Hard anodizing process for a multi-layered bottom pot

By spraying chemical liquid composed of nano-silicon sol, curing and sand processing, the problems of medium and high cost and complex operation of hard oxidation of the compound base pot are solved, and a low-cost and efficient hard oxidation process is achieved.

CN116200735BActive Publication Date: 2024-11-15ZHEJIANG SANHE KITCHENWARE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211539858.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-03
Publication Date
2024-11-15
Estimated Expiration
2042-12-03

AI Technical Summary

Technical Problem

The existing compound pots require high cost and complex operation during the hard oxidation process, resulting in waste of manpower, material resources and financial resources. The protective methods of compound negative films are complex and the operation requirements are high.

Method used

The chemical liquid composed of nano-silica sol, n-butanol, polyphenylmethyl methylsiloxane and purified water is spray-coated and coated with the negative film. After drying and curing, the outer sanding and hard oxidation are carried out to simplify Operation and reduce costs.

Benefits of technology

A low-cost, simple-operated hard oxidation process for compound base pans is realized. The chemical solution has strong sealing properties and acid- and alkali-resistant properties, reducing the cost of a single pot and improving process efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A hard oxidation process for a composite bottom pot comprises the following steps: S1: coating a composite bottom film with chemical liquid: atomizing the chemical liquid by a spray gun and coating it on the surface of the composite bottom film to be protected; S2: surface drying of the chemical liquid: using a drying furnace to dry the coated chemical liquid at 80°C for 2 minutes for curing; S3: external sandblasting: using a scouring wheel to sandblast the outer surface of a metal pot embryo; S4: hard oxidation: hard oxidation treatment of the composite bottom pot embryo.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hard oxidation process for a composite bottom pot. Background Art

[0002] At present, when the composite bottom pot embryo (i.e., the bottom of the pot embryo is composited with a composite film) is hard-oxidized, in order to protect the composite film from being corroded by sulfuric acid in the oxidation tank, most of them adopt the method of composite film laminating or tooling vacuuming (such as CN115251696A). In this case, a lot of manpower, material and financial resources are required, which is a great waste for the company. As for the method of laminating the composite film, the cost of a single pot is 2.5 yuan to 3.5 yuan (depending on the size of the film); as for the method of tooling vacuuming, the cost of a single pot fixture is more than 2.0 yuan (depending on the aging and frequency of use of the fixture, because even if the fixture is used repeatedly, it will age. At the same time, if the order for composite bottom oxidation is too small, the cost of a single pot caused by the investment of tooling fixtures will be higher). In addition, whether it is the method of laminating the composite film or the method of tooling vacuuming, it is very complicated to do, and it has high requirements for the operator's proficiency in operation. Summary of the invention

[0003] In order to overcome the above-mentioned deficiencies in the existing hard oxidation process of a composite bottom pot, the present invention provides a hard oxidation process of a composite bottom pot with low cost and simple operation.

[0004] The technical solution of the present invention to solve the technical problem is: a hard oxidation process of a composite bottom pot, comprising the following steps:

[0005] S1: Chemical liquid coating on the duplex film: The chemical liquid is atomized and coated on the surface of the duplex film to be protected by a spray gun;

[0006] The chemical liquid coating is composed of the following components:

[0007] Nano silica sol 7-15 parts by mass

[0008] 40-60 parts by mass of n-butanol

[0009] 3-8 parts by mass of polyphenylmethylsiloxane

[0010] 30-50 parts by weight of purified water;

[0011] S2: Chemical liquid surface drying: Use a drying oven to dry the coated chemical liquid at 80°C for 2 minutes for curing;

[0012] S3: External sandblasting: Use a scouring wheel to sandblast the outer surface of the metal pot embryo;

[0013] S4: Hard oxidation: The composite bottom pot embryo is subjected to hard oxidation treatment as a whole.

[0014] Preferably, the metal pot embryo is made of aluminum.

[0015] The beneficial effect of the present invention is that the present invention adopts an aqueous chemical solution for spraying the double negative film, and the spraying film thickness is only 2-3 μm. After solidification, the chemical solution has strong sealing and acid and alkali resistance, which can greatly meet the corrosion of strong acid and strong alkali solutions under hard oxidation conditions. Since the chemical raw materials used are the most conventional and the amount used is very small, the cost of a single pot is 0.3 yuan to 0.8 yuan, which greatly reduces the company's hard oxidation process investment, and it is also very simple to operate. DETAILED DESCRIPTION

[0016] The present invention is further described in detail below in conjunction with specific implementation modes.

[0017] Embodiment 1

[0018] A hard oxidation process for a composite bottom pot comprises the following steps:

[0019] S1: Chemical liquid coating on the duplex film: The chemical liquid is atomized and coated on the surface of the duplex film to be protected by a spray gun;

[0020] The chemical liquid coating is composed of the following components:

[0021] Nano silica sol 10 parts by mass

[0022] 50 parts by mass of n-butanol

[0023] 5 parts by mass of polyphenylmethylsiloxane

[0024] 40 parts by weight of purified water;

[0025] S2: Chemical liquid surface drying: Use a drying oven to dry the coated chemical liquid at 80°C for 2 minutes for curing;

[0026] S3: External sandblasting: Use a scouring wheel to sandblast the outer surface of the aluminum pot embryo;

[0027] S4: Hard oxidation: The composite bottom pot embryo is subjected to hard oxidation treatment as a whole.

[0028] Embodiment 2

[0029] A hard oxidation process for a composite bottom pot comprises the following steps:

[0030] S1: Chemical liquid coating on the duplex film: The chemical liquid is atomized and coated on the surface of the duplex film to be protected by a spray gun;

[0031] The chemical liquid coating is composed of the following components:

[0032] Nano silica sol 7 parts by mass

[0033] 45 parts by mass of n-butanol

[0034] 8 parts by mass of polyphenylmethylsiloxane

[0035] 48 parts by weight of purified water;

[0036] S2: Chemical liquid surface drying: Use a drying oven to dry the coated chemical liquid at 80°C for 2 minutes for curing;

[0037] S3: External sandblasting: Use a scouring wheel to sandblast the outer surface of the aluminum pot embryo;

[0038] S4: Hard oxidation: The composite bottom pot embryo is subjected to hard oxidation treatment as a whole.

[0039] Embodiment 3

[0040] A hard oxidation process for a composite bottom pot comprises the following steps:

[0041] S1: Chemical liquid coating on the duplex film: The chemical liquid is atomized and coated on the surface of the duplex film to be protected by a spray gun;

[0042] The chemical liquid coating is composed of the following components:

[0043] Nano silica sol 15 parts by mass

[0044] 55 parts by mass of n-butanol

[0045] 6 parts by mass of polyphenylmethylsiloxane

[0046] 30 parts by weight of purified water;

[0047] S2: Chemical liquid surface drying: Use a drying oven to dry the coated chemical liquid at 80°C for 2 minutes for curing;

[0048] S3: External sandblasting: Use a scouring wheel to sandblast the outer surface of the aluminum pot embryo;

[0049] S4: Hard oxidation: The composite bottom pot embryo is subjected to hard oxidation treatment as a whole.

[0050] Embodiment 4

[0051] A hard oxidation process for a composite bottom pot comprises the following steps:

[0052] S1: Chemical liquid coating on the duplex film: The chemical liquid is atomized and coated on the surface of the duplex film to be protected by a spray gun;

[0053] The chemical liquid coating is composed of the following components:

[0054] Nano silica sol 14 parts by mass

[0055] 40 parts by mass of n-butanol

[0056] 4 parts by mass of polyphenylmethylsiloxane

[0057] 45 parts by weight of purified water;

[0058] S2: Chemical liquid surface drying: Use a drying oven to dry the coated chemical liquid at 80°C for 2 minutes for curing;

[0059] S3: External sandblasting: Use a scouring wheel to sandblast the outer surface of the aluminum pot embryo;

[0060] S4: Hard oxidation: The composite bottom pot embryo is subjected to hard oxidation treatment as a whole.

[0061] Embodiment 5

[0062] A hard oxidation process for a composite bottom pot comprises the following steps:

[0063] S1: Chemical liquid coating on the duplex film: The chemical liquid is atomized and coated on the surface of the duplex film to be protected by a spray gun;

[0064] The chemical liquid coating is composed of the following components:

[0065] Nano silica sol 12 parts by mass

[0066] 60 parts by mass of n-butanol

[0067] 3 parts by mass of polyphenylmethylsiloxane

[0068] 50 parts by weight of purified water;

[0069] S2: Chemical liquid surface drying: Use a drying oven to dry the coated chemical liquid at 80°C for 2 minutes for curing;

[0070] S3: External sandblasting: Use a scouring wheel to sandblast the outer surface of the aluminum pot embryo;

[0071] S4: Hard oxidation: The composite bottom pot embryo is subjected to hard oxidation treatment as a whole.

[0072] Embodiment 6

[0073] A hard oxidation process for a composite bottom pot comprises the following steps:

[0074] S1: Chemical liquid coating on the duplex film: The chemical liquid is atomized and coated on the surface of the duplex film to be protected by a spray gun;

[0075] The chemical liquid coating is composed of the following components:

[0076] Nano silica sol 8 parts by mass

[0077] 58 parts by mass of n-butanol

[0078] 7 parts by mass of polyphenylmethylsiloxane

[0079] 35 parts by weight of pure water;

[0080] S2: Chemical liquid surface drying: Use a drying oven to dry the coated chemical liquid at 80°C for 2 minutes for curing;

[0081] S3: External sandblasting: Use a scouring wheel to sandblast the outer surface of the aluminum pot embryo;

[0082] S4: Hard oxidation: The composite bottom pot embryo is subjected to hard oxidation treatment as a whole.

Claims

1. A hard oxidation process for a composite bottom pot, characterized in that The following steps are involved: S1: Chemical liquid coating on the duplex film: The chemical liquid is atomized and coated on the surface of the duplex film to be protected by a spray gun; The chemical liquid is composed of the following components: Nano silica sol 7-15 parts by mass 40-60 parts by mass of n-butanol 3-8 parts by mass of polyphenylmethylsiloxane 30-50 parts by weight of purified water; S2: Chemical liquid surface drying: Use a drying oven to dry the coated chemical liquid at 80°C for 2 minutes for curing; S3: External sandblasting: Use a scouring wheel to sandblast the outer surface of the metal pot embryo; S4: Hard oxidation: The composite bottom pot embryo is hard-oxidized.

2. The hard oxidation process of a composite bottom pot as claimed in claim 1, characterized in that: The metal pot embryo is made of aluminum.