Flexible conductive hydrogel and its preparation method and application
Through the combination of hydrogen bond monomer, conductive filler material and photoinitiator, flexible conductive hydrogel with high ductility and high conductivity is formed, which solves the problem of insufficient mechanical strength and sensitivity of existing hydrogel sensors and achieves high strength , low modulus and wide linear range effects improve the performance of hydrogel sensors.
Patent Information
- Application Number
- CN202211588864.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-09
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-12-09
AI Technical Summary
Existing flexible hydrogel sensors have low mechanical strength, poor ductility, low sensitivity and low linear range, making it difficult to meet the performance requirements of wearable strain sensors at the same time.
Using a combination of hydrogen bond monomer, conductive filler material and photoinitiator, a flexible conductive hydrogel with high ductility and high conductivity is formed through hydrogen bonding and organic-inorganic complexing, and excellent results are obtained through ultraviolet curing preparation method. Hydrogels with mechanical properties and electrical conductivity.
The flexible conductive hydrogel is achieved with high strength, low modulus, good adhesion performance, high conductivity, high sensitivity and wide linear range, and the sensitivity and accuracy of the hydrogel strain sensor are improved.
Smart Images

Figure CN116217972B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of conductive hydrogels, and in particular to flexible conductive hydrogels and a preparation method and application thereof. Background Art
[0002] Flexible and stretchable electronic products usually refer to a type of electronic products that can still maintain normal operation under a certain range of mechanical deformation conditions, such as bending, folding, twisting, compression, stretching, etc. These electronic products can not only meet the requirements of bending, folding, twisting, compression, and stretching, but also have the ability to deform into any shape, which has greatly promoted the development of products such as flexible sensors, foldable displays, electronic skin, smart clothing, stretchable solar cells, and elastomeric actuators. Flexible wearable strain sensors with high ductility and high sensitivity have great application potential and application value in real-time monitoring of human health, intelligent human-computer interaction, flexible robots, and artificial electronic skin. By attaching flexible wearable strain sensors to clothing or directly applying them to the surface of human skin, real-time monitoring of individual physiological health signals such as pulse, blood pressure, and respiration can be achieved, and the data can be transmitted to medical service equipment and institutions to help doctors or family members make timely judgments on the health status of patients.
[0003] Conductive hydrogels have attracted much attention as a new type of electronic functional material. Conductive hydrogels mainly contain cross-linked hydrophilic substrates and conductive fillers (metal nanoparticles, carbon-based materials, conductive polymers, ions, etc.). By carefully combining and optimizing various conductive components and different types of polymer matrices, conductive hydrogel materials with widely adjustable or stimulus-responsive physical and chemical properties can be obtained. Conductive hydrogels have unique porous microstructures, large specific area, superior conductivity and electrochemical activity, showing excellent functions. Through various polymer chemistry and polymer processing technologies, conductive hydrogels are endowed with designability and controllability. They can be used as electrodes or electrolytes, and can be used in flexible sensors, environmental engineering, biomedical equipment, smart drug delivery systems, flexible energy storage equipment, etc. Among them, flexible sensors can convert external stimuli such as pressure, temperature and humidity into electrical signals, and have broad application prospects, including wearable electronics, health testing and implantable medical electronic materials. The hydrogel strain sensors reported so far generally have the advantages of a large strain measurement range, long service life, and convenient design and preparation. However, hydrogel strain sensors still have problems such as low mechanical strength, poor ductility, low sensitivity and low linear range, and these properties are difficult to meet at the same time, which restricts the development of wearable strain sensors. In order to improve the performance of flexible sensors, it is urgent to develop hydrogel sensors that combine excellent stretchability, high sensitivity and wide linear range.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a flexible conductive hydrogel and a preparation method and application thereof.
[0006] The present invention is achieved in that:
[0007] In a first aspect, the present invention provides a flexible conductive hydrogel, the raw materials of which include a hydrogen bonding monomer, a conductive filling material, a photoinitiator and water, wherein the hydrogen bonding monomer includes at least one of 2-ureido-4[1H]-pyrimidone and acryloserinamide.
[0008] In an optional embodiment, the hydrogen bonding monomer comprises 15 to 55 parts, the conductive filling material comprises 0.1 to 0.5 parts, the photoinitiator comprises 0.03 to 0.15 parts and the water comprises 45 to 85 parts by weight.
[0009] In an optional embodiment, the composition comprises, by weight: 20 to 50 parts of hydrogen bonding monomers, 0.1 to 0.3 parts of conductive filling materials, 0.05 to 0.1 parts of photoinitiators and 30 to 50 parts of water.
[0010] In an optional embodiment, the conductive filling material is selected from at least one of graphene, carbon nanotubes, Ti3C2Tx, Nb2CTx, Ti4N3Tx, and Ti3CNTx.
[0011] In an optional embodiment, the photoinitiator is selected from at least one of lithium phenyl-2,4,6-trimethylbenzoylphosphinate and 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone.
[0012] In a second aspect, the present invention provides a method for preparing a flexible conductive hydrogel, comprising:
[0013] Mixing: mixing the raw materials of the flexible conductive hydrogel according to any one of the aforementioned embodiments to obtain a prepolymer solution;
[0014] Curing: UV curing the prepolymer solution to obtain a flexible conductive hydrogel.
[0015] In an optional embodiment, the UV curing time is 2 minutes to 30 minutes.
[0016] In an optional embodiment, the light intensity of the ultraviolet light is 10Mw / cm 2 ~20Mw / cm 2 .
[0017] In a second aspect, the present invention provides an application of the flexible conductive hydrogel described in any one of the aforementioned embodiments in the field of strain sensors.
[0018] The present invention has the following beneficial effects:
[0019] 1. The flexible conductive hydrogel of the present invention exhibits excellent mechanical properties and adhesion properties due to hydrogen bonding and organic-inorganic composite effects, and has good ductility, high strength and low modulus; at the same time, the conductive filler is evenly dispersed in the network structure, and the conductive hydrogel has high conductivity, high sensitivity and a wide linear range.
[0020] 2. The preparation method of the flexible conductive hydrogel of the present invention is simple and easy, the raw materials are streamlined, and the preparation can be completed at room temperature.
[0021] 3. The flexible conductive hydrogel of the present invention is applied to sensors, which ensures the sensitivity and accuracy of the hydrogel strain sensor.
[0022] 4. The hydrogen bonding monomers in the flexible conductive hydrogel of the present invention include at least one of 2-ureido-4[1H]-pyrimidone and acryloserinamide. The 2-ureido-4[1H]-pyrimidone and acryloserinamide box walls and other hydrogen bonding monomers have advantages in stretchability, conductivity, sensitivity and adhesion performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0024] Figure 1 This is a test diagram of the mechanical properties of the conductive hydrogel prepared by the present invention;
[0025] Figure 2 The sensitivity of the conductive hydrogel prepared in the embodiment of the present invention under stretching;
[0026] Figure 3 The bonding strength of the conductive hydrogel prepared in the embodiment of the present invention on different substrates;
[0027] Figure 4 This is a test chart of the conductive properties of conductive hydrogels with different contents of conductive fillers prepared in an embodiment of the present invention. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0029] This embodiment provides a flexible conductive hydrogel, the raw materials of which include a hydrogen bonding monomer, a conductive filling material, a photoinitiator and water, wherein the hydrogen bonding monomer includes at least one of 2-ureido-4[1H]-pyrimidone and acryloserinamide.
[0030] The flexible conductive hydrogel in this embodiment is formed by light irradiation, and the hydrogel is connected to form a grid structure through hydrogen bonding and intermolecular forces, and the conductive filling material is dispersed in the grid structure. The hydrogen bonding and intermolecular forces inside the hydrogel give it high ductility, high strength and fatigue resistance.
[0031] In an optional embodiment, the hydrogen bonding monomer comprises 15 to 55 parts, the conductive filling material comprises 0.1 to 0.5 parts, the photoinitiator comprises 0.03 to 0.15 parts and the water comprises 45 to 85 parts by weight.
[0032] In an optional embodiment, the composition comprises, by weight: 20 to 50 parts of hydrogen bonding monomers, 0.1 to 0.3 parts of conductive filling materials, 0.05 to 0.1 parts of photoinitiators and 30 to 50 parts of water.
[0033] The conductive filler material in this embodiment needs to be added in an appropriate amount. Too much may affect the strength of the conductive hydrogel, while too little may affect the conductive performance.
[0034] In an optional embodiment, the conductive filling material is selected from at least one of graphene, carbon nanotubes, Ti3C2Tx, Nb2CTx, Ti4N3Tx, and Ti3CNTx.
[0035] In this embodiment, a conductive filling material is introduced and dispersed in the network structure. The conductive filling material has many advantages such as metal-like conductivity and large porosity. The most important thing is that its surface is rich in hydroxyl groups, oxygen, fluorine, etc., and further forms hydrogen bonds. The supramolecular structure is constructed through hydrogen bonding, which improves the conductive properties while also improving the mechanical properties and adhesion properties, broadens the carrier channel, and gives it high conductivity, high sensitivity and a wide linear range.
[0036] In an optional embodiment, the photoinitiator is selected from at least one of lithium phenyl-2,4,6-trimethylbenzoylphosphinate and 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone.
[0037] In a second aspect, the present invention provides a method for preparing a flexible conductive hydrogel, comprising:
[0038] Mixing: mixing the raw materials of the flexible conductive hydrogel according to any one of the aforementioned embodiments to obtain a prepolymer solution;
[0039] Curing: UV curing the prepolymer solution to obtain a flexible conductive hydrogel.
[0040] In an optional embodiment, the UV curing time is 2 minutes to 30 minutes.
[0041] In an optional embodiment, the light intensity of the ultraviolet light is 10Mw / cm 2 ~20Mw / cm 2 .
[0042] In a second aspect, the present invention provides an application of the flexible conductive hydrogel described in any one of the aforementioned embodiments in the field of strain sensors.
[0043] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0044] Example 1
[0045] This embodiment prepares a flexible conductive hydrogel, and the specific process is as follows:
[0046] Weigh 2g of acryloserinamide in a 5mL centrifuge tube, add 0.2mL of 10mg / mL photoinitiator LAP, add to 2.8mL deionized water, stir at room temperature to dissolve, then add 0.003g of graphene conductive filler (mass volume fraction is 0.1%), stir to make it evenly dispersed, and obtain a prepolymer solution. After the prepolymer solution is transferred to the mold, it is placed in a UV curing box, irradiated with UV light for 10min, and cured and cross-linked to prepare a conductive hydrogel PSA / Graphene.
[0047] Test Example 1
[0048] The amount of graphene in Example 1 was adjusted to a mass volume fraction of 0, 0.2% and 0.3%, and the mechanical properties of the prepared hydrogel were evaluated using a universal material mechanics tester. The detection method refers to GB / T 1040.1-2018.
[0049] Test results such as Figure 1As shown in the figure, from the tensile stress-strain curve, it can be seen that in the embodiment of the present invention, when the mass volume fraction of graphene in the gel is 0.1%, the maximum fracture strength of the prepared flexible conductive hydrogel can reach 4.8MPa, and the maximum elongation at break is 750%, which has excellent stretchability. The results show that in the conductive hydrogel, the hydrogen bonding between the conductive material graphene and the supramolecular enhances the fracture strength and elastic modulus of the hydrogel.
[0050] Test Example 2
[0051] The electrochemical workstation was used to detect the high sensitivity and wide linear range of the hydrogel prepared in Example 1 using the AC impedance method. The test results are shown in Figure 2 .
[0052] Result analysis: Figure 2 As shown in the figure, the sensitivity factor (GF) of the conductive hydrogel increases with the increase of elongation, and its linear range of sensitivity can be divided into three parts, among which the first part is when the elongation is 0% to 90%, the GF value is 2.05; when the elongation is 90% to 172%, the GF value is 3.35; when the elongation is 172% to 270%, the GF value is 5.2; This shows that the prepared conductive hydrogel can be used as a strain sensor, which not only has a wide linear range but also has high sensitivity, which can meet the needs of monitoring small or large deformations caused by human body movement, and has potential application prospects as a flexible wearable stress sensor.
[0053] Test Example 3
[0054] The adhesive properties of the hydrogel prepared in Example 1 were evaluated using a universal material mechanics tester. The test results are as follows: Figure 3 shown.
[0055] from Figure 3 It can be seen that PSA / Graphene conductive hydrogel shows better bonding performance on different adhesive substrates, and its bonding strength can reach up to 65KPa. The reason is that the flexibility and hydrogen bonding of the conductive hydrogel not only enable it to better contact with the substrate, but also enhance the hydrogen bonding at the contact point. Obviously, the prepared supramolecular conductive hydrogel has strong bonding strength. Therefore, the prepared conductive hydrogel has the potential to be used as a strain sensor and applied to electronic skin.
[0056] Test Example 4
[0057] The conductivity of the hydrogel prepared in Example 1 was tested by an electrochemical workstation using an AC impedance method. The test results are shown in Figure 4 .
[0058] like Figure 4As shown in the figure, the conductivity of the conductive hydrogel increases with the increase of the content of the conductive filler MXene, and the conductivity of the hydrogel is up to 17S / m. The reason is that the conductive filler has a good uniform dispersion in the supramolecular network structure, and the hydrogen bonding between the surface functional groups of the conductive filler and the polymer molecules promotes the movement of carriers, greatly improving the conductivity of the conductive hydrogel. The comparative example does not add conductive filler, and its conductivity is very low.
[0059] The experimental results of the above-mentioned test examples 1 to 4 show that the flexible conductive hydrogel of the present invention has high mechanical strength, high deformation, good adhesion, high conductive sensitivity, and a wide linear range, which is beneficial to improving the sensitivity and accuracy of the hydrogel strain sensor.
[0060] Example 2
[0061] This embodiment prepares a flexible conductive supramolecular hydrogel, which is mainly different from Embodiment 1 in that graphene is replaced by MXene (Ti4N3Tx).
[0062] The maximum breaking strength of the flexible conductive hydrogel prepared in this embodiment reaches 4.1 MPa, the maximum breaking elongation can reach 830%, the conductivity of the hydrogel can reach 12.2 S / m; and the bonding strength on polytetrafluoroethylene can reach 46.5 KPa.
[0063] Example 3
[0064] This example prepares a flexible conductive supramolecular hydrogel, and the specific process is as follows:
[0065] Weigh 1g of 2-ureido-4[1H]-pyrimidone, transfer it to a 5mL centrifuge tube, add 0.2mL of 10mg / mL photoinitiator LAP, add it to 0.8mL deionized water, stir and dissolve at room temperature, then add 0.1-0.3% Ti3C2Tx conductive filler material, stir to make it evenly dispersed, and obtain a prepolymer solution. After transferring the prepolymer solution to the mold, place it in a UV curing box, irradiate with UV light for 30min, and cure and crosslink to prepare the conductive hydrogel PU / MXene.
[0066] The maximum breaking strength of the flexible conductive hydrogel prepared in this embodiment reaches 2.4 MPa, the maximum breaking elongation can reach 740%, the conductivity of the hydrogel can reach 5.3 S / m; the linear sensitivity range is 0-315%; and the bonding strength on the glass sheet can reach 35 KPa.
[0067] Example 4
[0068] In this embodiment, a flexible conductive supramolecular hydrogel is prepared. The main difference from Example 1 is that the amount of acryloserinamide is adjusted to 20%, 30%, 40%, and 50% of the mass fraction of the conductive hydrogel, respectively. The results show that when the amount of acryloserinamide is 50%, the comprehensive performance is optimal, and when the amount of acryloserinamide is less than 20%, the mechanical properties are too poor.
[0069] Comparative Example 1
[0070] This comparative example prepared a conductive hydrogel, which is mainly different from Example 1 in that acryloserinamide is replaced with N-acryloylglycinamide. The maximum breaking strength of the prepared flexible conductive hydrogel can reach 4.8MPa, the maximum breaking elongation is 630%, the conductivity of the hydrogel is 17.3S / m; the linear sensitivity range is 0-125%; the bonding strength on the glass sheet is the highest, but only 2.7KPa.
[0071] Comparative Example 3
[0072] This comparative example prepares a conductive hydrogel, which is different from the embodiment in that the conductive filler material is replaced with polyaniline. The maximum breaking strength of the prepared flexible conductive hydrogel is 2.2MPa, the maximum breaking elongation is 440%, the conductivity of the hydrogel is 0.06S / m; the linear sensitivity range is 0-85%; the bonding strength on the glass sheet is the highest, but only 8KPa.
[0073] Comparative Example 4
[0074] This comparative example prepared a conductive hydrogel, which is different from the embodiment in that the conductive filler material is replaced with polypyrrole. The maximum breaking strength of the prepared flexible conductive hydrogel is only 2.5MPa, the maximum breaking elongation is 475%, the conductivity of the hydrogel is 0.045S / m; the linear sensitivity range is 0-90%; the bonding strength on the glass sheet is the highest, but only 10KPa.
[0075] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A flexible conductive hydrogel, characterized in that: The raw materials include hydrogen bonding monomers, conductive filling materials, photoinitiators and water, wherein the hydrogen bonding monomers include at least one of 2-ureido-4[1H]-pyrimidone and acryloserinamide; the conductive filling materials are selected from at least one of graphene, carbon nanotubes, Ti3C2Tx, Nb2CTx, Ti4N3Tx and Ti3CNTx; By weight, it comprises 15 to 55 parts of hydrogen bond monomer, 0.1 to 0.5 parts of conductive filling material, 0.03 to 0.15 parts of photoinitiator and 45 to 85 parts of water.
2. The flexible conductive hydrogel according to claim 1, characterized in that: Calculated by weight, it comprises: 20 to 50 parts of hydrogen bond monomer, 0.1 to 0.3 parts of conductive filling material, 0.05 to 0.1 parts of photoinitiator and 30 to 50 parts of water.
3. The flexible conductive hydrogel according to claim 1, characterized in that: The photoinitiator is selected from at least one of phenyl-2,4,6-trimethylbenzoylphosphinate lithium and 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone.
4. A method for preparing a flexible conductive hydrogel, characterized in that: include: Mixing, mixing the raw materials of the flexible conductive hydrogel according to any one of claims 1 to 3 to obtain a prepolymer solution; Curing: UV curing the prepolymer solution to obtain a flexible conductive hydrogel.
5. The method for preparing the flexible conductive hydrogel according to claim 4, characterized in that: The UV curing time is 2 minutes to 30 minutes.
6. The method for preparing the flexible conductive hydrogel according to claim 4, characterized in that: The light intensity of the ultraviolet light is 10Mw / cm 2 ~20Mw / cm 2 .