Three-electrode cell structure, three-electrode battery and negative electrode potential monitoring method
By setting multiple reference electrodes in the three-electrode cell structure, the problems of reference electrode consumption and lithium ion concentration in the prior art are solved, and the negative electrode potential is accurately monitored after a long period, which improves the battery detection accuracy and security.
Patent Information
- Application Number
- CN202310229452.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-10
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-03-10
AI Technical Summary
When testing the negative potential of the existing three-electrode batteries, the consumption of the reference electrode and the lithium ion concentration affect the test accuracy, especially the potential data measured after a long period of time is inaccurate, affecting battery performance and safety.
A three-electrode battery cell structure is designed, including multiple reference electrodes, located outside the battery cell to be tested. By monitoring the negative potential difference in the negative electrode at different stages, the error of the reference electrode pair test is eliminated and the detection accuracy is improved.
It realizes accurate monitoring of the negative electrode potential after a long period of time, reduces the influence of the reference electrode on electrochemical performance, improves the accuracy of the negative electrode potential detection and the safety of the battery, can quantitatively analyze the consumption of active lithium, and guides battery design and management. system.
Smart Images

Figure CN116207357B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-ion batteries, and in particular to a three-electrode battery cell structure, a three-electrode battery and a method for monitoring negative electrode potential. Background Art
[0002] As a new type of high-energy green battery, lithium-ion batteries are widely used in new energy electric vehicles and other fields. This puts higher requirements on the performance and safety of lithium-ion batteries. At the same time, the performance and safety issues of lithium-ion batteries are becoming increasingly prominent, which has attracted great attention from the industry. As a complex electrochemical system, the life and safety of lithium-ion batteries are currently one of the main bottlenecks restricting their development. Among the many factors that cause battery degradation and battery safety problems, the deposition of lithium on the surface of the negative electrode is one of the main reasons for battery capacity degradation and threat to battery safety. When charging under normal conditions, lithium ions are released from the positive electrode and embedded in the negative electrode through the diaphragm. However, when charging at high rates or low temperatures, because the lithium insertion potential of the negative electrode is similar to the deposition potential of metallic lithium, lithium ions do not have time to embed into the negative electrode and lithium precipitation occurs on the surface of the negative electrode, resulting in lithium dendrites. The deposited metallic lithium reacts with the electrolyte to consume active lithium, resulting in increased battery capacity degradation; at the same time, dendritic lithium may pierce the diaphragm, causing the battery to short-circuit, which in turn causes safety problems. Therefore, accurately judging the negative electrode potential to determine the lithium deposition situation of the battery can ensure that the battery always works at an appropriate voltage and current, reducing the consumption of active lithium, which is of great significance to improving the battery cycle life and safety.
[0003] The in-situ test of the negative electrode potential of a three-electrode battery is a common method for judging the lithium deposition of the battery. Usually, a reference electrode is placed between the positive electrode and the negative electrode, and the negative electrode potential is taken as 0V as the standard. When the negative electrode potential is less than 0V, lithium deposition is considered to have occurred. However, due to the presence of lithium ion concentration between the reference electrodes, the lithium ion transfer between the positive and negative electrodes is affected, which affects the performance of the battery to a certain extent. For example, a lithium-plated copper wire is used as a reference electrode and placed between the positive and negative electrodes to monitor the negative electrode potential. Since the copper wire is thin and the amount of lithium plating is limited, the lithium will be gradually consumed during the test, or even completely consumed, exposing the complete copper surface, resulting in inaccurate potential data measured after long-term cycling.
[0004] Therefore, when using the three-electrode method to test the negative electrode potential in the prior art, it is necessary to design a battery and method that can accurately monitor the negative electrode potential after a long period of testing, which can eliminate the error caused by the reference electrode to the test accuracy to the greatest extent and accurately detect the negative electrode potential after a certain period. Summary of the invention
[0005] The present invention provides a three-electrode cell structure, a three-electrode battery and a negative electrode potential monitoring method, which are used to solve the defects of the in-situ testing of the negative electrode potential of the three-electrode battery in the prior art, and can eliminate the error caused by the reference electrode to the test accuracy to the greatest extent, and accurately detect the negative electrode potential after a certain period.
[0006] The present invention provides a three-electrode battery cell structure, comprising an outer shell, an electrolyte encapsulated in the inner shell, and a battery cell to be tested consisting of a first positive electrode sheet, a first negative electrode sheet and a separator of the battery cell to be tested, and also comprising a reference battery cell, wherein the reference battery cell comprises at least two reference electrodes, and the reference battery cell is encapsulated in the inner shell and located outside the battery cell to be tested.
[0007] According to a three-electrode battery cell structure provided by the present invention, there are a plurality of the first positive electrode sheet, the first negative electrode sheet and the battery cell separator to be tested, respectively, and the first positive electrode sheet, the battery cell separator to be tested and the first negative electrode sheet are stacked in sequence to form a laminated electrode group;
[0008] The reference cell is composed of a second positive electrode sheet, a reference cell separator and at least two reference electrodes. The reference cell separator wraps the second positive electrode sheet, and the reference electrode is located between the reference cell separator and the laminated electrode group.
[0009] According to a three-electrode battery cell structure provided by the present invention, the first positive electrode sheet, the first negative electrode sheet, the second positive electrode sheet and the reference electrode respectively form a first positive electrode tab, a first negative electrode tab, a second positive electrode tab and a reference tab outside the outer shell, and there are at least two reference tabs.
[0010] According to a three-electrode battery cell structure provided by the present invention, the reference electrode is a copper wire, a gold wire, a nickel wire or a tinned copper wire.
[0011] According to a three-electrode battery cell structure provided by the present invention, the reference electrode is made of copper wire, the first end of which is a bare copper wire end, and the second end is an enameled copper wire end, the first end of the reference electrode is located between the reference battery cell diaphragm and the laminated electrode group, the second end of the reference electrode extends to the outside of the outer shell, and a nickel strip is welded to the second end to form the reference electrode ear.
[0012] According to a three-electrode battery cell structure provided by the present invention, the reference battery cell separator is a single-layer glue-coated separator or a double-layer glue-coated separator.
[0013] According to a three-electrode battery cell structure provided by the present invention, the first positive electrode plate and the second positive electrode plate are oxide positive electrodes or phosphate positive electrodes, and the first negative electrode plate is a silicon-based negative electrode or a graphite negative electrode.
[0014] The present invention also provides a three-electrode battery, comprising the above three-electrode battery cell structure.
[0015] The present invention also provides a method for monitoring the negative electrode potential of a three-electrode battery, which is applicable to the above three-electrode battery and comprises the following steps:
[0016] Step 1: plating lithium on one of the reference electrodes in the three-electrode battery cell structure through the second positive electrode sheet, and not plating lithium on the other reference electrodes;
[0017] Step 2: testing the potential difference between the reference electrode after lithium plating in step 1 and the first negative electrode plate, and monitoring the potential of the negative electrode of the battery cell to be tested;
[0018] Step 3: After the three-electrode battery is used for a period of time, the second reference electrode in the three-electrode battery structure is plated with lithium through the second positive electrode sheet, and the remaining reference electrodes are not plated with lithium;
[0019] Step 4: testing the potential difference between the reference electrode after lithium plating in step 3 and the first negative electrode plate, and monitoring the potential of the negative electrode of the battery cell to be tested;
[0020] Step 5: Using the methods in step 3 and step 4, perform potential tests on the negative electrode in the cell to be tested through the remaining reference electrodes in the three-electrode cell structure in turn, obtain the potential difference between the reference electrode and the first negative electrode plate, and monitor the potential of the negative electrode of the cell to be tested.
[0021] According to a method for monitoring the negative electrode potential of a three-electrode battery provided by the present invention, step 2 and step 4 include the following processes:
[0022] S1, constant current I 1c Charging, constant current charging condition I 1c ≤8C, the charging end condition is that the positive and negative electrode voltages V1≤4.6V, the charged three-electrode battery is left to stand for a certain time t1, t1≤12h; during the charging process, the potential difference between the reference electrode and the first negative electrode is monitored;
[0023] S2, discharging the three-electrode battery after standing still, with the discharge end condition being the lower limit voltage of the positive and negative electrode voltages, and standing still for a certain time t2, t2≤12h; during the discharge process, monitoring the potential difference between the reference electrode and the first negative electrode plate.
[0024] The present invention provides a three-electrode cell structure, a three-electrode battery and a method for monitoring the negative electrode potential. A reference cell with multiple reference electrodes is arranged outside the cell to be tested. By monitoring the potential difference between the negative electrode of the cell to be tested and the multiple reference electrodes at different stages, the negative electrode potential test is accurately completed to determine the lithium deposition at the negative electrode. Not only can the error caused by the reference electrode to the test accuracy be eliminated, so that the reference electrode has no effect on the electrochemical performance of the cell to be tested, but also the accuracy of the negative electrode reference voltage detection can be improved. By monitoring the negative electrode potential, the active lithium consumption in the battery can be quantitatively analyzed, which has important guiding significance for the design and development of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 is a cross-sectional schematic diagram of a three-electrode battery cell structure provided by the present invention;
[0027] Figure 2 is a schematic structural diagram of a three-electrode battery provided by the present invention;
[0028] Figure 3 It is a schematic diagram of implementation data of a specific embodiment of the negative electrode potential monitoring method provided by the present invention;
[0029] Figure 4 yes Figure 3 A magnified schematic diagram of part A.
[0030] Reference numerals:
[0031] 1. Outer shell; 2. First positive electrode plate; 3. First negative electrode plate; 4. Test cell diaphragm; 5. Second positive electrode plate; 6. Reference cell diaphragm; 7. Reference electrode; 8. First positive electrode tab; 9. First negative electrode tab; 10. Second positive electrode tab; 11. Reference tab. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] In the description of the embodiments of the present invention, it should be noted that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present invention and simplifying the description, and do not indicate or imply that the devices or elements referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limitations on the embodiments of the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.
[0034] In the description of the embodiments of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "connected" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the embodiments of the present invention can be understood according to specific circumstances.
[0035] In the embodiments of the present invention, unless otherwise clearly specified and limited, the first feature being "above" or "below" the second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, the first feature being "above", "above" and "above" the second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. The first feature being "below", "below" and "below" the second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0036] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the embodiment of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0037] The present invention provides a specific embodiment of a three-electrode battery cell structure, referring to Figure 1As shown, the three-electrode battery cell structure includes a shell 1, an electrolyte encapsulated inside the shell 1, and a battery cell to be tested composed of a first positive electrode plate 2, a first negative electrode plate 3 and a battery cell diaphragm 4 to be tested, and also includes a reference battery cell, the reference battery cell includes at least two reference electrodes 7, and the reference battery cell is encapsulated inside the shell 1 and is located outside the battery cell to be tested. In this embodiment, there are at least two reference electrodes 7, that is, there are multiple reference electrodes 7, and multiple reference electrodes can be formed to perform corresponding tests with the first negative electrode plate 3 respectively. Multiple reference electrodes can be plated with lithium at different stages, which can be used for negative electrode reference potential identification in long-cycle battery cycles, and improve the accuracy of negative electrode reference voltage detection. Moreover, since the reference electrode 7 is not between the positive and negative electrode plates, the lithium ion transfer between the positive and negative electrode plates will not be affected by the lithium ion concentration between the reference electrodes, and the electrochemical performance of the battery will not be affected.
[0038] This embodiment further refines the above three-electrode battery cell structure. In this embodiment, there are multiple first positive electrode sheets 2, first negative electrode sheets 3 and battery cell separators 4 to be tested. The first positive electrode sheets 2 and the second positive electrode sheets 5 are oxide positive electrodes or phosphate positive electrodes, the first negative electrode sheets 3 are silicon-based negative electrodes or graphite negative electrodes, and the reference battery cell separator 6 is a single-layer glue-coated separator or a double-layer glue-coated separator. The first positive electrode sheet 2, the battery cell separator 4 to be tested and the first negative electrode sheet 3 are stacked in sequence to form a laminated electrode group, and the stacking method is: shell 1-first positive electrode sheet 2-battery cell separator 4 to be tested-first negative electrode sheet 3-battery cell separator 4 to be tested-first positive electrode sheet 2-battery cell separator 4 to be tested-first negative electrode sheet 3-·······-first positive electrode sheet 2-battery cell separator 4 to be tested-first negative electrode sheet 3-battery cell separator 4 to be tested.
[0039] See also Figure 1 As shown, the reference cell is composed of a second positive electrode sheet 5, a reference cell diaphragm 6 and at least two reference electrodes 7. The reference cell diaphragm 6 wraps the second positive electrode sheet 5. The reference electrode 7 is located between the reference cell diaphragm 6 and the laminated electrode group, that is, immediately following the test cell diaphragm 4 at the bottom of the laminated electrode group, and downwards in the following order: test cell diaphragm 4 - reference electrode 7 - reference cell diaphragm 6 - second positive electrode sheet 5 - reference cell diaphragm 6 - shell 1. The first positive electrode sheet 2, the first negative electrode sheet 3, the second positive electrode sheet 5 and the reference electrode 7 respectively form a first positive electrode tab 8, a first negative electrode tab 9, a second positive electrode tab 10 and a reference tab 11 outside the shell 1. There are at least two reference tabs 11. Figure 2In the process of monitoring the negative electrode potential of the three-electrode battery, the first reference electrode ear is plated with lithium through the second positive electrode ear 10 for the first time, and the potential difference between the first reference electrode ear and the first negative electrode ear 9 is tested; after the battery is used for a period of time, the second reference electrode ear is plated with lithium through the second positive electrode ear 10, and the potential difference between the second reference electrode ear and the first negative electrode ear 9 is tested, and the cycle is repeated until the potential difference between the nth reference electrode ear and the first negative electrode ear 9 is finally tested.
[0040] In the above three-electrode cell structure, the reference electrode 7 can be, but is not limited to, copper wire, gold wire, nickel wire or tinned copper wire. This embodiment provides a specific embodiment of the reference electrode 7. In this embodiment, the reference electrode 7 is made of copper wire, the first end of which is a bare copper wire end, and the second end is an enameled copper wire end. The first end of the reference electrode 7 is located between the reference cell diaphragm 6 and the laminated electrode group, and the second end of the reference electrode 7 extends to the outside of the housing 1, and the second end is welded with a nickel strip to form a reference pole ear 11.
[0041] The present invention also provides a three-electrode battery, comprising the above three-electrode battery cell structure, see Figure 2 As shown, the assembled three-electrode battery is a square battery, with a first positive electrode tab 8 and a first negative electrode tab 9 on the left side of the square battery, a second positive electrode tab 10 on the right side of the square battery, and n reference tabs 11 at the bottom of the square battery.
[0042] The present invention also provides a method for monitoring the negative electrode potential of the three-electrode battery, comprising the following steps:
[0043] Step 1: lithium-plating one reference electrode 7 in the three-electrode cell structure through the second positive electrode plate 5, and the remaining reference electrodes 7 are not plated with lithium;
[0044] Step 2: testing the potential difference between the reference electrode 7 after lithium plating in step 1 and the first negative electrode plate 3, and monitoring the potential of the negative electrode of the battery cell to be tested;
[0045] Step 3: After the three-electrode battery is used for a period of time, the second reference electrode 7 in the three-electrode battery structure is plated with lithium through the second positive electrode plate 5, and the remaining reference electrodes 7 are not plated with lithium;
[0046] Step 4: testing the potential difference between the reference electrode 7 after lithium plating in step 3 and the first negative electrode plate 3, and monitoring the potential of the negative electrode of the battery cell to be tested;
[0047] Step 5: Using the methods in step 3 and step 4, perform potential tests on the negative electrode in the cell to be tested through the remaining reference electrodes 7 in the three-electrode cell structure in turn, obtain the potential difference between the reference electrode 7 and the first negative electrode plate 3, and monitor the potential of the negative electrode of the cell to be tested.
[0048] Among them, step 2 and step 4 include the following processes:
[0049] S1, constant current I 1c Charging, constant current charging condition I 1c ≤8C, the charging end condition is that the positive and negative electrode voltage V1≤4.6V, the charged three-electrode battery is left to stand for a certain time t1, t1≤12h; during the charging process, the potential difference between the reference electrode 7 and the first negative electrode plate 3 is monitored;
[0050] S2, discharge the three-electrode battery after standing, the discharge end condition is the lower limit voltage of the positive and negative electrode voltage discharge, stand for a certain time t2, t2≤12h; during the discharge process, monitor the potential difference between the reference electrode 7 and the first negative electrode plate 3.
[0051] Specifically, this embodiment provides a detailed negative electrode potential monitoring process of a three-electrode battery:
[0052] (1) Preparation process of the battery cell to be tested: The prepared soft-pack laminated three-electrode battery has a capacity of 2Ah, the negative electrode is a graphite negative electrode, the first negative electrode plate 3 is made of graphite, the length is 105mm, the width is 55mm, and the thickness is 0.1mm; the first positive electrode plate 2 and the second positive electrode plate 5 are 523NCM ternary positive electrodes, the length is 100mm, the width is 50mm, and the thickness is 0.1mm; the battery cell separator 4 in the battery cell to be tested is a porous polymer membrane purchased from ZTE New Materials Technology Co., Ltd.
[0053] (2) Reference cell preparation process: Wrap a single 30mm*30mm second positive electrode plate 5 with a reference cell diaphragm 6. Prepare two enameled copper wires with a diameter of 50um, and place one end of the enameled copper wire about 1.5cm in concentrated sulfuric acid to remove the paint layer on the surface, and obtain two reference electrodes 7 with a first end being a bare copper wire end and a second end being an enameled copper wire end, which serve as the first reference electrode and the second reference electrode of the reference cell; place the first end of the reference electrode 7 between the second positive electrode plate 5 wrapped with the reference cell diaphragm 6 and the cell to be tested, and guide the second end of the reference electrode 7 out of the outer shell 1, and weld a nickel strip on the second end to form a first reference pole ear and a second reference pole ear; then, package the cell to be tested, the reference cell, the outer shell 1 and the electrolyte according to the soft-pack laminated cell production process, as shown in the following figure. Figure 1 and Figure 2 shown.
[0054] (3) First reference electrode lithium plating process: Use a current of 100uA to plate lithium on the first reference electrode, and form a metallic lithium layer on the first end of the first reference electrode to obtain a reference battery cell.
[0055] (4) Negative electrode potential test:
[0056] At 25°C, the battery cell to be tested is charged at 0.5C with a cutoff condition of 4.2V and allowed to stand for 0.5h. At 25°C, it is discharged at 1 / 3C to 2.8V and allowed to stand for 0.5h. While charging, the potential change of the first reference electrode to the negative electrode (i.e., the first reference electrode tab to the first negative electrode tab 9) is monitored. When the potential difference between the first reference electrode tab and the first negative electrode tab 9 is positive, it indicates that lithium deposition at the negative electrode of the battery is normal and does not affect the continued use of the battery. When the potential difference between the first reference electrode tab and the first negative electrode tab 9 is negative, it indicates that lithium deposition at the negative electrode of the battery is serious, which has affected the electrochemical performance of the battery and is prone to safety problems.
[0057] (5) The battery cell to be tested is subjected to charge and discharge cycles at 25°C, 1C, 2.8-4.2V until the capacity retention rate reaches 80%. During the charge and discharge process, the potential change of the first reference electrode to the negative electrode is simultaneously monitored.
[0058] (6) If the potential difference between the first reference electrode and the negative electrode monitored in steps (4) and (5) is positive, it does not affect the use of the battery. After the battery is used for a period of time, the negative electrode of the battery can be monitored again and lithium plating can be performed for the second time. Second reference electrode lithium plating process: Use a current of 100uA to plate lithium on the second reference electrode, and a metal lithium layer is formed on the first end of the first reference electrode to obtain a reference battery cell.
[0059] (7) Repeat steps (4) and (5) to complete the negative electrode potential test.
[0060] The negative electrode potential monitoring process of the above-mentioned three-electrode battery describes a process in which the three-electrode battery has two reference electrodes. The three-electrode battery of the present invention has at least two reference electrodes, and can also have multiple reference electrodes. When the battery has multiple reference electrodes, the negative electrode potential is monitored with reference to the following specific implementation process.
[0061] This embodiment provides a negative electrode potential monitoring process of a three-electrode battery with three reference electrodes:
[0062] (1) The preparation process of the battery cell to be tested is the same as the above two reference electrode embodiments.
[0063] (2) The reference cell preparation process uses three reference electrodes, and the other steps are the same as the above two reference electrode embodiment.
[0064] (3) First reference electrode lithium plating process: Use a current of 100uA to plate lithium on the first reference electrode, and form a metal lithium layer on the first end of the first reference electrode to obtain a reference battery cell;
[0065] (4) Negative electrode potential test:
[0066] At 25°C, the battery cell to be tested is charged at 0.5C with a cutoff condition of 4.2V and allowed to stand for 0.5h. At 25°C, it is discharged at 1 / 3C to 2.8V and allowed to stand for 0.5h. While charging, the potential change of the first reference electrode to the negative electrode (i.e., the first reference electrode tab to the first negative electrode tab 9) is monitored. When the potential difference between the first reference electrode tab and the first negative electrode tab 9 is positive, it indicates that lithium deposition at the negative electrode of the battery is normal and does not affect the continued use of the battery. When the potential difference between the first reference electrode tab and the first negative electrode tab 9 is negative, it indicates that lithium deposition at the negative electrode of the battery is serious, which has affected the electrochemical performance of the battery and is prone to safety problems.
[0067] (5) The battery cell to be tested is subjected to charge and discharge cycles at 25°C, 1C, 2.8-4.2V until the capacity retention rate reaches 80%. During the charge and discharge process, the potential change of the first reference electrode to the negative electrode is simultaneously monitored.
[0068] (6) If the potential difference between the first reference electrode and the negative electrode monitored in steps (4) and (5) is positive, it does not affect the use of the battery. After the battery is used for a period of time, the negative electrode of the battery can be monitored again and lithium plating can be performed for the second time. Second reference electrode lithium plating process: Use a current of 100uA to plate lithium on the second reference electrode, and a metal lithium layer is formed on the first end of the first reference electrode to obtain a reference battery cell.
[0069] (7) Negative electrode potential test:
[0070] At 25°C, the battery cell to be tested is charged at 0.5C with a cutoff condition of 4.2V and allowed to stand for 0.5h. At 25°C, it is discharged at 1 / 3C to 2.8V and allowed to stand for 0.5h. While charging, the potential change of the second reference electrode to the negative electrode (i.e., the second reference electrode tab to the first negative electrode tab 9) is monitored. When the potential difference between the second reference electrode tab and the second negative electrode tab 9 is positive, it indicates that lithium deposition at the negative electrode of the battery is normal and does not affect the continued use of the battery. When the potential difference between the second reference electrode tab and the first negative electrode tab 9 is negative, it indicates that lithium deposition at the negative electrode of the battery is serious, which has affected the electrochemical performance of the battery and is prone to safety problems.
[0071] (8) The battery cell to be tested is subjected to charge and discharge cycles at 25°C, 1C, 2.8-4.2V until the capacity retention rate reaches 50%. During the charge and discharge process, the potential change of the first reference electrode relative to the negative electrode is simultaneously monitored.
[0072] (9) If the potential difference between the second reference electrode and the negative electrode monitored in steps (7) and (8) is positive, it does not affect the use of the battery. After the battery is used for a period of time, the negative electrode of the battery can be monitored again and lithium plating can be performed for the third time. The lithium plating process of the third reference electrode: a current of 100uA is used to plate lithium on the third reference electrode, and a metal lithium layer is formed on the first end of the first reference electrode to obtain a reference battery cell.
[0073] (10) Negative electrode potential test: Repeat steps (7) and (8) to complete the negative electrode potential test.
[0074] Compared with the embodiment with two reference electrodes, there are three reference electrodes in the reference cell in this embodiment. When the cells to be tested are in the same state, the negative reference potentials in the cells to be tested are substantially the same under the same conditions.
[0075] In order to accurately reflect the accuracy of the three-electrode battery of the present invention in monitoring the negative electrode potential, the present invention provides a comparative embodiment for comparison with the above two embodiments, that is, a three-electrode battery with a reference electrode is used for experimental comparison, as follows:
[0076] (1) The preparation process of the battery cell to be tested is the same as the above two embodiments.
[0077] (2) In the reference cell preparation process, one reference electrode is used, and the other steps are the same as those in the above two embodiments.
[0078] (3) First reference electrode lithium plating process: Use a current of 100uA to plate lithium on the first reference electrode, and form a metallic lithium layer on the first end of the first reference electrode to obtain a reference battery cell.
[0079] (4) Negative electrode potential test:
[0080] At 25°C, the battery cell to be tested is charged at 0.5C with a cutoff condition of 4.2V and allowed to stand for 0.5h. At 25°C, it is discharged at 1 / 3C to 2.8V and allowed to stand for 0.5h. While charging, the potential change of the first reference electrode to the negative electrode (i.e., the first reference electrode tab to the first negative electrode tab 9) is monitored. When the potential difference between the first reference electrode tab and the first negative electrode tab 9 is positive, it indicates that lithium deposition at the negative electrode of the battery is normal and does not affect the continued use of the battery. When the potential difference between the first reference electrode tab and the first negative electrode tab 9 is negative, it indicates that lithium deposition at the negative electrode of the battery is serious, which has affected the electrochemical performance of the battery and is prone to safety problems.
[0081] (5) The battery cell to be tested is subjected to charge and discharge cycles at 25°C, 1C, 2.8-4.2V until the capacity retention rate reaches 80%. During the charge and discharge process, the potential change of the first reference electrode to the negative electrode is simultaneously monitored.
[0082] (6) If the potential difference between the first reference electrode and the negative electrode monitored in steps (4) and (5) is positive, it does not affect the use of the battery. After the battery is used for a period of time, the negative electrode of the battery is monitored again. Negative electrode potential test: At 25°C, the battery cell to be tested is charged at 0.5C, with a cutoff condition of 4.2V, and allowed to stand for 0.5h; at 25°C, 1 / 3C is discharged to 2.8V, and allowed to stand for 0.5h. While charging, the potential change of the first reference electrode to the negative electrode (i.e., the first reference electrode tab to the first negative electrode tab 9) is monitored.
[0083] The experimental results of the above three embodiments are as follows: Figure 3 As shown, from Figure 3 Combination Figure 4 It can be seen that the potentials of the negative electrode and the reference electrode are monitored in the early stage of the three-electrode battery, and the three curves in the three embodiments are completely consistent, indicating that the reference electrode in the three embodiments has good reproducibility. However, after a certain period of use (the capacity retention rate drops from 100% to 80%), when the negative electrode potential is monitored again, it is found that the potentials in the comparative embodiments are lower than those in the two embodiments of the present invention (the negative electrode potential in the three-electrode battery with two reference electrodes and the three-electrode battery with three reference electrodes is very reproducible), indicating that the stability of the reference electrode in the comparative embodiment is reduced, resulting in inaccurate detection of the negative electrode potential after long-cycle testing. However, the negative electrode potential in the three-electrode battery with two reference electrodes and the three-electrode battery with three reference electrodes of the present invention is very reproducible, further illustrating that the three-electrode cell structure, three-electrode battery and negative electrode potential monitoring method provided by the present invention can effectively improve the accuracy of negative electrode potential monitoring after a long period of use of the three-electrode battery.
[0084] In addition, the negative electrode potential monitoring method of the present invention can quantitatively analyze the active lithium consumption in the battery, that is, it can detect the boundary conditions of lithium precipitation, which has important guiding significance for the design and development of the battery, and can be used in the battery management system to provide a fast charging strategy for the management system. On the one hand, the positive and negative electrode capacity ratio of the battery can be designed based on this, and on the other hand, the negative electrode can be pre-lithiated in advance according to the actual failure mechanism analysis, so as to further improve the cycle life of the battery and avoid the subsequent use of the battery due to insufficient or excessive lithium replenishment of the negative electrode plate during the battery preparation process. The negative electrode potential monitoring method of the present invention has a simple process and a high degree of accuracy.
[0085] In summary, the three-electrode cell structure, three-electrode battery and negative electrode potential monitoring method provided by the present invention have multiple advantages:
[0086] (1) In the three-electrode cell structure and the three-electrode battery of the present invention, n (n≥2) reference electrodes can be designed in the reference cell, and the reference cells are all located outside the cell to be tested, and have no effect on the electrochemical performance of the cell to be tested.
[0087] (2) The three-electrode cell structure and the three-electrode battery of the present invention can be plated with lithium at different stages, and can be used to identify the negative electrode reference potential during long-term cycle use of the battery, thereby improving the accuracy of negative electrode reference voltage detection.
[0088] (3) The lithium plating boundary conditions detected by the negative electrode potential monitoring method provided by the present invention can be used in a battery management system to provide a fast charging strategy for the management system, thereby reducing the possibility of lithium plating in the battery and improving the safety of the battery.
[0089] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A three-electrode cell structure, comprising a housing (1), an electrolyte encapsulated in the housing (1), and a cell to be tested consisting of a first positive electrode sheet (2), a first negative electrode sheet (3) and a cell to be tested separator (4), characterized in that: Also included is a reference cell, which is encapsulated inside the housing (1) and located outside the cell to be tested; There are a plurality of the first positive electrode sheet (2), the first negative electrode sheet (3) and the battery cell separator (4) to be tested, respectively; the first positive electrode sheet (2), the battery cell separator (4) to be tested and the first negative electrode sheet (3) are stacked in sequence to form a stacked electrode group; The reference cell is composed of a second positive electrode sheet (5), a reference cell separator (6) and n reference electrodes (7), wherein n is an integer not less than 2, the reference cell separator (6) wraps the second positive electrode sheet (5), the reference electrode (7) is located between the reference cell separator (6) and the laminated electrode group, and the reference electrode (7) is a copper wire, a gold wire, a nickel wire or a tinned copper wire; The first positive electrode sheet (2), the first negative electrode sheet (3), the second positive electrode sheet (5) and the reference electrode (7) respectively form a first positive electrode tab (8), a first negative electrode tab (9), a second positive electrode tab (10) and n reference tabs (11) outside the housing (1), wherein there are at least two reference tabs (11); During the negative electrode potential monitoring process of the three-electrode battery, the first reference electrode tab (11) is plated with lithium through the second positive electrode tab (10) for the first time, and the potential difference between the first reference electrode tab (11) and the first negative electrode tab (9) is tested; after the battery is used for a period of time, the second reference electrode tab (11) is plated with lithium through the second positive electrode tab (10), and the potential difference between the second reference electrode tab (11) and the first negative electrode tab (9) is tested, and the cycle is repeated until the potential difference between the nth reference electrode tab (11) and the first negative electrode tab (9) is finally tested.
2. A three-electrode battery cell structure according to claim 1, characterized in that: The reference electrode (7) is made of copper wire, the first end of which is a bare copper wire end, and the second end of which is an enameled copper wire end. The first end of the reference electrode (7) is located between the reference cell diaphragm (6) and the laminated electrode group, and the second end of the reference electrode (7) extends to the outside of the housing (1). A nickel strip is welded to the second end to form the reference electrode ear (11).
3. A three-electrode battery cell structure according to claim 1, characterized in that: The reference battery cell diaphragm (6) is a single-layer glue-coated diaphragm or a double-layer glue-coated diaphragm.
4. A three-electrode battery cell structure according to claim 1, characterized in that: The first positive electrode plate (2) and the second positive electrode plate (5) are oxide positive electrodes or phosphate positive electrodes, and the first negative electrode plate (3) is a silicon-based negative electrode or a graphite negative electrode.
5. A three-electrode battery, characterized in that: A three-electrode battery cell structure comprising any one of claims 1 to 4.
6. A method for monitoring the negative electrode potential of a three-electrode battery, characterized in that: The three-electrode battery according to claim 5 comprises the following steps: Step 1: lithium-plating is performed on one of the reference electrodes (7) in the three-electrode battery cell structure through the second positive electrode plate (5), and the remaining reference electrodes (7) are not plated with lithium; Step 2: testing the potential difference between the reference electrode (7) after lithium plating in step 1 and the first negative electrode plate (3), and monitoring the potential of the negative electrode of the battery cell to be tested; Step 3: After the three-electrode battery has been used for a period of time, the second reference electrode (7) in the three-electrode battery cell structure is plated with lithium through the second positive electrode plate (5), and the remaining reference electrodes (7) are not plated with lithium; Step 4: testing the potential difference between the reference electrode (7) after lithium plating in step 3 and the first negative electrode plate (3), and monitoring the potential of the negative electrode of the battery cell to be tested; Step 5: Using the methods in step 3 and step 4, the remaining reference electrodes (7) in the three-electrode cell structure are used to perform potential tests on the negative electrode in the cell to be tested, and the potential difference between the reference electrode (7) and the first negative electrode plate (3) is obtained, so as to monitor the potential of the negative electrode of the cell to be tested.
7. The method for monitoring the negative electrode potential of a three-electrode battery according to claim 6, characterized in that: The steps 2 and 4 include the following processes: S1, constant current for the cell to be tested Charging, constant current charging conditions , the charging end condition is the positive and negative voltage , let the charged three-electrode battery stand for a certain period of time , During the charging process, the potential difference between the reference electrode (7) and the first negative electrode (3) is monitored; S2, discharge the three-electrode battery after standing still, the discharge end condition is the lower limit voltage of the positive and negative electrode voltage discharge, and stand still for a certain period of time During the discharge process, the potential difference between the reference electrode (7) and the first negative electrode plate (3) is monitored.