A kind of X-type molecular sieve and preparation method thereof

Through the methods of aging and second-stage crystallization, the packing density of X-type molecular sieve is improved, which solves the problem of insufficient packing density in the existing technology, realizes the improvement of equipment filling rate and the recycling of raw materials, and is suitable for industrial applications.

CN116216737BActive Publication Date: 2024-10-22CHALCO SHANDONG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310080301.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-31
Publication Date
2024-10-22
Estimated Expiration
2043-01-31

AI Technical Summary

Technical Problem

In the existing technology, the X-type molecular sieve has a low packing density, which results in insufficient equipment loading and reduces equipment utilization.

Method used

Using aging and two-stage crystallization methods, by mixing silicon sources and aluminum sources, a silica-alumina gel is formed, and combined with a crystal orientation agent, gel-forming and aging are performed, and finally two crystallizations are performed to prepare a silicon-alumina gel with large X-type molecular sieve with single crystal particle size and high packing density.

Benefits of technology

It increases the packing density of the X-type molecular sieve, improves the equipment filling rate, improves economic benefits, and realizes the recycling of raw material mother liquor. It is suitable for industrial production, is environmentally friendly, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116216737B_ABST
    Figure CN116216737B_ABST
Patent Text Reader

Abstract

The present application relates to an X-type molecular sieve and a preparation method thereof, belonging to the technical field of molecular sieves; the method comprises: obtaining a seed orienting agent; mixing a silicon source and an aluminum source to obtain a silica-alumina gel; mixing the silica-alumina gel and the seed orienting agent, and then performing a gelling treatment to obtain a colloid; mixing the colloid and the seed orienting agent, and then performing aging and a first crystallization to obtain an intermediate slurry; adding the aluminum source to the intermediate slurry, and then performing a second crystallization to obtain an X-type molecular sieve; by combining aging and two-stage crystallization (i.e., the first crystallization and the second crystallization), the single crystal particle size of the prepared X-type molecular sieve is 3-6 microns, and the bulk density is greater than 0.7g / ml, which effectively improves the packing density of the X-type molecular sieve, thereby achieving an improvement in the equipment filling rate and the equipment utilization rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of molecular sieves, and in particular to an X-type molecular sieve and a preparation method thereof. Background Art

[0002] X-type molecular sieve has a wide range of industrial applications due to its specific structure, such as gas drying, adsorption separation and purification of air separation gases, and treatment of wastewater contaminated by heavy metals.

[0003] At present, the X-type molecular sieve is synthesized by hydrothermal method in China, mostly with the technology of directing agent, which can synthesize X-type molecular sieve with stable quality. However, after using the directing agent, the molecular sieve D50 is generally 1-3 microns, but the crystal particle size is much smaller than this particle size, and the crystal agglomeration phenomenon is serious. The crystal grains become smaller and the bulk density is low. This kind of powder is used for molding, and the bulk density of the product is relatively low, which is 0.55-0.63g / ml. In industrial applications, it cannot meet the equipment's requirements for the loading amount of molecular sieve, thereby reducing the utilization rate of the equipment. Summary of the invention

[0004] The present application provides an X-type molecular sieve and a preparation method thereof, so as to improve the problem that the current X-type molecular sieve has low packing density.

[0005] In a first aspect, the present application provides a method for preparing an X-type molecular sieve, the method comprising:

[0006] obtaining a seed crystal directing agent;

[0007] Mixing a silicon source and an aluminum source to obtain a silicon-aluminum gel;

[0008] The silica-alumina gel and the seed crystal directing agent are mixed, and then subjected to a gelling treatment to obtain a colloid;

[0009] The colloid and the seed crystal directing agent are mixed, and then aged and first crystallized to obtain an intermediate slurry;

[0010] The aluminum source is added to the intermediate slurry, and then a second crystallization is performed to obtain an X-type molecular sieve.

[0011] As an optional embodiment, the step of obtaining the seed crystal directing agent specifically includes:

[0012] Sodium hydroxide, water, sodium aluminate and water glass are mixed, and then statically aged to obtain a seed crystal orientation agent;

[0013] Wherein, sodium hydroxide, water, sodium aluminate and water glass are mixed according to the molar ratio of Na2O:Al2O3:SiO2:H2O of (15-20):1:(15-23):(260-400);

[0014] The static aging temperature is 30-50°C;

[0015] The static aging time is 1-7 days.

[0016] As an optional embodiment, the silicon source and the aluminum source are mixed according to a molar ratio of Na2O:Al2O3:SiO2:H2O of (2.5-3.5):1:(2.5-3.2):(150-300).

[0017] As an optional embodiment, in the mixture of the silica-alumina gel and the seed orienting agent, the volume addition amount of the seed orienting agent accounts for 1-100 ppm of the volume of the mixture.

[0018] As an optional embodiment, the temperature of the gelling treatment is 30-50°C.

[0019] As an optional embodiment, the aging temperature is 50-75°C; and / or

[0020] The aging time is 1-5h.

[0021] As an optional embodiment, the temperature of the first crystallization is 90-105° C.; and / or

[0022] The first crystallization time is 8-20 hours.

[0023] As an optional implementation, the added amount of the aluminum source accounts for 20%-40% of the mass of the aluminum oxide in the intermediate slurry.

[0024] As an optional embodiment, the temperature of the second crystallization is 90-105° C.; and / or

[0025] The second crystallization time is 1-3 hours.

[0026] In a second aspect, the present application provides an X-type molecular sieve, wherein the X-type molecular sieve is prepared by the preparation method of the X-type molecular sieve described in the first aspect.

[0027] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0028] The method provided in the embodiment of the present application combines aging and two-stage crystallization (i.e., the first crystallization and the second crystallization) to prepare a single crystal particle size of the X-type molecular sieve of 3-6 microns and a bulk density greater than 0.7 g / ml, which effectively improves the packing density of the X-type molecular sieve, thereby achieving an improvement in the equipment filling rate and equipment utilization rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0030] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0031] Figure 1 This is a scanning electron microscope (SEM) image of the X-type molecular sieve provided in Example 1 of the present application;

[0032] Figure 2 The XRD spectrum of the X-type molecular sieve provided in Example 1 of the present application;

[0033] Figure 3 A flowchart of a method provided in an embodiment of the present application. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0035] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0036] X-type molecular sieve has a wide range of industrial applications due to its specific structure, such as gas drying, adsorption separation and purification of air separation gases, and treatment of wastewater contaminated by heavy metals.

[0037] At present, the X-type molecular sieve is synthesized by hydrothermal method in China, mostly with the technology of directing agent, which can synthesize X-type molecular sieve with stable quality. However, after using the directing agent, the molecular sieve D50 is generally 1-3 microns, but the crystal particle size is much smaller than this particle size, and the crystal agglomeration phenomenon is serious. The crystal grains become smaller and the bulk density is low. This kind of powder is used for molding, and the bulk density of the product is relatively low, which is 0.55-0.63g / ml. In industrial applications, it cannot meet the equipment's requirements for the loading amount of molecular sieve, thereby reducing the utilization rate of the equipment.

[0038] The research of UOP in the United States on X-type molecular sieve is only conventional research, and the bulk density of its products is between 0.60-0.63g / ml. Increasing the crystal particle size of X-type molecular sieve and the bulk density of powder can increase the bulk density of formed molecular sieve and improve the utilization rate of filling equipment.

[0039] like Figure 3 As shown, the present application embodiment provides a method for preparing an X-type molecular sieve, the method comprising:

[0040] S1. Obtaining a seed crystal directing agent;

[0041] In some embodiments, the step of obtaining a seed crystal directing agent specifically comprises:

[0042] Sodium hydroxide, water, sodium aluminate and water glass are mixed, and then statically aged to obtain a seed crystal orientation agent;

[0043] Wherein, sodium hydroxide, water, sodium aluminate and water glass are mixed according to the molar ratio of Na2O:Al2O3:SiO2:H2O of (15-20):1:(15-23):(260-400);

[0044] The static aging temperature is 30-50°C;

[0045] The static aging time is 1-7 days.

[0046] Specifically, in this embodiment, sodium hydroxide, water, sodium aluminate and water glass are mixed evenly according to the molar ratio of (15-20) Na2O: Al2O3: (15-23) SiO2: (260-400) H2O, and statically aged at 30-50°C for 1-7 days to obtain a seed crystal orientation agent. In this step, the concentration of silicon in the water glass solution is 220-250g / L, and the modulus is 2.8-3.2. The concentration of aluminum oxide in the sodium aluminate solution is 35-45g / L, and the caustic coefficient is 10-14. The alkali source is liquid sodium hydroxide or evaporation concentrated mother liquor.

[0047] S2. mixing the silicon source and the aluminum source to obtain a silicon-aluminum gel;

[0048] In some embodiments, the silicon source and the aluminum source are mixed according to the molar ratio of Na2O:Al2O3:SiO2:H2O of (2.5-3.5):1:(2.5-3.2):(150-300). The silicon source is a mother liquor for water glass, and water is adjusted to a fixed concentration; the aluminum source is aluminum hydroxide, sodium hydroxide, water, and a mother liquor adjusted to a fixed concentration. In this step, the concentration of silicon in the water glass solution is 110-130 g / L, and the modulus is 2.8-3.2. The concentration of aluminum oxide in the sodium aluminate solution is 45-55 g / L, and the caustic coefficient is 1.8-2.3. The alkali source is liquid sodium hydroxide or evaporation concentrated mother liquor.

[0049] Specifically, in this embodiment, the aluminum source and the silicon source are stirred according to the molar ratio of (2.5-3.5) Na2O:Al2O3:(2.5-3.2) SiO2:(150-300) H2O to synthesize silica-alumina gel.

[0050] S3. The silica-alumina gel and the seed crystal directing agent are mixed, and then subjected to a gelling treatment to obtain a colloid;

[0051] In some embodiments, in the mixture of the silica-alumina gel and the seed directing agent, the volume addition amount of the seed directing agent accounts for 1-100 ppm of the volume of the mixture.

[0052] In some embodiments, the temperature of the gelling treatment is 30-50°C.

[0053] Specifically, in this embodiment, a seed orienting agent is added to the silica-alumina gel, wherein the amount of the seed orienting agent added accounts for 1-100 ppm of the volume of the final synthetic mixture; then, under stirring conditions, the silicon source and the aluminum source are simultaneously added to the reactor at a designed flow rate, and the gelation temperature is controlled to be 30-50°C; continuous gelation is carried out to obtain a colloid.

[0054] S4. The colloid and the seed crystal directing agent are mixed, and then aged and first crystallized to obtain an intermediate slurry;

[0055] In some embodiments, the aging temperature is 50-75° C.; the aging time is 1-5 h.

[0056] In some embodiments, the temperature of the first crystallization is 90-105° C.; the time of the first crystallization is 8-20 hours.

[0057] Specifically, in this embodiment, the continuously gelled colloid is continuously fed into a crystallization tank, a seed orienting agent is added to the crystallization tank, and the mixture is stirred for 30 to 60 minutes. Then, high-pressure steam is introduced to raise the system temperature to 50 to 75°C, stirring is stopped, and aging is performed for 1 to 5 hours. After aging, stirring is started, and high-pressure steam is introduced again to raise the system temperature to 90 to 105°C, and static crystallization is performed for 8 to 20 hours.

[0058] S5. Add the aluminum source into the intermediate slurry, and then perform a second crystallization to obtain an X-type molecular sieve.

[0059] In some embodiments, the added amount of the aluminum source accounts for 20%-40% of the mass of the aluminum oxide in the intermediate slurry.

[0060] In some embodiments, the temperature of the second crystallization is 90-105° C.; the time of the second crystallization is 1-3 hours.

[0061] Specifically, in this embodiment, after the first crystallization is completed, stirring is started, and an aluminum source is added, the amount of aluminum source added accounts for 20-40% of the mass fraction of aluminum oxide in the solution, and the temperature is kept unchanged for static crystallization for 1-3 hours; after the second crystallization is completed, stirring is started, and the slurry is separated into solid molecular sieve crystals and mother liquor by a vertical filter press, and the solid product is washed with water to pH = 10-11, and dried at 150-200 ° C to obtain a molecular sieve raw powder product with a particle size of 3-6 microns and a bulk density of 0.7g / ml. The mother liquor is used to prepare water glass and sodium aluminate solution.

[0062] The method combines aging and two-stage crystallization (i.e., the first crystallization and the second crystallization) to prepare an X-type molecular sieve having the characteristics of large crystal grains, high bulk density, and large adsorption capacity. The single crystal particle size is 3-6 microns, the bulk density is greater than 0.7g / ml, and the static saturated water adsorption is greater than 33.5% at 35°C and 50% relative humidity. The X-type molecular sieve packing density is effectively improved, more molecular sieves can be loaded in a limited volume, and the economic benefits and equipment utilization rate are improved. At the same time, through the two-stage crystallization, the recycling of the raw material mother liquor is realized, which is suitable for industrialization, environmentally friendly, and cost-reduced.

[0063] Based on a general inventive concept, an embodiment of the present application further provides an X-type molecular sieve, wherein the X-type molecular sieve is prepared by the preparation method of the X-type molecular sieve as described above.

[0064] The X-type molecular sieve is prepared based on the above method. The specific steps of the method can refer to the above embodiment. Since the X-type molecular sieve adopts part or all of the technical solutions of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment, which will not be described one by one here.

[0065] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0066] Example 1

[0067] A method for preparing an X-type molecular sieve, the method comprising:

[0068] 1) Take silicon source and aluminum source in a molar ratio of 20Na2O:Al2O3:23SiO2:400H2O, add them into the reactor in sequence under stirring, stir at room temperature for 2 hours, and let stand at 40°C for 2-7 days to obtain seed crystals.

[0069] 2) According to the molar ratio of 3.0Na2O:Al2O3:3.0SiO2:180H2O, according to the set flow rate of aluminum source (AO 55g / l, caustic coefficient 2.0) and silicon source (SiO2120g / l, modulus 2.9), add to the reactor simultaneously under stirring, control the temperature at 40°C, immediately move into the crystallization tank, add 5ppm seed crystal directing agent in the crystallization tank, stir for 0.5 hours, pass high pressure steam to raise the temperature for aging, the temperature is 65°C, control the grains to be uniform, the aging time is 2 hours, pass high pressure steam to raise the temperature to the crystallization temperature and stop stirring, the temperature is controlled at 99°C, the first crystallization time is 15 hours; stir the crystallization liquid, add 30% sodium aluminate solution (aluminum source is the same as above, accounting for the mass fraction of the feed aluminum oxide) to the solution for second stage crystallization, the temperature is controlled at 99°C, and the second stage crystallization time is 1 hour. Separation, washing and drying, separation is to separate the solid and liquid by a vertical filter press after the crystallization is completed, and the mother liquor is recycled. Washing: Wash with water on a filter press until the pH value is 10-11, and dry with a flash dryer to obtain a large-grain X-type molecular sieve.

[0070] Example 2

[0071] A method for preparing an X-type molecular sieve, the method comprising:

[0072] 1) The orienting agent was prepared according to the method of Example 1, except that the standing temperature was 35°C.

[0073] 2) According to the molar ratio of 3.3Na2O:Al2O3:3.0SiO2:180H2O, according to the set flow rate of aluminum source (AO 53g / l, caustic coefficient 2.0) and silicon source (SiO2110g / l, modulus 2.9), add to the reactor simultaneously under stirring, control the temperature at 45°C, immediately move into the crystallization tank, add 3ppm seed crystal directing agent in the crystallization tank, stir for 0.5 hours, pass high pressure steam to raise the temperature for aging, the temperature is 60°C, control the grains to be uniform, the aging time is 5 hours, pass high pressure steam to raise the temperature to the crystallization temperature and stop stirring, the temperature is controlled at 98°C, the first crystallization time is 13 hours; stir the crystallization liquid, add 30% sodium aluminate solution (aluminum source is the same as above, accounting for the mass fraction of the feed aluminum oxide) to the solution for second stage crystallization, the temperature is controlled at 98°C, and the second stage crystallization time is 1 hour. Separation, washing and drying, separation is to separate the solid and liquid by a vertical filter press after the crystallization is completed, and the mother liquor is recycled. Washing: Wash with water on a filter press until the pH value is 10-11, and dry with a flash dryer to obtain a large-grain X-type molecular sieve.

[0074] Example 3

[0075] A method for preparing an X-type molecular sieve, the method comprising:

[0076] 1) A seed crystal orienting agent was prepared according to the method of Example 1, except that the standing temperature was 45°C.

[0077] 2) Molar ratio of 2.8Na2O:Al2O3:3.0SiO2:182H2O SiO2 / Al2O3=3.0, Na2O / Al2O3=2.8, H2O / Na2O=65, design aluminum source (AO 50g / l, caustic coefficient 1.9) and silicon source (SiO2120g / l, modulus 3.2), add them into the reactor simultaneously under stirring, control the temperature at 40°C, immediately move them into the crystallization tank, add 10ppm seed crystal directing agent into the crystallization tank, stir for 0.5 hour, pass high pressure steam to raise the temperature for aging, the temperature is 65°C, control the grains to be uniform, the aging time is 3 hours, pass high pressure steam to raise the temperature to the crystallization temperature and stop stirring, the temperature is controlled at 98°C, and the first crystallization time is 10 hours; stir the crystallization solution, add 30% sodium aluminate solution (accounting for the mass fraction of the charged alumina) into the solution for second stage crystallization, the temperature is controlled at 98°C, and the second stage crystallization time is 1.5 hours. Separation, washing and drying: after crystallization is completed, the solid-liquid separation is carried out by using a vertical filter press, and the mother liquor is recycled. Washing is done by washing with water on the filter press until the pH value is 10-11, and drying is done by using a flash dryer; the original powder of large-grain X-type molecular sieve is obtained.

[0078] Comparative Example 1

[0079] A method for preparing an X-type molecular sieve, the method comprising:

[0080] 1) Take silicon source and aluminum source in a molar ratio of 20Na2O:Al2O3:23SiO2:400H2O, add them into the reactor in sequence under stirring, stir at room temperature for 2 hours, and let stand at 40°C for 2-7 days to obtain seed crystals.

[0081] 2) According to the molar ratio of 3.0Na2O:Al2O3:3.0SiO2:180H2O, according to the set flow rate of aluminum source (AO 55g / l, caustic coefficient 2.0) and silicon source (SiO2120g / l, modulus 2.9), add to the reactor simultaneously under stirring, control the temperature at 40°C, immediately move into the crystallization tank, add 5ppm seed crystal directing agent in the crystallization tank, stir for 0.5 hours, pass high pressure steam to raise the temperature for aging, the temperature is 65°C, control the grains to be uniform, the aging time is 2 hours, pass high pressure steam to raise the temperature to the crystallization temperature and stop stirring, the temperature is controlled at 80°C, the first crystallization time is 15 hours; stir the crystallization liquid, add 30% sodium aluminate solution (aluminum source is the same as above, accounting for the mass fraction of the feed aluminum oxide) to the solution for second stage crystallization, the temperature is controlled at 80°C, and the second stage crystallization time is 1 hour. Separation, washing and drying, separation is to separate the solid and liquid by a vertical filter press after the crystallization is completed, and the mother liquor is recycled. Washing: Wash with water on a filter press until the pH value is 10-11, and dry with a flash dryer to obtain a large-grain X-type molecular sieve.

[0082] Comparative Example 2

[0083] A method for preparing an X-type molecular sieve, the method comprising:

[0084] 1) Take silicon source and aluminum source in a molar ratio of 20Na2O:Al2O3:23SiO2:400H2O, add them into the reactor in sequence under stirring, stir at room temperature for 2 hours, and let stand at 40°C for 2-7 days to obtain seed crystals.

[0085] 2) According to the molar ratio of 3.0Na2O:Al2O3:3.0SiO2:180H2O, according to the set flow rate of aluminum source (AO 55g / l, caustic coefficient 2.0) and silicon source (SiO2120g / l, modulus 2.9), add to the reactor simultaneously under stirring, control the temperature at 40°C, immediately move into the crystallization tank, add 5ppm seed crystal directing agent in the crystallization tank, stir for 0.5 hours, pass high pressure steam to age at 65°C, control the grains to be uniform, age for 2 hours, pass high pressure steam to the crystallization temperature and stop stirring, control the temperature at 110°C, the first crystallization time is 15 hours; stir the crystallization liquid, add 30% sodium aluminate solution (aluminum source is the same as above, accounting for the mass fraction of the feed aluminum oxide) to the solution for second stage crystallization, control the temperature at 110°C, the second stage crystallization time is 1 hour. Separation, washing and drying, separation is to separate the solid and liquid by vertical filter press after the crystallization is completed, and the mother liquor is recycled. Washing: Wash with water on a filter press until the pH value is 10-11, and dry with a flash dryer to obtain a large-grain X-type molecular sieve.

[0086] The X-type molecular sieves provided in Example 1-3 and Comparative Example 1-2 were tested, and the results are shown in the following table:

[0087]

[0088]

[0089] It can be seen from the above table that the single crystal particle size of the X-type molecular sieve prepared by the method provided in the embodiment of the present application is above 3 μm, the bulk density is greater than 0.7 g / ml, and the static saturated water adsorption is greater than 33.5% at 35°C and 50% relative humidity.

[0090] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0091] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.

[0092] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for preparing an X-type molecular sieve, characterized in that: The method comprises: obtaining a seed crystal directing agent; Mixing a silicon source and an aluminum source to obtain a silicon-aluminum gel; The silica-alumina gel and the seed crystal directing agent are mixed, and then subjected to a gelling treatment to obtain a colloid; The colloid and the seed crystal directing agent are mixed, and then aged and first crystallized to obtain an intermediate slurry; Adding the aluminum source into the intermediate slurry, and then performing a second crystallization to obtain an X-type molecular sieve; The method of obtaining the seed crystal directing agent specifically comprises: Sodium hydroxide, water, sodium aluminate and water glass are mixed, and then statically aged to obtain a seed crystal orientation agent; Wherein, sodium hydroxide, water, sodium aluminate and water glass are mixed according to the molar ratio of Na2O:Al2O3:SiO2:H2O of (15-20):1:(15-23):(260-400); The static aging temperature is 30-50°C; The static aging time is 1-7 days; The temperature of the gelling treatment is 30-50°C, and the temperature of the aging treatment is 50-75°C. The temperature of the first crystallization is 90-105° C., and the time of the first crystallization is 8-20 hours; The amount of the aluminum source added is 20%-40% of the mass of the aluminum oxide in the intermediate slurry; The temperature of the second crystallization is 90-105° C., and the time of the second crystallization is 1-3 hours; The single crystal particle size of the X-type molecular sieve is 3-6 microns, and the bulk density is greater than 0.7 g / ml; The silicon source and the aluminum source are mixed according to the molar ratio of Na2O:Al2O3:SiO2:H2O of (2.5-3.5):1:(2.5-3.2):(150-300).

2. The method for preparing type X molecular sieve according to claim 1, characterized in that: In the mixture of the silica-alumina gel and the seed orienting agent, the volume addition amount of the seed orienting agent accounts for 1-100 ppm of the volume of the mixture.

3. The method for preparing type X molecular sieve according to claim 1, characterized in that: The aging time is 1-5h.

4. An X-type molecular sieve, characterized in that The X-type molecular sieve is prepared by the preparation method of the X-type molecular sieve according to any one of claims 1 to 3.