A modified polyvinyl alcohol film and its preparation method and application
By forming a polyvinyl alcohol-waterborne silica sol layer on a polyvinyl alcohol film and spraying a fluorine-containing surface treatment layer, the problem of insufficient tensile strength of polyvinyl alcohol films in a water vapor environment was solved, and high-strength and low-cost modified film preparation was achieved.
Patent Information
- Application Number
- CN202310337649.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing polyvinyl alcohol films have difficulty maintaining tensile strength above 93% in a water-vapor environment, and their preparation cost is relatively high.
By forming a polyvinyl alcohol-waterborne silica sol layer on the surface of a polyvinyl alcohol film and spraying a fluorine-containing surface treatment layer, a cross-linked microstructure is formed, which blocks water penetration and improves the barrier properties and mechanical properties of the film.
Modified polyvinyl alcohol films can retain more than 95% of their tensile strength in a water-vapor environment, and have good waterproof, oil-proof, and stain-proof effects, while also having low preparation costs.
Smart Images

Figure GDA0005004713960000091 
Figure GDA0005004713960000101 
Figure GDA0005004713960000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of packaging materials, and in particular to a modified polyvinyl alcohol film and a preparation method and application thereof. Background Art
[0002] Polyvinyl alcohol (PVA) is a water-soluble polymer made from vinyl acetate by polymerization and alcoholysis. It is not only simple to prepare and low-cost, but also has excellent hydrophilicity, gas barrier properties, acid and alkali resistance, organic solvent resistance, outstanding biosafety and good film-forming ability. Therefore, it is widely used as a membrane material in food packaging, pervaporation, sewage treatment and other fields. PVA has a linear polymer structure and a large number of hydroxyl groups on the side chain. Although PVA film has excellent hydrophilic and anti-pollution properties, it is easy to swell or even dissolve in water, and the mechanical strength of the film is poor, which cannot meet the use requirements of PVA film in practical applications.
[0003] At present, the water resistance and mechanical properties of PVA film can be improved by modifying PVA. Patent CN106883442A discloses a method for preparing a fluoride-modified polyvinyl alcohol film, which sprays a fluoride-containing surface treatment composition solution with a concentration of 1wt% on the surface of a polyvinyl alcohol film substrate to obtain a fluoride-modified polyvinyl alcohol film. This patent improves the tensile strength of the film after treatment in a water vapor environment, but its tensile strength retention rate is still difficult to reach more than 93%; at the same time, to achieve the improvement effect of this patent, it is necessary to use a fluoride-containing surface treatment composition solution with a concentration of 1wt% to treat the surface of the polyvinyl alcohol film substrate, and the preparation cost is relatively high. Therefore, there is an urgent need for a polyvinyl alcohol film whose tensile strength retention rate in a water vapor environment can still reach more than 93% and has a low preparation cost. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a modified polyvinyl alcohol film and a preparation method and application thereof. The modified polyvinyl alcohol film provided by the present invention can retain more than 95% of its tensile strength in a water vapor environment, has good barrier properties, and has low preparation cost.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] A modified polyvinyl alcohol film, the film comprising a polyvinyl alcohol-aqueous silica sol layer and a fluorine-containing surface treatment layer from bottom to top;
[0007] The polyvinyl alcohol-aqueous silica sol layer is obtained by casting after the polyvinyl alcohol solution and the aqueous silica sol are mixed; the fluorine-containing surface treatment layer is obtained by spraying the fluorine-containing surface treatment composition solution on the polyvinyl alcohol-aqueous silica sol layer;
[0008] The particle size of the aqueous silica sol is above 40nm and the pH value is not more than 8.
[0009] Preferably, the concentration of the fluorine-containing surface treatment composition is 0.2 wt% to 0.8 wt%, and the spraying amount is 100 g to 500 g of the fluorine-containing surface treatment composition solution per square meter of polyvinyl alcohol-aqueous silica sol layer.
[0010] Preferably, the degree of polymerization of the polyvinyl alcohol in the polyvinyl alcohol solution is medium; the polyvinyl alcohol solution and the aqueous silica sol are blended by first preparing the polyvinyl alcohol into a polyvinyl alcohol aqueous solution with a relatively high concentration, then adding the aqueous silica sol, mixing well, and then diluting with water to a polyvinyl alcohol concentration of 7wt%.
[0011] Preferably, the particle size of the aqueous silica sol is 80 nm, and the addition amount of the aqueous silica sol is 0.5% to 5% of the weight of the polyvinyl alcohol.
[0012] More preferably, the added amount of the aqueous silica sol is 1% to 4% by weight of the polyvinyl alcohol.
[0013] Preferably, the fluorine-containing surface treatment composition comprises a first reactive compound and a second reactive compound; the first reactive compound is a reactive compound containing a perfluoropolyether group, and the second reactive compound is a reactive compound containing a perfluoroalkyl group.
[0014] Preferably, the content of the first reactive compound and the second reactive compound in the fluorine-containing surface treatment composition is both ≥ 10 wt %.
[0015] Preferably, the first reactive compound is as shown in Formula I:
[0016] B-PFPE-A-(Si(OR 1 )3) a Formula I;
[0017] Among them, PFPE is a perfluoropolyether group, A is an a+1 valent organic group, R 1 is an alkyl group, a is an integer from 1 to 10, and B is F or A-(Si(OR 1 )3) a The group represented;
[0018] The second reactive compound is shown in Formula II or Formula III:
[0019] R f -B-Si-(OR 2 )3 Formula II;
[0020] M(CH2CR1(-DR f ))m (CH2CR2(-E-Si(OR 3 )3)) n (CH2CR3(-I)) p N-type III;
[0021] Among them, R f is a monovalent perfluoroalkyl group, B is a divalent organic group, R 2 and R 3 is an alkyl group, M and N are monovalent organic groups, R1, R2 and R3 are H or CH3, D and E are divalent organic groups, I is a monovalent organic group, m and n are positive integers, and p is 0 or a positive integer.
[0022] The present invention also provides a method for preparing the modified polyvinyl alcohol film described in the above scheme, comprising the following steps:
[0023] S1, mixing the polyvinyl alcohol solution with the aqueous silica sol, diluting with water and casting into a film, and naturally air-drying at room temperature to obtain a polyvinyl alcohol-aqueous silica sol layer;
[0024] S2. Spraying the fluorine-containing surface treatment composition solution onto the polyvinyl alcohol-aqueous silica sol layer, and curing it for 22 to 26 hours after natural air drying at room temperature to obtain a modified polyvinyl alcohol film.
[0025] The present invention also provides an application of the modified polyvinyl alcohol film in the above solution in packaging materials.
[0026] Beneficial technical effects: The present invention provides a modified polyvinyl alcohol film and its preparation method and application. The present invention forms a polyvinyl alcohol-aqueous silica sol layer by mixing polyvinyl alcohol and aqueous silica sol, and sprays a fluorine-containing surface treatment layer thereon. The fluorine-containing surface treatment layer can block water from penetrating into the polyvinyl alcohol layer, avoid changes in the aggregate structure of the polyvinyl alcohol layer, and effectively maintain the barrier properties and mechanical properties of the film; and the aqueous silica sol, polyvinyl alcohol and fluorine-containing surface treatment composition form a cross-linked microstructure, further improving the tensile strength of the film in a water vapor environment. The modified polyvinyl alcohol film of the present invention can maintain a tensile strength retention rate of more than 95% in a water vapor environment, has good waterproof, oil-proof and antifouling effects, and has a low preparation cost. DETAILED DESCRIPTION
[0027] The present invention provides a modified polyvinyl alcohol film, which comprises a polyvinyl alcohol-aqueous silica sol layer and a fluorine-containing surface treatment layer in order from bottom to top;
[0028] The polyvinyl alcohol-aqueous silica sol layer is obtained by casting after mixing a polyvinyl alcohol solution with an aqueous silica sol; the fluorine-containing surface treatment layer is obtained by spraying a fluorine-containing surface treatment composition solution on the polyvinyl alcohol-aqueous silica sol layer; the present invention forms a polyvinyl alcohol-aqueous silica sol layer by mixing polyvinyl alcohol and aqueous silica sol, and sprays the fluorine-containing surface treatment layer thereon; the fluorine-containing surface treatment layer can block the penetration of moisture into the polyvinyl alcohol layer, avoid changes in the aggregated structure of the polyvinyl alcohol layer, and effectively maintain the barrier properties and mechanical properties of the film; and the aqueous silica sol, polyvinyl alcohol and the fluorine-containing surface treatment composition form a cross-linked microstructure, which further improves the tensile strength of the film in a water vapor environment.
[0029] In the present invention, the particle size of the aqueous silica sol is preferably above 40nm, more preferably 80nm. The pH value of the aqueous silica sol is preferably not more than 8, more preferably 3-8. The amount of the aqueous silica sol added is 0.5% to 5% of the weight of polyvinyl alcohol, more preferably 1% to 4%, and most preferably 2%. By controlling the particle size of the aqueous silica sol, the present invention can ensure that the tensile strength of the modified polyvinyl alcohol film is maximized and the retention rate of its tensile strength in a water vapor environment is maintained. If the particle size of the aqueous silica sol is too small, the tensile strength and retention rate of the final polyvinyl alcohol film will be affected. At the same time, the present invention controls the amount of aqueous silica sol added to achieve a certain balance between the aqueous silica sol and the polyvinyl alcohol molecules to maintain the tensile strength of the final film. If the amount of aqueous silica sol added is too high, it will affect the entanglement between different polyvinyl alcohol molecules and reduce the tensile strength of the film.
[0030] In the present invention, the concentration of the fluorine-containing surface treatment composition is preferably 0.2 wt% to 0.8 wt%, and the spraying amount is preferably 100 g to 500 g of the fluorine-containing surface treatment composition solution per square meter of polyvinyl alcohol-aqueous silica sol layer.
[0031] In the present invention, the degree of polymerization of polyvinyl alcohol in the polyvinyl alcohol solution is medium; the polyvinyl alcohol solution and the aqueous silica sol are blended by first preparing the polyvinyl alcohol into a polyvinyl alcohol aqueous solution with a relatively high concentration, then adding the aqueous silica sol, mixing evenly, and then diluting with water to a polyvinyl alcohol concentration of 7wt%.
[0032] In the present invention, preferably, the fluorine-containing surface treatment composition comprises a first reactive compound and a second reactive compound; the first reactive compound is a reactive compound containing a perfluoropolyether group, and the second reactive compound is a reactive compound containing a perfluoroalkyl group; the contents of the first reactive compound and the second reactive compound in the fluorine-containing surface treatment composition are both ≥10wt%.
[0033] In the present invention, preferably, the first reactive compound is as shown in Formula I:
[0034] B-PFPE-A-(Si(OR 1 )3) a Formula I;
[0035] Among them, PFPE is a perfluoropolyether group, A is an a+1 valent organic group, R 1 is an alkyl group, a is an integer from 1 to 10, and B is F or A-(Si(OR 1 )3) a The perfluoropolyether group is preferably F(CF(CF3)CF2O) a CF(CF3)-, F(CF(CF3)CF2O) a CF2CF2-, CF3O(CF2CF2O) a CF2-, CF3O(CF2O) b (CF2CF2O) a CF2-, -CF(CF3)O(CF(CF3)CF2O) a CF(CF3)-,-CF2CF2O(CF(CF3)CF2O) a CF2CF2-, -CF2O(CF2CF2O) a CF2-, -CF2O(CF2O) b (CF2CF2O) a CF2-, etc., wherein a and b are integers from 1 to 100; the a+1 valent organic group is preferably: -CONH(CH2) k -、-CH2O(CH2) k -、-CH2OCONH(CH2) k -、-CONHCH2CH2OCONH(CH2) k -、-CH2OCOCH2CH2N(CH3)(CH2) k -, -CH2OCH2CH2CH2Si(CH3)2OSi(CH3)2CH2CH2-, -CON((CH2) k -)2, etc., wherein k is an integer from 2 to 10; the alkyl group is preferably: CH3, CH2CH3, CH(CH3)2, C(CH3)3, etc.
[0036] The first reactive compound is more preferably as shown in Formula I-1:
[0037] B-PFPE-CON(CH2CH2CH2Si(OR 1 )3)2 Formula Ⅰ-1;
[0038] Wherein, PFPE in Formula I-1 is a perfluoropolyether group, R 1 C1~4 alkyl, B is F or CON(CH2CH2CH2Si(OR 1 )3)2;
[0039] The first reactive compound is most preferably as shown in Formula I-2:
[0040] B-PFPE-CON(CH2CH2CH2Si(OCH3)3)2 formula I-2;
[0041] Wherein, PFPE in formula Ⅰ-2 is a perfluoropolyether group, and B is F or CON(CH2CH2CH2Si(OCH3)3)2;
[0042] In the present invention, the first reactive compound may be preferably one or more of the compounds shown in Formula I. In the first reactive compound, B is A-(Si(OR 1 )3) a The compound having the group represented by represents at least 50% of the first reactive compound.
[0043] In the present invention, the second reactive compound is preferably a reactive compound containing a perfluoroalkyl group; the second reactive compound is as shown in Formula II or Formula III:
[0044] R f -B-Si-(OR 2 )3 Formula II;
[0045] M(CH2CR1(-DR f )) m (CH2CR2(-E-Si(OR 3 )3)) n (CH2CR3(-I)) p N-type III;
[0046] Among them, R f is a monovalent perfluoroalkyl group, B is a divalent organic group, R 2 and R 3 is an alkyl group, M and N are monovalent organic groups, R1, R2 and R3 are H or CH3, D and E are divalent organic groups, I is a monovalent organic group, m and n are positive integers, and p is 0 or a positive integer. The perfluoroalkyl group is preferably CF3 (CF2) c 、(CF3)2CF(CF2) c, CF3, etc., wherein c is an integer from 0 to 20; the divalent organic group is preferably: -CH2CH2-, -CH2OCH2CH2CH2-, -CH2CH2OCH2CH2CH2-, -CH2CH2OCONHCH2CH2CH2-, etc.; the alkyl group is preferably: CH3, CH2CH3, CH(CH3)2, C(CH3)3, etc.
[0047] The compounds containing perfluoroalkyl groups represented by formula (II) can be listed as follows: CF3(CF2)3CH2CH2Si(OCH3)3, CF3(CF2)5CH2CH2Si(OCH3)3, CF3(CF2)3CH2CH2Si(OCH2CH3)3, CF3(CF2)5CH2CH2Si(OCH2CH3)3, (CF3)2CF(CF2)3CH2CH2Si(OCH3)3, CF3CH2CH2Si(OCH3)3, CF3CF2CH2OCH2CH2CH2Si(OCH2CH3)3, CF3(CF2)3CH2CH2OCH2CH2CH2Si(OCH3)3, CF3(CF2)3CH2CH2OCONHCH2CH2CH2Si(OCH3)3. The compound containing a perfluoroalkyl group represented by formula (III) is usually obtained by free radical copolymerization of a perfluoroalkyl monomer having an unsaturated double bond and a siloxane monomer having an unsaturated double bond, and a third monomer component may also be added. The perfluoroalkyl monomer having an unsaturated double bond such as CH2=C(R)COOCH2CH2(CF2) d CF3, CH2=C(R)COOCH2CH2N(R′)SO2(CF2) d CF3, etc., wherein R and R' are H or C1-4 alkyl, d is an integer of 0-20, and specifically, CH2=C(CH3)COO CH2CH2N(CH3)SO2C4F9, CH2=C(CH3)COOCH2CH2N(CH3)SO2C6F 13 、CH2=C(CH3)COOCH2CH2C6F 13 , CH2=CHCOOCH2CH2C4F9, CH2=CHCOO CH2CH2C8F 17 Siloxane monomers with unsaturated double bonds such as CH2=CHSi(OR 3 )3. CH2=CHCH2Si(OR 3 )3. CH2=C(R″)COOCH2CH2CH2Si(OR 3 )3, etc., where R 3 Same as above, R″ is C 1~4The third component monomers include: non-fluorinated alkyl (meth)acrylates, chloroalkyl (meth)acrylates, styrene, vinyl chloride, vinylidene chloride, glycidyl (meth)acrylate, and the like.
[0048] In the present invention, without affecting the final properties of the modified polyvinyl alcohol film, the fluorine-containing surface treatment composition may contain an appropriate amount of other non-fluorine components, such as a fluorine-containing surface treatment composition containing both an isocyanate group or a blocked isocyanate group and -Si-(OR 4 )3 group or a compound without a fluorine-containing group and an isocyanate group or a blocked isocyanate group, containing -Si-(OR 5 )3 groups of siloxane, wherein R 4 , R 5 C 1~4 of alkyl.
[0049] The isocyanate group or the blocked isocyanate group and -Si-(OR 4 )3 group compounds, such as: OCNCH2CH2CH2Si(OCH)3, OCN-T-NHCONHCH2CH2CH2Si(OCH)3, OCN-T-NHCONHCH2CH2CH2Si(OCH2CH)3, Y-CONH-T-NHCONHCH2CH2CH2Si(OCH)3, (OCN)2-Q-NH CONHCH2CH2CH2Si(OCH)3, (Y-OCONH)2-Q-NHCONHCH2CH2CH2Si(OCH)3, etc., wherein T is the residue after removing the diisocyanate group of hexamethyl diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, etc., Q is the residue after removing the triisocyanate group of a trimer of hexamethyl diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, etc., or triphenylmethane triisocyanate, and Y is the residue after removing the activated glassy hydrogen of 2-methylimidazole, methyl ethyl ketone oxime, etc.
[0050] The present invention does not contain fluorine-containing groups and isocyanate groups or blocked isocyanate groups, contains -Si-(OR 5 )3 groups of siloxane, wherein R 4 , R 5 C 1~4Alkyl groups such as ethyl orthosilicate (Si(OCH2CH3)4), methyltrimethoxysilane (CH3Si(OCH3)3), ethyltrimethoxysilane (CH3CH2Si(OCH3)3), cyclohexyltrimethoxysilane, isobutyltriethoxysilane, n-hexyltriethoxysilane, n-butyltrimethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, dodecyltrimethoxysilane, hexadecyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, phenyltrimethoxysilane, etc.
[0051] The present invention also provides a method for preparing the modified polyvinyl alcohol film described in the above scheme, comprising the following steps:
[0052] S1, mixing the polyvinyl alcohol solution with the aqueous silica sol, diluting with water and casting into a film, and naturally air-drying at room temperature to obtain a polyvinyl alcohol-aqueous silica sol layer;
[0053] S2. Spraying the fluorine-containing surface treatment composition solution onto the polyvinyl alcohol-aqueous silica sol layer, and curing it for 22 to 26 hours after natural air drying at room temperature to obtain a modified polyvinyl alcohol film.
[0054] In the preparation process of the modified polyvinyl alcohol film of the present invention, before spraying the fluorine-containing surface treatment composition solution, a primer layer of a non-fluorine silicone composition solution can be sprayed on the polyvinyl alcohol-aqueous silica sol layer without affecting the final performance of the modified polyvinyl alcohol film. The preparation method of the modified polyvinyl alcohol film containing the primer layer comprises the following steps:
[0055] S1, mixing the polyvinyl alcohol solution with the aqueous silica sol, diluting with water and casting into a film, and naturally air-drying at room temperature to obtain a polyvinyl alcohol-aqueous silica sol layer;
[0056] S2, spraying the non-fluorinated silicone composition solution onto the polyvinyl alcohol-aqueous silica sol layer, and naturally air-drying at room temperature to obtain a non-fluorinated silicone layer;
[0057] S3. Spray the fluorine-containing surface treatment composition solution onto the non-fluorine silicone layer, dry naturally at room temperature, and then cure for 22 to 26 hours to obtain a modified polyvinyl alcohol film.
[0058] In the present invention, the concentration of the non-fluorinated silicone composition solution is preferably 0.1wt% to 5wt%, more preferably 0.3wt% to 3wt%, and most preferably 1wt% to 2wt%; the solvent of the non-fluorinated silicone composition is preferably one or more of butyl acetate, ethyl acetate, heptane, hexane, cyclohexane, petroleum ether, D40, methyl isoamyl ketone, diethylene glycol dimethyl ether, and N,N-dimethylformamide.
[0059] In the present invention, the parameters of the raw materials and each layer are the same as those described above and will not be described in detail herein.
[0060] The present invention also provides an application of the modified polyvinyl alcohol film in the above solution in packaging materials.
[0061] There is no particular limitation on the type of application in the present invention, and any type of application acceptable to the fluorine-modified polyvinyl alcohol film in this field may be used.
[0062] In order to better understand the present invention, the content of the present invention is further explained in conjunction with the following examples, but the content of the present invention is not limited to the following examples. The materials, reagents, etc. used in the examples and test examples of the present invention, unless otherwise specified, can be obtained from commercial channels; the methods used in the examples and test examples of the present invention, unless otherwise specified, are conventional methods.
[0063] Examples 1 to 5 and Comparative Examples 1 to 7
[0064] 1.1 Materials
[0065] (1) First reactive compound:
[0066] a: The first reactive compound PFPE-CONH(CH2CH2CH2Si(OCH3)3)2 shown in formula I is prepared by reacting perfluoropolyether monocarboxylate (PFPE-COOCH3 purchased from Solvay) with NH2(CH2CH2CH2Si(OCH3)3)2 (purchased from Nanjing Nengde).
[0067] b: The first reactive compound ((H3CO)3SiCH2CH2CH2)2NHCO-PFPE-CONH(CH2CH2CH2Si(OCH3)3)2 shown in formula I is prepared by reacting perfluoropolyether dicarboxylate (H3COCO-PFPE-COOCH3 purchased from Solvay) with NH2(CH2CH2CH2Si(OCH3)3)2.
[0068] (2) Second Reactive Compound
[0069] c: CF3(CF2)5CH2CH2Si(OCH3)3 (purchased from Juhua Group);
[0070] d: CH2=C(CH3)COOCH2CH2(CF2)5CF5 (purchased from Fujian Sannong New Materials Co., Ltd.), CH2=CHCOOCH2(CH2) 10 CH3 (purchased from Hubei Jusheng Technology Co., Ltd.) and CH2=CHCH2Si(OCH3)3 were copolymerized in a mass ratio of 6:2:2 by free radical solution copolymerization to obtain a reactive compound containing a perfluoroalkyl group as shown in Formula III.
[0071] (3) Aqueous silica sol:
[0072] k1: aqueous silica sol, particle size 80 nm, pH 7.4, concentration 30 wt% (purchased from Zhangjiagang Churen New Materials Technology Co., Ltd.);
[0073] k2: aqueous silica sol, particle size 80 nm, pH 4.0, concentration 30 wt% (purchased from Zhangjiagang Churen New Materials Technology Co., Ltd.);
[0074] k3: aqueous silica sol, particle size 80nm, pH value 9.5, concentration 30wt% (purchased from Zhangjiagang Churen New Materials Technology Co., Ltd.)
[0075] k4: aqueous silica sol, particle size 10 nm to 25 nm, pH 7.2, concentration 30 wt% (purchased from Zhangjiagang Churen New Materials Technology Co., Ltd.).
[0076] (6) Polyvinyl alcohol:
[0077] The degree of polymerization of polyvinyl alcohol (purchased from Shanghai Kaidu Industrial Development Co., Ltd.) is medium.
[0078] 1.2 Preparation method
[0079] (1) Examples 1-5, Comparative Examples 1-2 and Comparative Examples 5-7 210 g of polyvinyl alcohol was dissolved in 2000 g of water, and then 14 g of the aqueous silica sol solution shown in Table 1 (containing 4.2 g of aqueous silica sol, accounting for 2% of the weight of polyvinyl alcohol) was added. After mixing evenly, the mixture was diluted to 3000 g to prepare an aqueous silica sol solution with a polyvinyl alcohol concentration of 7 wt%. Comparative Example 3 210 g of polyvinyl alcohol was dissolved in 2790 g of water to prepare a solution with a polyvinyl alcohol concentration of 7 wt%. Example 4-1 210 g of polyvinyl alcohol was dissolved in 2000 g of water, and then 7 g of the aqueous silica sol solution shown in Table 1 (containing 2.1 g of silica sol, accounting for 1% of the weight of polyvinyl alcohol) was added. After mixing evenly, the mixture was diluted to 3000 g to prepare an aqueous silica sol solution with a polyvinyl alcohol concentration of 7 wt%. Example 4-2 210g of polyvinyl alcohol was dissolved in 2000g of water, and then 28g of the aqueous silica sol solution shown in Table 1 (containing 8.4g of silica sol, accounting for 4% of the weight of polyvinyl alcohol) was added. After mixing evenly, the mixture was diluted to 3000g to prepare an aqueous silica sol solution with a polyvinyl alcohol concentration of 7wt%. Comparative Example 4 210g of polyvinyl alcohol was dissolved in 2000g of water, and then 38.5g of the aqueous silica sol solution shown in Table 1 (containing 11.55g of silica sol, accounting for 5.5% of the weight of polyvinyl alcohol) was added. After mixing evenly, the mixture was diluted to 3000g to prepare an aqueous silica sol solution with a polyvinyl alcohol concentration of 7wt%.
[0080] (2) According to the ratio (mass ratio) in Table 1, the fluorine-containing surface treatment composition of Example 1 was prepared into a solution with a concentration of 0.2wt%, and the solvent was 7100; the fluorine-containing surface treatment composition of Example 2 was prepared into a solution with a concentration of 0.8wt%, and the solvent was 7100; the fluorine-containing surface treatment composition of Example 3 was prepared into a solution with a concentration of 0.4wt%, and the solvent was 7100; the fluorine-containing surface treatment compositions of Examples 4, 4-1, 4-2, 5 and Comparative Examples 1 to 7 were prepared into solutions with a concentration of 0.5wt%, and the solvent was fluorocarbon solvent 7200.
[0081] Table 1 Ratio (mass ratio) of each raw material in Examples 1 to 5 and Comparative Examples 1 to 6
[0082]
[0083]
[0084] (3) According to the settings of each embodiment and comparative example, the polyvinyl alcohol-aqueous silica sol solution is respectively cast into a film, and naturally air-dried at room temperature to obtain a polyvinyl alcohol-aqueous silica sol layer; the fluorine-containing surface treatment composition solution is sprayed on the polyvinyl alcohol-aqueous silica sol layer, and the solvent is naturally air-dried to obtain a fluorine-containing surface treatment layer, which is cured at room temperature to obtain a modified polyvinyl alcohol film;
[0085] Among them, the spraying concentration of the fluorine-containing surface treatment composition solution of Example 1 is 300g per square meter of polyvinyl alcohol-aqueous silica sol base film, the spraying concentration of the fluorine-containing surface treatment composition solution of Example 2 is 100g per square meter of polyvinyl alcohol-aqueous silica sol base film, the spraying concentration of the fluorine-containing surface treatment composition solution of Example 3 is 500g per square meter of polyvinyl alcohol-aqueous silica sol base film, and the spraying concentration of the fluorine-containing surface treatment composition solution of Examples 4, 4-1, 4-2, 5 and Comparative Examples 1 to 7 is 200g per square meter of polyvinyl alcohol-aqueous silica sol base film;
[0086] Example 1 was cured at room temperature for 26 hours; Example 2 was cured at room temperature for 22 hours; Examples 3 to 5, 4-1, 4-2 and Comparative Examples 1 to 7 were cured at room temperature for 24 hours to obtain modified polyvinyl alcohol films.
[0087] 1.3 Performance Testing
[0088] (1) Waterproof test
[0089] The modified polyvinyl alcohol films obtained in Examples 1 to 5 and Comparative Examples 1 to 7 were respectively tested for water resistance, and the water resistance evaluation standard was implemented according to GB / T4745-1997 "Test for Determination of Wetness Resistance of Textile Fabric Surfaces by Water Spraying";
[0090] Table 2 Waterproof evaluation standard
[0091] Waterproof grade state 5 No wet surface 4 Slightly moist surface 3 Partially wet surface 2 Surface Wetting 1 All surfaces are wet
[0092] (2) Oil resistance test
[0093] The modified polyvinyl alcohol films obtained in Examples 1 to 5 and Comparative Examples 1 to 7 were respectively tested for oil repellency, and the oil repellency evaluation standard was implemented according to GB / T19977-2005 "Test for Oil Repellency and Hydrocarbon Resistance of Textiles".
[0094] Table 3 Oil resistance evaluation standard
[0095] serial number Test fluid composition Surface tension (N / m, 25℃) 8 n-Heptane 0.0198 7 n-octane 0.0214 6 n-Decane 0.0235 5 n-Dodecane 0.0247 4 n-Tetradecane 0.0264 3 n-Hexadecane 0.0273 2 Hexadecane 35 / white mineral oil 65 mixture 0.0296 1 White mineral oil 0.0315
[0096] (3) Evaluation of antifouling performance
[0097] The modified polyvinyl alcohol films obtained in Examples 1 to 5 and Comparative Examples 1 to 7 were respectively evaluated for antifouling performance. Oil pen test: a line was drawn on the modified surface with an oil pen, and then the changes in the ink traces were carefully observed and evaluated according to the following standards:
[0098] E: Ink shrinks quickly
[0099] F: Ink shrinkage
[0100] NG: The ink hardly shrinks.
[0101] (4) Tensile strength
[0102] The modified polyvinyl alcohol films obtained in Examples 1 to 5 and Comparative Examples 1 to 7 were respectively subjected to tensile strength tests, and the width of the test samples was 5 cm. The test samples for tensile strength needed to be double-sided treated. The treatment in a water vapor environment means placing the double-sided treated test samples in an environment with a humidity of 80% for 24 hours. At the same time, the obtained tensile strength was converted into the tensile strength when the film thickness was 50 μm.
[0103] 1.4 Results
[0104] The performance test results of the modified polyvinyl alcohol films obtained in Examples 1 to 5 and Comparative Examples 1 to 7 are shown in Table 4.
[0105] Table 4 Performance test results of modified polyvinyl alcohol films obtained in Examples 1 to 5 and Comparative Examples 1 to 7
[0106]
[0107] As can be seen from Table 1, the waterproof performance grade of the modified polyvinyl alcohol film obtained in Examples 1 to 5 can reach 5, the oil repellency grade is 7 to 8, and the antifouling performance grade is E, which are all better than the waterproof performance, oil repellency and antifouling performance of Comparative Examples 1 to 7. At the same time, the tensile strength of the modified polyvinyl alcohol film obtained in Examples 1 to 5 can reach 57.8 MPa to 62.5 MPa, the tensile strength after treatment in a water vapor environment is 55.1 MPa to 60.1 MPa, and the tensile strength retention rate can reach 95.3% to 96.5%, which is significantly higher than the tensile strength of the fluorine-modified polyvinyl alcohol film obtained in Comparative Examples 1 to 7, the tensile strength after treatment in a water vapor environment, and the tensile strength retention rate.
[0108] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A modified polyvinyl alcohol film, characterized in that: The film comprises, from bottom to top, a polyvinyl alcohol-aqueous silica sol layer and a fluorine-containing surface treatment layer; The polyvinyl alcohol-aqueous silica sol layer is obtained by casting after the polyvinyl alcohol solution and the aqueous silica sol are mixed; the fluorine-containing surface treatment layer is obtained by spraying the fluorine-containing surface treatment composition solution on the polyvinyl alcohol-aqueous silica sol layer; The particle size of the aqueous silica sol is above 40 nm and the pH value is not more than 8; The concentration of the fluorine-containing surface treatment composition is 0.2wt% to 0.8wt%, and the spraying amount is 100g to 500g of the fluorine-containing surface treatment composition solution per square meter of polyvinyl alcohol-aqueous silica sol layer; The particle size of the aqueous silica sol is 80 nm, and the addition amount of the aqueous silica sol is 0.5% to 5% of the weight of the polyvinyl alcohol; The fluorine-containing surface treatment composition comprises a first reactive compound and a second reactive compound; the first reactive compound is a reactive compound containing a perfluoropolyether group, and the second reactive compound is a reactive compound containing a perfluoroalkyl group; The content of the first reactive compound and the second reactive compound in the fluorine-containing surface treatment composition is both ≥ 10 wt %; The first reactive compound is shown in Formula I: B-PFPE-A-(Si(OR 1 )3) a Formula I; Among them, PFPE is a perfluoropolyether group, A is an a+1 valent organic group, R 1 is an alkyl group, a is an integer from 1 to 10, and B is F or A-(Si(OR 1 )3) a The first reactive compound is one or more compounds of formula I, and in the first reactive compound, B is A-(Si(OR 1 )3) a The compound of the group represented by represents at least 50% of the first reactive compound; The second reactive compound is shown in Formula II or Formula III: Rf-B-Si-(OR 2 )3 of formula II; M(CH2CR1(-D-R f )) m (CH2CR2(-E-Si(OR 3 )3)) n (CH2CR3(-I)) p Formula N III; Among them, R f is a monovalent perfluoroalkyl group, B is a divalent organic group, R 2 and R 3 is an alkyl group, M and N are monovalent organic groups, R1, R2 and R3 are H or CH3, D and E are divalent organic groups, I is a monovalent organic group, m and n are positive integers, and p is 0 or a positive integer.
2. The modified polyvinyl alcohol film according to claim 1, characterized in that: The degree of polymerization of the polyvinyl alcohol in the polyvinyl alcohol solution is medium; the polyvinyl alcohol solution and the aqueous silica sol are blended by first preparing the polyvinyl alcohol into a polyvinyl alcohol aqueous solution with a relatively high concentration, then adding the aqueous silica sol, mixing evenly, and then diluting with water to a polyvinyl alcohol concentration of 7wt%.
3. The modified polyvinyl alcohol film according to claim 1, characterized in that: The added amount of the aqueous silica sol is 1% to 4% of the weight of the polyvinyl alcohol.
4. A method for preparing the modified polyvinyl alcohol film according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1, mixing the polyvinyl alcohol solution with the aqueous silica sol, diluting with water and casting into a film, and naturally air-drying at room temperature to obtain a polyvinyl alcohol-aqueous silica sol layer; S2. Spraying the fluorine-containing surface treatment composition solution onto the polyvinyl alcohol-aqueous silica sol layer, and curing it for 22 to 26 hours after natural air drying at room temperature to obtain a modified polyvinyl alcohol film.
5. Use of the modified polyvinyl alcohol film according to any one of claims 1 to 3 in packaging materials.
Citation Information
Patent Citations
Preparation method of fluoride-modified polyvinyl alcohol thin film
CN106883442A
Laminated film having gas barrier characteristics
CN101267938A
Modified polyvinylalcohol (PVA) base film, preparation method thereof and polarizer
CN102432899A
Method for preparing nano polyvinyl alcohol coating liquid by adopting sol-gel method and coating formed by nano polyvinyl alcohol coating liquid
CN103122171A
Preparation method of coating paint film containing modified silica sol
CN106811094A