage and driving safety. In addition, the anti-skid performance of micro-surfacing decays quickly, the noise is loud, and the appearance is poor. It is no longer recommended by many road maintenance units.

[0003] Recently, there are many asphalt pavement anti-skid maintenance technologies in China that use similar synchronous gravel seal construction processes, such as fine anti-skid protective layer, super surface treatment, fine surface treatment, etc. The construction process of fine anti-skid protective layer is similar to that of fine solid seal, but there are large differences in the manufacturing process and formula of the bonding layer materials and stabilization layer materials used, resulting in the problems of slow curing, high floating sand and poor durability of the fine anti-skid protective layer technology. Summary of the invention

[0004] The present invention overcomes the shortcomings of the prior art. Its main purpose is to improve the components and construction method of the fine sealing layer, so that after paving, it can obtain a road maintenance cover with outstanding anti-skid and water-proof scour performance, thin thickness, low cost, fast curing, less floating sand, high bonding strength, good durability, uniform and beautiful surface, and low driving noise, thereby providing a skid and scour-resistant fine sealing layer for asphalt pavement.

[0005] The second object of the present invention is to provide a construction method for a skid-resistant and scour-resistant asphalt pavement fine seal layer.

[0006] To achieve the above first purpose, the technical solution adopted by the present invention is:

[0007] An anti-skid and anti-scouring asphalt pavement fine sealing layer comprises a stabilizing layer located at an upper layer, a bonding layer located at a lower layer, and a wear-resistant crushed stone layer arranged between the stabilizing layer and the bonding layer;

[0008] The bonding layer comprises the following components in parts by weight:

[0009]

[0010] The modified epoxy resin is an epoxy resin modified by the synergistic action of nano-alumina and polydimethylsiloxane; the epoxy resin is a bisphenol A epoxy resin, and more preferably, the ratio of nano-alumina to polydimethylsiloxane is 3:2. By using nano-alumina and polydimethylsiloxane to synergistically modify the bisphenol A epoxy resin, adding nano-alumina particles to the epoxy resin can significantly improve the mechanical properties of the resin body. The nano-particles dispersed in the polymer matrix can inhibit the slippage of the resin macromolecules and play a role of dispersion strengthening in the resin matrix, thereby improving the hardness of the resin matrix, thereby improving the bearing capacity and wear resistance of the resin coating. As the amount of nano-alumina added gradually increases, the viscosity of the resin gradually increases, the pore size in the resin also increases, and the fluidity decreases. This is because nano-alumina is prone to agglomeration, so 3wt.% of nano-alumina modified bisphenol A epoxy resin is preferred to improve the bonding strength and hardness of the resin. The addition of polydimethylsiloxane increases the toughness of the resin, making it less likely to crack under the action of cyclic shear. The addition of nano-alumina improves the bearing capacity of the resin. As a bonding layer, it has excellent bonding strength and the effect of blending with the wear-resistant crushed stone layer. The bonding layer is prepared by adding modified resin, quaternary ammonium salt cationic emulsifier and SBS modified emulsified asphalt. It has low water content, short curing time and fast strength. In addition, it uses a variety of polymer composite modifications, has a high softening point, good bonding strength, good durability, and excellent anti-slip and water erosion resistance.

[0011] Preferably, the polydimethylsiloxane is a hydroxyl-terminated polydimethylsiloxane. By adopting the hydroxyl-terminated polydimethylsiloxane and the nano-alumina for synergistic modification, it has good high temperature resistance, oxidation resistance, chemical stability and lubrication performance. Because of its unique silicon oxygen chain structure, it can migrate to the surface layer, so that the surface free energy is reduced, thereby improving the corrosion resistance of the polymer. However, the introduction of polydimethylsiloxane will cause the resin to lose certain mechanical properties. Therefore, the nano-alumina is selected to be added to the epoxy resin material, which can enhance the mechanical properties of the epoxy resin while significantly improving its anti-friction performance.

[0012] Preferably, the crystal form of the nano-alumina is γ-Al2O3. By selecting γ-crystalline alumina, it has a high specific surface area, a large number of active centers distributed on the surface, and good stability within a suitable catalytic temperature range. It has high selectivity and high reactivity, is easy to form porous spherical aggregates, and has strong adsorption capacity. When added to epoxy resin materials, it can significantly improve the hardness, mechanical properties and friction and wear properties of the resin material. It helps to form an ideal interface with the epoxy resin in the epoxy resin with a special three-dimensional cross-linked structure, so as to enhance the dispersibility and compatibility of the nano-alumina in the polymer matrix.

[0013] Preferably, the preparation method of the modified epoxy resin comprises the following steps:

[0014] The nano-alumina is placed in anhydrous ethanol containing 1% silane coupling agent for activation, and the activated nano-alumina is poured into bisphenol A epoxy resin preheated at 50°C, stirred at a rate of 200r / min for 3-5min, polydimethylsiloxane is added, and stirred at a rate of 800r / min for 40-50min to obtain a modified epoxy resin. More preferably, the silane coupling agent is γ-methacryloxypropyltrimethoxysilane. The surface of the γ-crystalline nano-alumina is first activated, and then the nano-alumina is blended with the epoxy resin, and then the end-hydroxyl-terminated polydimethylsiloxane is added. The preparation method is simple and easy to operate. After the prepared modified epoxy resin is mixed with emulsified asphalt, the anti-skid and waterproof scouring properties of the road surface can be significantly improved.

[0015] Preferably, the stabilization layer is composed of the following components by weight:

[0016]

[0017]

[0018] By using fast-cracking asphalt emulsifier for emulsification, the solid content is greater than 60%, and no water dilution is required during use. The needle penetration of the evaporation residue is small, the surface dries quickly, and it does not stick to the wheels. The oil film on the upper layer is thick, and the stabilization effect of the gravel layer is greatly improved. After the road is opened to traffic, there is less floating sand. At the same time, the road surface is darker, more beautiful and uniform, and has better durability.

[0019] Preferably, the wear-resistant crushed stone layer includes 5% basalt, 8% white corundum, 4% zirconia and 5% gabbro. By using basalt, white corundum, zirconia and gabbro, they themselves have excellent anti-stripping and water erosion resistance, which can improve the driving conditions of the original road surface, improve its anti-skid performance, repair minor cracks, increase the friction coefficient of the original road surface, and extend the service life of the original road surface, which greatly reduces the cost of maintenance and repair of the road surface due to insufficient anti-skid performance. It can also be used for the cover layer of the road surface being paved, which can effectively ensure road driving safety, and at the same time, the bonding between the bonding layer and the stabilizing layer is tighter.

[0020] Preferably, the wear-resistant crushed stone has a particle size of 2-4 mm, 3-5 mm or 4-6 mm and is manufactured by a single particle size impact crushing process.

[0021] In order to achieve the above second purpose, the technical solution adopted by the present invention is:

[0022] A construction method of the above-mentioned anti-skid and anti-scour asphalt pavement fine sealing layer comprises the following steps:

[0023] S1. The pre-treated wear-resistant crushed stone and the bonding layer are constructed simultaneously. After the bonding layer is paved, the wear-resistant crushed stone layer is immediately spread and cured;

[0024] S2: After the curing is completed, the bonding layer and the wear-resistant crushed stone layer spread in step S1 are rolled and kneaded, and the excess crushed stone is recovered, and then cured;

[0025] S3. After the curing is completed, a stabilizing layer is spread on the surface of the wear-resistant crushed stone layer in step S2. After the curing reaches a certain strength, traffic is opened and the construction is completed.

[0026] Preferably, the specific steps of pretreating the wear-resistant crushed stone in step S1 are: placing the wear-resistant crushed stone in an aqueous solution containing 2-5% tromethamine, ultrasonically stirring for 20-30 minutes, high-speed centrifugal precipitation, separation and drying. By first immersing the wear-resistant crushed stone in an aqueous solution containing tromethamine, the dispersion performance of the wear-resistant crushed stone in the resin matrix can be effectively improved. When spreading the crushed stone, the polarity difference between the crushed stone and the resin matrix can be further overcome, thereby comprehensively improving the anti-slip and water erosion damage resistance of the overall fine solid sealing layer.

[0027] Preferably, the amount of the adhesive layer sprayed in step S1 is 0.8-1.3 kg / m 2 , the spreading amount of wear-resistant crushed stone layer is 5-10kg / m 2 The amount of the stabilizing layer in step S3 is 0.4-0.6kg / m 2 .

[0028] Compared with the prior art, the present invention has the following advantages:

[0029] 1. The present application provides a skid-resistant and scour-resistant asphalt pavement fine sealing layer, which adopts a three-layer sandwich structure and places a wear-resistant crushed stone layer in the middle, so as to give full play to the skid-resistant performance of the wear-resistant crushed stone layer and the bonding performance of the bonding layer and the original pavement. The toughness of the resin is increased by adding polydimethylsiloxane, so that the resin is not easy to crack under the action of cyclic shearing. The addition of nano-alumina improves the bearing capacity of the resin. As a bonding layer, it has excellent bonding strength and can be blended with the wear-resistant crushed stone layer, thereby increasing the service life of the pavement. The bonding layer material and the stabilizing layer material used are both emulsified asphalt materials, which greatly reduce the production cost compared with solvent asphalt. At the same time, it is low-carbon, environmentally friendly and safe to use.

[0030] 2. The present application provides a method for constructing a skid-resistant and scour-resistant asphalt pavement seal layer, which is simple and quick, does not require a large asphalt mixture mixing plant, and can be constructed on a single lane at room temperature. Compared with hot-mix asphalt concrete overlays and micro-surfacing, the thickness of the paving layer can be greatly reduced, thereby reducing construction and material costs. DETAILED DESCRIPTION

[0031] The specific technical scheme of the present invention is described below in conjunction with specific embodiments 1-3 and comparative examples 1-3:

[0032] (1) Preparation of modified epoxy resin:

[0033] γ-Al2O3 is placed in anhydrous ethanol containing 1% γ-methacryloxypropyltrimethoxysilane for activation, wherein the concentration of γ-Al2O3 is 100g / L, and the activated nano-alumina is poured into the bisphenol A epoxy resin preheated at 50°C at a ratio of 3wt.% of the bisphenol A epoxy resin, and stirred at a rate of 200r / min for 5min, and 2wt.% of polydimethylsiloxane is added and stirred at a rate of 800r / min for 50min to obtain the bisphenol A epoxy resin synergistically modified by nano-alumina and polydimethylsiloxane.

[0034] (2) Pretreatment of wear-resistant crushed stone

[0035] The wear-resistant crushed stone was placed in an aqueous solution containing 5% tromethamine, ultrasonicated and fully stirred for 30 minutes, precipitated by high-speed centrifugation, separated and dried, the ultrasonic frequency was 80 kHz, and the stirring rate was 100 r / min.

[0036] Embodiment 1:

[0037] S1. Mix all the components in the bonding layer according to Table 1 and then apply them simultaneously with the pre-treated 2-4 mm wear-resistant crushed stone. The amount of bonding layer applied is 0.8 kg / m 2After the bonding layer is paved, the wear-resistant crushed stone layer is immediately spread. The amount of wear-resistant crushed stone spread is 5kg / m 2 , health preservation;

[0038] S2. After the curing is completed, the adhesive layer and the wear-resistant crushed stone layer spread in step S1 are rolled and kneaded using a rubber-wheel roller, and the excess crushed stone is recovered by a vacuum cleaner, and then the curing is carried out;

[0039] S3. After the curing is completed, the stabilizing layer is spread on the surface of the wear-resistant crushed stone layer in step S2 according to Table 1. After the curing reaches a certain strength, traffic is opened and the construction is completed. The spreading amount of the stabilizing layer is 0.4kg / m 2 .

[0040] Embodiment 2:

[0041] S1. Mix all the components in the bonding layer according to Table 1 and then apply them simultaneously with the pre-treated 3-5 mm wear-resistant crushed stone. The spreading amount of the bonding layer is 1.0 kg / m 2 After the bonding layer is paved, the wear-resistant crushed stone layer is immediately spread. The amount of wear-resistant crushed stone spread is 8kg / m 2 , health preservation;

[0042] S2. After the curing is completed, the adhesive layer and the wear-resistant crushed stone layer spread in step S1 are rolled and kneaded using a rubber-wheel roller, and the excess crushed stone is recovered by a vacuum cleaner, and then the curing is carried out;

[0043] S3. After the curing is completed, the stabilizing layer is spread on the surface of the wear-resistant crushed stone layer in step S2 according to Table 1. After the curing reaches a certain strength, traffic is opened and the construction is completed. The spreading amount of the stabilizing layer is 0.5kg / m 2 .

[0044] Embodiment 3:

[0045] S1. Mix all the components in the bonding layer according to Table 1 and then apply them simultaneously with the pre-treated 4-6 mm wear-resistant crushed stone. The amount of bonding layer applied is 1.3 kg / m 2 After the bonding layer is paved, the wear-resistant crushed stone layer is immediately spread. The amount of wear-resistant crushed stone spread is 10kg / m 2 , health preservation;

[0046] S2. After the curing is completed, the adhesive layer and the wear-resistant crushed stone layer spread in step S1 are rolled and kneaded using a rubber-wheel roller, and the excess crushed stone is recovered by a vacuum cleaner, and then the curing is carried out;

[0047] S3. After the curing is completed, the stabilizing layer is spread on the surface of the wear-resistant crushed stone layer in step S2 according to Table 1. After the curing reaches a certain strength, traffic is opened and the construction is completed. The spreading amount of the stabilizing layer is 0.6kg / m 2 .

[0048] Comparative Example 1

[0049] The modified epoxy resin was replaced with ordinary bisphenol A epoxy resin, and the other components and steps were consistent with those in Example 1.

[0050] Comparative Example 2

[0051] 5% of basalt, 8% of white corundum, 4% of zirconium oxide and 5% of gabbro are removed from the wear-resistant crushed stone and replaced with 3-5 mm crushed stone prepared by ordinary impact crushing process, the main components of which are limestone, quartz sand and silica. The other components and steps are consistent with Example 1.

[0052] Comparative Example 3

[0053] S1. Mix all the components in the bonding layer according to Table 1 and then apply them simultaneously with the untreated 2-4 mm wear-resistant crushed stone. The amount of bonding layer applied is 0.8 kg / m 2 After the bonding layer is paved, the wear-resistant crushed stone layer is immediately spread. The amount of wear-resistant crushed stone spread is 5kg / m 2 , health preservation;

[0054] S2. After the curing is completed, the adhesive layer and the wear-resistant crushed stone layer spread in step S1 are rolled and kneaded using a rubber-wheel roller, and the excess crushed stone is recovered by a vacuum cleaner, and then the curing is carried out;

[0055] S3. After the curing is completed, the stabilizing layer is spread on the surface of the wear-resistant crushed stone layer in step S2 according to Table 1. After the curing reaches a certain strength, traffic is opened and the construction is completed. The spreading amount of the stabilizing layer is 0.4kg / m 2 .

[0056] Table 1: Components of the bonding layer and the stabilizing layer in Examples 1-3 and Comparative Examples 1-3

[0057]

[0058] Examples 1-3 and Comparative Examples 1-3 were tested according to JTG 3450-2019 "Field Test Procedure for Highway Roadbed and Pavement" and JT / T 535-2015 "Water-based Asphalt-based Waterproof Coating for Roads and Bridges", and the test results are shown in Table 2.

[0059] Table 2: Test results of Examples 1-3 and Comparative Examples 1-3

[0060]

[0061] It can be seen from Table 2 that when the unmodified epoxy resin is directly used to prepare the asphalt emulsion, the bonding strength between the epoxy resin and the wear-resistant crushed stone layer is weak, resulting in a certain decrease in its anti-skid performance. The anti-skid performance of the crushed stone without the wear-resistant crushed stone component in the present application and without the pre-treatment of tromethamine immersion is sharply reduced. Therefore, by using nano-alumina and polydimethylsiloxane to synergistically modify the bisphenol A type epoxy resin, adding nano-alumina particles to the epoxy resin can significantly improve the mechanical properties of the resin body. The nano-particles dispersed in the polymer matrix can inhibit the slippage of the resin macromolecules, play a dispersion strengthening role in the resin matrix, and can improve the hardness of the resin matrix. The bearing capacity and wear resistance of the resin coating are thereby improved. The surface of the γ-crystalline nano-alumina is first activated, and then the nano-alumina is blended with the epoxy resin, and then the end-hydroxyl-terminated polydimethylsiloxane is added. The preparation method is simple and convenient to operate. After the prepared modified epoxy resin is mixed with the emulsified asphalt, the anti-skid and water-resistant scour performance of the road surface can be significantly improved. By first immersing the wear-resistant crushed stone in an aqueous solution containing tromethamine, the dispersion performance of the wear-resistant crushed stone in the resin matrix can be effectively improved. When the crushed stone is spread, the polarity difference between the crushed stone and the resin matrix can be further overcome, thereby comprehensively improving the anti-skid and water-resistant scour damage performance of the overall fine solid seal layer.

[0062] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A skid-resistant and scour-resistant asphalt pavement seal, characterized by: It comprises a stabilizing layer located at the upper layer, a bonding layer located at the lower layer, and a wear-resistant crushed stone layer arranged between the stabilizing layer and the bonding layer; The bonding layer comprises the following components in parts by weight: The modified epoxy resin is an epoxy resin modified by nano-alumina and polydimethylsiloxane; the epoxy resin is a bisphenol A type epoxy resin; The wear-resistant crushed stone layer includes 5% basalt, 8% white corundum, 4% zirconium oxide and 5% gabbro; The pretreatment steps of the wear-resistant crushed stone layer are: placing the wear-resistant crushed stone in an aqueous solution containing 2-5% tromethamine, ultrasonicating and fully stirring for 20-30 minutes, high-speed centrifugation precipitation, and separation and drying.

2. The anti-skid and anti-scour asphalt pavement fine seal layer according to claim 1 is characterized by: The polydimethylsiloxane is a hydroxyl-terminated polydimethylsiloxane.

3. The anti-skid and anti-scour asphalt pavement fine seal layer according to claim 1 is characterized by: The crystal form of the nano-alumina is γ-Al2O3.

4. The anti-skid and anti-scour asphalt pavement fine seal layer according to claim 1 is characterized by: The preparation method of the modified epoxy resin comprises the following steps: Place the nano-alumina in anhydrous ethanol containing 1% silane coupling agent for activation, pour the activated nano-alumina into bisphenol A epoxy resin preheated at 50°C, stir at a rate of 200r / min for 3-5min, add polydimethylsiloxane, stir at a rate of 800r / min for 40-50min, and obtain the modified epoxy resin.

5. The anti-skid and anti-scour asphalt pavement fine seal layer according to claim 1 is characterized by: The stabilization layer is composed of the following components by weight:

6. The anti-skid and anti-scour asphalt pavement fine seal layer according to claim 1 is characterized by: The wear-resistant crushed stone has a particle size of 2-4 mm, 3-5 mm or 4-6 mm and is manufactured by a single particle size impact crushing process.

7. A method for constructing a skid-resistant and scour-resistant asphalt pavement fine seal layer according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. The pre-treated wear-resistant crushed stone and the bonding layer are constructed simultaneously. After the bonding layer is paved, the wear-resistant crushed stone layer is immediately spread and cured; S2: After the curing is completed, the bonding layer and the wear-resistant crushed stone layer spread in step S1 are rolled and kneaded, and the excess crushed stone is recovered, and then cured; S3. After the curing is completed, a stabilizing layer is spread on the surface of the wear-resistant crushed stone layer in step S2. After the curing reaches a certain strength, traffic is opened and the construction is completed.

8. The construction method of the anti-skid and anti-scour asphalt pavement fine seal layer according to claim 7 is characterized by: The amount of the adhesive layer sprayed in step S1 is 0.8-1.3 kg / m 2 , the spreading amount of wear-resistant crushed stone layer is 5-10kg / m 2 The amount of the stabilizing layer in step S3 is 0.4-0.6kg / m 2 .

Citation Information

Patent Citations

  • Epoxy resin coating layer having wear resistance and preparation method thereof

    CN108300149A

  • Multi-level precise surface treatment preventive maintenance method

    CN111411556A