A kind of heat-conducting insulating silicone gasket and preparation method thereof

Through the use of nano-aluminum nitride, aluminum nitride and diamond composite materials, the problem of poor thermal conductivity and insulation effect of thermally conductive silicone sheets is solved, and a silicone gasket with high thermal conductivity and insulation is achieved, suitable for high heat source dissipation Scene.

CN116218233BActive Publication Date: 2024-12-03SHENZHEN LEIZDUN NEW MATERIAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310271399.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-12-03
Estimated Expiration
2043-03-20

AI Technical Summary

Technical Problem

The thermal conductivity and insulation effects of existing thermally conductive insulated silicone sheets are not good, which limits its application scope, especially in scenarios where high heat source dissipation needs.

Method used

Nanoaluminum nitride, aluminum nitride and diamond composite materials are used as thermally conductive insulating fillers. Through filling and surface treatment of different particle sizes, vinyl silicone oil, crosslinking agent and vulcanizing agent are combined to form a silicone pad with high thermal conductivity and insulation. piece.

Benefits of technology

It has achieved thermally conductive insulated silicone gaskets with a thermal conductivity of up to 15W, which has good insulation and heat dissipation effect. It is more practical than carbon fiber thermal conductivity gaskets and is suitable for high heat source dissipation scenarios such as network servers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004134800300000051
    Figure BDA0004134800300000051
  • Figure BDA0004134800300000061
    Figure BDA0004134800300000061
  • Figure BDA0004134800300000091
    Figure BDA0004134800300000091
Patent Text Reader

Abstract

The present application relates to the field of silicone materials, and more specifically, it relates to a thermally conductive insulating silicone gasket and a preparation method thereof. The thermally conductive insulating filler comprises 2100-3750 parts of thermally conductive insulating filler, 100 parts of vinyl silicone oil, 0.05-0.1 parts of cross-linking agent, 0.5-0.8 parts of inhibitor, and 0.5-1 parts of vulcanizing agent; the thermally conductive insulating filler is composed of the following raw materials in parts by weight: 300-600 parts of nano-aluminum nitride, 900-1650 parts of aluminum nitride, and 900-1500 parts of diamond. The present application is compounded by nano-aluminum nitride, aluminum nitride, and diamond, and their properties are combined to achieve both better thermal conductivity and insulation effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of silicone materials, and more specifically, to a thermally conductive insulating silicone gasket and a preparation method thereof. Background Art

[0002] A thermal pad is a silicone sheet with heat-conducting function. It is often used in heating devices such as network servers, optical modules, military products, and drones. When used, the silicone sheet needs to be filled in the gap between the heat source and the surface of the radiator to improve the heat conduction efficiency. Currently, most of the thermally conductive silicone gaskets above 15W on the market are made of directional carbon fiber. Although carbon fiber thermal pads have good thermal conductivity, carbon fiber has a certain electrical conductivity, which makes the carbon fiber thermal pads also have a certain electrical conductivity, thus limiting its application range.

[0003] Therefore, some people proposed to use thermally conductive insulating silicone sheets, which have both insulation and thermal conductivity. However, the current thermally conductive insulating silicone sheets still have poor thermal conductivity and insulation effects, so further research on thermally conductive insulating silicone sheets is needed. Summary of the invention

[0004] In order to make the thermally conductive insulating silicone sheet have both good thermal conductivity and insulation effects, the present application provides a thermally conductive insulating silicone gasket and a preparation method thereof.

[0005] In a first aspect, the present application provides a thermally conductive insulating silicone gasket, which uses the following thermally conductive insulating silicone gasket, comprising the following raw material components in parts by weight:

[0006] Thermally conductive insulating filler 2100-3750 parts

[0007] 100 parts of vinyl silicone oil

[0008] Crosslinking agent 0.05-0.1 parts

[0009] Inhibitor 0.5-0.8 parts

[0010] Vulcanizing agent 0.5-1 part.

[0011] The composition of the above raw materials and the weight proportions of the raw materials are both within the preferred ranges of the present application, wherein vinyl silicone oil is used as a carrier, the cross-linking agent has a cross-linking effect, the inhibitor has an inhibitory effect, the vulcanizing agent has a vulcanizing effect, and the thermally conductive insulating filler has both good thermal conductivity and insulating effects, thereby being able to improve the conductivity and insulation of the thermally conductive insulating silicone sheet obtained.

[0012] Preferably, the thermally conductive insulating filler is composed of the following raw materials in parts by weight:

[0013] Nano aluminum nitride 300-600 parts

[0014] Aluminum nitride 900-1650 parts

[0015] Diamond 900-1500 pieces.

[0016] Among the above raw materials, the particle size of nano aluminum nitride is 10-50nm. The nano aluminum nitride selected in the above particle size range has good dispersibility, thermal conductivity and insulation. When used as a thermally conductive insulating silicone gasket, it can improve the thermal conductivity and heat dissipation effect of the thermally conductive insulating silicone gasket. Aluminum nitride also has the advantages of high thermal conductivity and high dielectric strength. Diamond is a mineral composed of carbon elements, and its spatial structure is a stable regular tetrahedron alternately linked, with super high thermal conductivity and insulation. Therefore, this application uses aluminum nitride, nano aluminum nitride, and diamond composite to play a synergistic role, thereby enabling the thermally conductive insulating silicone gasket to obtain better thermal conductivity and insulation effects. The thermal conductivity of the thermally conductive insulating silicone gasket prepared by this application is as high as 15w, and it has an insulating effect. Compared with the carbon fiber thermal conductive gasket, it is more practical.

[0017] Preferably, the aluminum nitride is composed of the following raw materials in parts by weight:

[0018] 5μm aluminum nitride 300-900 copies

[0019] 10μm aluminum nitride 0-750 parts

[0020] 30μm aluminum nitride 0-600 parts.

[0021] Preferably, the diamond particle size is 100-150 μm.

[0022] Diamond and boron nitride within the above particle size range are selected to combine, so that the thermally conductive insulating silicone gasket produced has both good thermal conductivity and insulation effects.

[0023] Specifically, since the thermally conductive insulating silicone sheet is coated with silicone oil and formed into a silicone sheet under auxiliary agents and high temperature, in this process, in order to make the structure of the obtained thermally conductive insulating silicone sheet more compact, fillers with different particle sizes are selected for filling; in this process, 900-1500 parts of diamond with a particle size of 100-150μm can be used as the skeleton of the thermally conductive insulating silicone sheet, and then 300-900 parts of aluminum nitride with a particle size of 5μm, 0-750 parts of aluminum nitride with a particle size of 10μm, and 0-600 parts of aluminum nitride with a particle size of 30μm are added to fill the pores formed between the diamond particles, thereby improving the compactness of the thermally conductive insulating silicone sheet structure, so that the thermal conductivity and insulation effects are better.

[0024] Furthermore, 300-600 parts of nano-aluminum nitride are added to make the structure of the thermally conductive insulating silicone sheet more compact, thereby making the thermally conductive insulating silicone sheet have better thermal conductivity and insulation properties, which is more conducive to dissipating the heat source on the network server and improving practicality.

[0025] Preferably, the viscosity of the vinyl silicone oil is 30-80 CPS.

[0026] The viscosity of the vinyl silicone oil is selected to effectively load the thermally conductive insulating filler, reduce the phenomenon of damage or collapse of the thermally conductive insulating silicone sheet, and improve its practicality. The viscosity is the viscosity at 23°C. The vinyl content of the vinyl silicone oil is 0.36-0.80%.

[0027] When the viscosity is greater than 80CPS, the viscosity is too high, which is not conducive to the uniform mixing of the thermally conductive insulating filler and the vinyl silicone oil, and thus part of the thermally conductive insulating filler is not coated by the vinyl silicone oil, and thus the obtained thermally conductive insulating silicone sheet is easy to collapse. When the viscosity is less than 30CPS, the viscosity is too low, and thus the thermally conductive insulating filler cannot be tightly connected, so that the obtained thermally conductive insulating silicone sheet is easy to collapse or break.

[0028] Preferably, the cross-linking agent is hydrogen-containing silicone oil.

[0029] Using hydrogen-containing silicone oil as a cross-linking agent can make the vinyl silicone oil cross-linked at high temperature, so as to form a sheet-like thermally conductive insulating silicone sheet.

[0030] Preferably, the vulcanizing agent is a platinum vulcanizing agent.

[0031] Platinum vulcanizer can be used as a vulcanizer for vinyl silicone oil, which facilitates the molding of the raw material system of thermally conductive insulating silicone sheets.

[0032] Preferably, the inhibitor is one or more of acetylene cyclohexanol, polyvinyl, maleate, and dihexyl maleate.

[0033] Inhibitors composed of one or more of acetylene cyclohexanol, polyvinyl, maleic acid ester, and dihexyl maleate all have good inhibitory effects and improve the quality stability of the production of thermally conductive insulating silicone gaskets.

[0034] Preferably, the nano aluminum nitride, 5 μm aluminum nitride / 10 μm aluminum nitride / 30 μm aluminum nitride, and diamond are all obtained through a surface treatment process.

[0035] Preferably, the surface treatment process of nano aluminum nitride, 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride, and diamond is as follows:

[0036] According to weight, 0.3-0.8 parts of β-hydroxypropyl acrylate, 0.7-1.3 parts of glycidyl methacrylate, and 5-8 parts of polyvinyl pyrrolidone are weighed and mixed evenly, heated to 60-80° C., 0.05-0.1 parts of ammonium persulfate are added, and stirred at a speed of 120-300 r / min for 30-50 min; 0.1-0.5 parts of Y-methacryloxytrimethoxysilane are added, and stirred at a speed of 200-500 r / min for 30-50 min to obtain a coating agent; 0.05-0.1 parts of sodium dodecyl sulfate, 1-3 parts of sodium hydroxide, 3-5 parts of ammonia water, 0.5-1 parts of sodium hexametaphosphate and 100 parts of water are weighed, and stirred evenly to obtain an activator;

[0037] Diamond surface treatment: weigh 35-45 parts of diamond by weight, add to 30-50 parts of activator, heat to 45-55°C, stir at a speed of 300-500r / min for 25-45min, filter, dry to obtain activated diamond; then weigh 2-7 parts of coating agent, add 8-15 parts of activated diamond, ball mill for 1-3h, dry, and screen the particle size to 100-150μm to obtain surface-treated diamond.

[0038] Surface treatment of nano aluminum nitride: according to weight parts, weigh 10-16 parts of coating agent and dilute it in 100 parts of anhydrous ethanol to obtain a coating solution, weigh 30-50 parts of activated nano aluminum nitride and add it to the coating solution, stir for 30-60 minutes, filter, dry, grind, and screen the particle size to 10-50nm to obtain surface-treated nano aluminum nitride.

[0039] Surface treatment of 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride: According to weight, weigh 3.5-6 parts of coating agent and dilute them in 100 parts of anhydrous ethanol solution to obtain a coating solution, then weigh 10-20 parts of 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride and mix them with the coating solution, stir for 40-70 minutes, and dry to obtain surface-treated 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride.

[0040] Since diamond, nano-aluminum nitride, and aluminum nitride are all inorganic fillers, their surfaces are highly inert and thus difficult to compound with vinyl silicone oil. Therefore, surface modification is required to improve their compatibility and dispersibility in the thermally conductive insulating silicone sheet raw material system.

[0041] Acrylic acid-β-hydroxypropyl ester is used as a cross-linking monomer and has good adhesion, while glycidyl methacrylate has good adhesion and adsorption, etc. Polyvinyl pyrrolidone has film-forming properties and adhesion, and Y-methacryloxytrimethoxysilane is a coupling agent and can serve as a connecting bridge between the inorganic filler and the polymer. Therefore, the present application compounds acrylate-β-hydroxypropyl ester, glycidyl methacrylate, polyvinyl pyrrolidone, and Y-methacryloxytrimethoxysilane under the action of ammonium persulfate, and combines their properties to obtain a coating agent that has good film-forming properties, adhesion, and compatibility with the polymer.

[0042] The present invention uses sodium dodecyl sulfate as a surfactant, sodium hydroxide and ammonia water as hydroxyl ions as alkaline regulators, and sodium hexametaphosphate as a stabilizer. The activator thus obtained has a good activation effect.

[0043] Specifically, in the diamond surface treatment process: since the surface inertness of diamond is relatively large, the present application activates its surface through an activation liquid during the surface treatment process, and the activation liquid needs to be stirred for 25-45 minutes at a heating temperature of 45-55°C and a rotation speed of 300-500r / min to fully activate the diamond surface and reduce the surface inertness of the diamond. The coating agent and the activated diamond are then ball-milled to fully coat the surface of the activated diamond with the coating agent, so that a coating film is formed on the surface of the surface-treated diamond. When the diamond is used in a thermally conductive insulating silicone sheet, it can be fully and evenly mixed with the raw material system of the thermally conductive insulating silicone sheet, thereby improving the density, thermal conductivity and insulation of the thermally conductive insulating silicone sheet structure.

[0044] The surface inertness of nano aluminum nitride, 5μm aluminum nitride, 10μm aluminum nitride, and 30μm aluminum nitride is lower than that of diamond. Therefore, there is no need for activation. Instead, the coating agent is diluted and then the surface treatment is performed. This method is not only simple to operate, but also has high production efficiency.

[0045] The diamond, nano aluminum nitride, 5μm aluminum nitride, 10μm aluminum nitride, and 30μm aluminum nitride of the present application are surface treated and then used in combination with vinyl silicone oil to improve the describing property and dispersibility of the thermally conductive insulating filler in the raw material system, thereby improving the thermal conductivity and insulation of the thermally conductive insulation.

[0046] In a second aspect, the present application provides a method for preparing a thermally conductive insulating silicone gasket, which adopts the following technical scheme: 1) weighing vinyl silicone oil, a crosslinking agent, nano-aluminum nitride and aluminum nitride in parts by weight, heating to 140-160° C., stirring for 25-45 minutes, and obtaining a mixture A;

[0047] 2) Weigh diamond according to parts by weight, add it to the mixture A obtained in 1), stir for 20-40 minutes, and cool to obtain a mixture B;

[0048] 3) Weigh the inhibitor and the vulcanizing agent according to parts by weight, mix them evenly with the mixture B obtained in 2), evacuate the mixture, calender the mixture, and heat and cure the mixture in an oven at 120-150° C. to obtain a thermally conductive silicone gasket.

[0049] In summary, this application has the following beneficial effects:

[0050] 1. The present application uses aluminum nitride, nano aluminum nitride, and diamond composite to achieve synergistic effects, thereby enabling the thermally conductive insulating silicone gasket to obtain better thermal conductivity and insulation effects. The thermally conductive insulating silicone gasket prepared by the present application has a thermal conductivity of up to 15w and has an insulating effect. Compared with carbon fiber thermal conductive gaskets, it is more practical;

[0051] 2. By using aluminum nitride of different particle sizes to fill in a certain weight ratio, the structure of the thermally conductive insulating silicone sheet is made denser, so that the thermally conductive insulating silicone sheet has both better thermal conductivity and insulation properties. This is more conducive to dissipating the heat source on the network server and improving practicality.

[0052] 3. Diamond, nano aluminum nitride, 5μm aluminum nitride, 10μm aluminum nitride, and 30μm aluminum nitride are surface treated and then combined with vinyl silicone oil to improve the describing and dispersibility of thermal conductive insulation fillers in the raw material system, thereby improving the thermal conductivity and insulation of thermal conductive insulation. DETAILED DESCRIPTION

[0053] The present application is further described in detail below with reference to the embodiments.

[0054] Example

[0055] Example 1

[0056] A thermally conductive insulating silicone gasket is prepared by the following method:

[0057] 1) Weigh 100 g of vinyl silicone oil, 0.1 g of a crosslinking agent (hydrogen-containing silicone oil), 600 g of nano aluminum nitride, 600 g of 5 μm aluminum nitride, and 300 g of 10 μm aluminum nitride into a kneader, heat to 150° C., and stir for 30 min to obtain a mixture A;

[0058] 2) Weigh 1500 g of diamond, add the mixture A obtained in 1), stir for 30 min, and cool to room temperature to obtain a mixture B;

[0059] 3) Weigh 0.5 g of acetylene cyclohexanol and 0.5 g of a vulcanizing agent (inhibitor), mix them evenly with the mixture B obtained in 2), evacuate the mixture, roll the mixture into a shape, and heat and cure the mixture in an oven at 130° C. to obtain a thermally conductive silicone gasket.

[0060] The viscosity of the vinyl silicone oil is 50 CPS, the particle size of the diamond is 120 μm, and the particle size of the nano-aluminum nitride is 30 nm; the hydrogen content of the hydrogen-containing silicone oil is 1.55%.

[0061] Embodiment 2-5

[0062] The difference between Example 2-5 and Example 1 is that the amount of raw materials used is different, as shown in Table 1;

[0063] Table 1 Raw materials (g) and process parameters of Examples 1-5

[0064]

[0065]

[0066] Example 6

[0067] The difference between Example 6 and Example 1 is that the nano aluminum nitride, 5 μm aluminum nitride, 10 μm aluminum nitride, 30 μm aluminum nitride, and diamond are all surface treated;

[0068] The specific treatment process is as follows:

[0069] Weigh 0.3 kg of β-hydroxypropyl acrylate, 0.7 kg of glycidyl methacrylate, and 5 kg of polyvinyl pyrrolidone, mix them evenly, heat to 60° C., add 0.05 kg of ammonium persulfate, and stir at a speed of 120 r / min for 30 min; add 0.1 kg of Y-methacryloxytrimethoxysilane, and stir at a speed of 200 r / min for 30 min to obtain a coating agent; weigh 0.005 kg of sodium dodecyl sulfate, 0.1 kg of sodium hydroxide, 0.3 kg of ammonia water, 0.05 kg of sodium hexametaphosphate, and 10 kg of water, and stir until the sodium hydroxide and sodium dodecyl sulfate are completely dissolved to obtain an activator;

[0070] Diamond surface treatment: Weigh 0.35kg of diamond, add it to 0.3kg of activator, heat to 45℃, stir at a speed of 300r / min for 0.8h, filter, put it into a 50℃ oven for drying to obtain activated diamond; then weigh 2kg of coating agent, put it into a ball mill together with 8kg of activated diamond, ball mill for 1h, and then put it into a 50℃ oven for drying for 2h, screen the particle size to 100μm, and obtain surface-treated diamond.

[0071] Surface treatment of nano-aluminum nitride: weigh 1 kg of coating agent and dilute it in 10 kg of anhydrous ethanol to obtain a coating solution, weigh 3 kg of activated nano-aluminum nitride and add it to the coating solution, stir for 30 minutes, filter, and then put it in an oven at 50°C to dry for 2 hours, grind, and screen the particle size to 10 nm to obtain surface-treated nano-aluminum nitride.

[0072] Surface treatment of 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride: weigh 0.35kg of coating agent and dilute it in 10kg of anhydrous ethanol solution to obtain a coating solution, then weigh 10kg of 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride and mix them with the coating solution, stir for 40 minutes, and dry to obtain surface-treated 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride.

[0073] Example 7

[0074] The difference between Example 7 and Example 6 is that the nano aluminum nitride, 5 μm aluminum nitride, 10 μm aluminum nitride, 30 μm aluminum nitride, and diamond are all surface treated;

[0075] The specific treatment process is as follows:

[0076] Weigh 0.5 kg of β-hydroxypropyl acrylate, 1 kg of glycidyl methacrylate, and 6 kg of polyvinyl pyrrolidone, mix them evenly, heat to 70° C., add 0.08 kg of ammonium persulfate, and stir at a speed of 200 r / min for 40 min; add 0.3 kg of Y-methacryloxytrimethoxysilane, and stir at a speed of 300 r / min for 40 min to obtain a coating agent; weigh 0.008 kg of sodium dodecyl sulfate, 0.2 kg of sodium hydroxide, 0.4 kg of ammonia water, 0.08 kg of sodium hexametaphosphate, and 10 kg of water, and stir until the sodium hydroxide and sodium dodecyl sulfate are completely dissolved to obtain an activator;

[0077] Diamond surface treatment: Weigh 0.40kg of diamond, add it to 0.4kg of activator, heat to 50℃, stir at a speed of 400r / min for 30min, filter, put it into a 50℃ oven for drying to obtain activated diamond; then weigh 5kg of coating agent, put it into a ball mill together with 12kg of activated diamond, ball mill for 2h, and then put it into a 50℃ oven for drying for 2h. The particle size is screened to 120μm to obtain surface-treated diamond.

[0078] Surface treatment of nano-aluminum nitride: weigh 1.3 kg of coating agent and dilute it in 10 kg of anhydrous ethanol to obtain a coating solution; weigh 4 kg of activated nano-aluminum nitride and add it to the coating solution, stir for 50 minutes, filter, and then put it in an oven at 50°C to dry for 2 hours, grind, and screen the particle size to 20 nm to obtain surface-treated nano-aluminum nitride.

[0079] Surface treatment of 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride: weigh 0.5kg of coating agent and dilute it in 10kg of anhydrous ethanol solution to obtain a coating solution, then weigh 15kg of 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride and mix them with the coating solution, stir for 55 minutes, and dry to obtain surface-treated 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride.

[0080] Example 8

[0081] The difference between Example 8 and Example 6 is that the nano aluminum nitride, 5 μm aluminum nitride, 10 μm aluminum nitride, 30 μm aluminum nitride, and diamond are all surface treated;

[0082] The specific treatment process is as follows:

[0083] Weigh 0.8 kg of β-hydroxypropyl acrylate, 1.3 kg of glycidyl methacrylate, and 8 kg of polyvinyl pyrrolidone, mix them evenly, heat to 70°C, add 0.1 kg of ammonium persulfate, and stir at a speed of 300 r / min for 50 min; add 0.5 kg of Y-methacryloxytrimethoxysilane, and stir at a speed of 500 r / min for 50 min to obtain a coating agent; weigh 0.01 kg of sodium dodecyl sulfate, 0.3 kg of sodium hydroxide, 0.5 kg of ammonia water, 0.1 kg of sodium hexametaphosphate, and 10 kg of water, and stir until the sodium hydroxide and sodium dodecyl sulfate are completely dissolved to obtain an activator;

[0084] Diamond surface treatment: Weigh 0.45kg of diamond, add it to 0.5kg of activator, heat to 55℃, stir at a speed of 500r / min for 45min, filter, put it into a 50℃ oven for drying to obtain activated diamond; then weigh 7kg of coating agent, put it into a ball mill together with 15kg of activated diamond, ball mill for 3h, and then put it into a 50℃ oven for drying for 2h, and screen the particle size to 150μm to obtain surface-treated diamond.

[0085] Surface treatment of nano-aluminum nitride: weigh 1.6 kg of coating agent and dilute it in 10 kg of anhydrous ethanol to obtain a coating solution; weigh 4 kg of activated nano-aluminum nitride and add it to the coating solution, stir for 60 minutes, filter, and then put it into an oven at 50°C to dry for 2 hours, grind, and screen the particle size to 30 nm to obtain surface-treated nano-aluminum nitride.

[0086] Surface treatment of 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride: weigh 0.6kg of coating agent and dilute it in 10kg of anhydrous ethanol solution to obtain a coating solution, then weigh 20kg of 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride and mix them with the coating solution, stir for 70 minutes, and dry to obtain surface-treated 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride.

[0087] Comparative Example

[0088] Comparative Example 1

[0089] The difference between Comparative Example 1 and Example 1 is that an equal amount of nano-aluminum nitride is replaced by 5 μm aluminum nitride.

[0090] Comparative Example 2

[0091] The difference between Comparative Example 2 and Example 1 is that 5 μm aluminum nitride is replaced by 10 μm aluminum nitride in equal amounts.

[0092] Comparative Example 3

[0093] The difference between Comparative Example 3 and Example 1 is that an equal amount of diamond is replaced by 30 μm aluminum nitride.

[0094] Comparative Example 4

[0095] The difference between Comparative Example 4 and Example 1 is that an equal amount of diamond is replaced by 120 μm hexagonal boron nitride.

[0096] Comparative Example 5

[0097] The difference between Comparative Example 5 and Example 1 is that the amount of diamond used is 1800 g, and the amount of 5 μm aluminum nitride used is 0 g.

[0098] Performance testing

[0099] Detection method / test method

[0100] The thermally conductive insulating silicone sheets obtained in Examples 1-8 and Comparative Examples 1-5 were subjected to the following performance tests.

[0101] 1. Refer to ISO22007-2 to test thermal conductivity;

[0102] 2. Refer to ASTM D257 to test volume resistance;

[0103] 3. Refer to ASTM D149 to test the dielectric strength;

[0104] 4. Rubber material state: observe the rubber material state of the obtained thermally conductive insulating silicone sheet. When the obtained thermally conductive insulating silicone sheet is good and has no defects, it is in good loading state. When the thermally conductive insulating silicone sheet collapses or is not in sheet form, it is unqualified.

[0105] Specifically, the data are shown in Table 2 below;

[0106] Table 2 Experimental data of Examples 1-8 and 1-5

[0107]

[0108] Combining Example 1 with Comparative Examples 1-3 and Table 3, it can be seen that the volume resistivity, thermal conductivity and dielectric strength of Example 1 are all higher than those of Comparative Examples 1-3. This indicates that when nano aluminum nitride / 5 μm aluminum nitride / diamond is not added, the thermal conductivity and insulation effects of the thermally conductive insulating silicone sheet are reduced.

[0109] Comparing Examples 1-8 with Comparative Example 4, the thermal conductivity of Comparative Example 4 is only 11.129, while the thermal conductivity of Example 1 is as high as 19.827, indicating that the thermal conductivity effect of adding diamond is better. Moreover, the dielectric strength and volume resistivity of Example 1 are higher than those of the comparative example, indicating that the insulation effect of adding diamond is better.

[0110] Comparing Example 1 with Comparative Example 5, the rubber material of Comparative Example 5 shows a phenomenon of disintegration, which indicates that the silicone sheet obtained within the raw material range of the present application is easy to form a thermal conductive sheet and is not prone to disintegration.

[0111] Comparing Example 1 and Example 6, the volume resistivity, thermal conductivity and dielectric strength of Example 6 are all higher than those of Example 1, indicating that the surface-treated nano-aluminum nitride, aluminum nitride and diamond can be evenly mixed with the raw material system of the thermally conductive insulating silicone sheet, so that the thermally conductive insulating silicone sheet can obtain better thermal conductivity and insulation effects.

[0112] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A thermally conductive insulating silicone gasket, characterized in that: The invention comprises the following raw materials in parts by weight: Thermally conductive insulating filler 2100-3750 parts 100 parts of vinyl silicone oil Crosslinking agent 0.05-0.1 parts Inhibitor 0.5-0.8 parts Vulcanizing agent 0.5-1 part; The thermally conductive insulating filler is composed of the following raw materials in parts by weight: Nano aluminum nitride 300-600 parts Aluminum nitride 900-1650 parts Diamond 900-1500 parts; The aluminum nitride is composed of the following raw materials in parts by weight: 5μm aluminum nitride 300-900 copies 10μm aluminum nitride 0-750 parts 30μm aluminum nitride 0-600 parts; Nano-aluminum nitride is 30nm; The nano aluminum nitride, 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride, and diamond are all made through a surface treatment process; The surface treatment processes of nano aluminum nitride, 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride and diamond are as follows: According to weight, 0.3-0.8 parts of β-hydroxypropyl acrylate, 0.7-1.3 parts of glycidyl methacrylate, and 5-8 parts of polyvinyl pyrrolidone are weighed and mixed evenly, heated to 60-80° C., 0.05-0.1 parts of ammonium persulfate are added, and stirred at a speed of 120-300 r / min for 30-50 min; 0.1-0.5 parts of Y-methacryloxytrimethoxysilane are added, and stirred at a speed of 200-500 r / min for 30-50 min to obtain a coating agent; 0.05-0.1 parts of sodium dodecyl sulfate, 1-3 parts of sodium hydroxide, 3-5 parts of ammonia water, 0.5-1 parts of sodium hexametaphosphate and 100 parts of water are weighed, and stirred evenly to obtain an activator; Diamond surface treatment: according to weight, weigh 35-45 parts of diamond, add to 30-50 parts of activator, heat to 45-55°C, stir at a speed of 300-500r / min for 25-45min, filter, dry to obtain activated diamond; then weigh 2-7 parts of coating agent, add 8-15 parts of activated diamond, ball mill for 1-3h, dry, screen the particle size to 100-150μm, and obtain surface-treated diamond; Surface treatment of nano aluminum nitride: according to weight, weigh 10-16 parts of coating agent and dilute it in 100 parts of anhydrous ethanol to obtain a coating solution, weigh 30-50 parts of activated nano aluminum nitride and add it to the coating solution, stir for 30-60 minutes, filter, dry, grind, and screen the particle size of 10-50nm to obtain surface-treated nano aluminum nitride; Surface treatment of 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride: According to weight, weigh 3.5-6 parts of coating agent and dilute them in 100 parts of anhydrous ethanol solution to obtain a coating solution, then weigh 10-20 parts of 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride and mix them with the coating solution, stir for 40-70 minutes, and dry to obtain surface-treated 5μm aluminum nitride / 10μm aluminum nitride / 30μm aluminum nitride.

2. A thermally conductive insulating silicone gasket according to claim 1, characterized in that: The diamond particle size is 100-150 μm.

3. A thermally conductive insulating silicone gasket according to claim 1, characterized in that: The viscosity of the vinyl silicone oil is 30-80 CPS.

4. The thermally conductive insulating silicone gasket according to claim 1, characterized in that: The cross-linking agent is hydrogen-containing silicone oil.

5. The thermally conductive insulating silicone gasket according to claim 1, characterized in that: The vulcanizing agent is a platinum vulcanizing agent.

6. The thermally conductive insulating silicone gasket according to claim 1, characterized in that: The inhibitor is one or more of acetylene cyclohexanol, polyvinyl, maleate, and dihexyl maleate.

7. A method for preparing a thermally conductive insulating silicone gasket as claimed in any one of claims 1 to 6, characterized in that: The following steps are involved: 1) Weigh vinyl silicone oil, crosslinking agent, nano aluminum nitride and aluminum nitride according to weight, mix, heat to 140-160° C., and stir for 25-45 minutes to obtain mixture A; 2) According to parts by weight, weigh diamond, add 1) obtained mixture A, stir for 20-40min, cool, to obtain a mixture B; 3) Weigh the inhibitor and the vulcanizing agent in parts by weight, mix them evenly with the mixture B obtained in 2), evacuate the mixture, calender the mixture, and heat and cure the mixture in an oven at 120-150° C. to obtain a thermally conductive silicone gasket.

Citation Information

Patent Citations

  • Nano-diamond-containing high-power LED heat dissipation ceramic substrate

    CN106220182A

  • Heat-conducting gasket and preparation method thereof

    CN115260998A

  • Heat-conducting sheet and manufacturing method thereof

    KR101552636B1

  • Diamond-based thermally conductive filler and preparation method, composite thermally conductive material and electronic device

    WO2023024570A1