A high-toughness anti-rust protective film and its processing technology

Through the multi-layer structure of high-tough anti-rust protective film, combined with the wire braided layer of radiation crosslinked polyolefin heat shrinkable material and anti-rust oil, the problem of insufficient toughness of the existing liquid protective film is solved, and efficient rust prevention for metal objects is achieved and impact resistance.

CN116218396BActive Publication Date: 2024-12-06TAICANG HONGYUN PACKAGING MATERIAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211479542.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-24
Publication Date
2024-12-06
Estimated Expiration
2042-11-24

AI Technical Summary

Technical Problem

The existing liquid protective film has low toughness and cannot effectively resist external shocks, resulting in small-scale corrosion of metal products that have not been processed during long-term storage.

Method used

High tough rust-proof protective film with multi-layer structure, including copolypropylene layer, linear low-density polyethylene layer, sealed hot melt adhesive layer, high-pressure polyethylene layer and polyvinyl chloride layer, combined with radiation crosslinked polyolefin heat shrinkable material wire The braided layer and anti-rust oil form a high-tough composite film through extrusion film formation and multi-film gluing process.

Benefits of technology

It improves the waterproofing ability and rust resistance of the composite film, enhances the protection of metal objects, reduces the possibility of rust, and takes into account toughness, flexibility and electrical insulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116218396B_ABST
    Figure CN116218396B_ABST
Patent Text Reader

Abstract

The invention discloses a high-toughness anti-rust protective film and a processing technology thereof, and relates to the technical field of protective films; the high-toughness anti-rust protective film comprises a copolymerized polypropylene layer, the lower surface of the copolymerized polypropylene layer is bonded with a linear low-density polyethylene layer, the lower surface of the linear low-density polyethylene layer is bonded with a sealing hot-melt adhesive layer, the lower surface of the sealing hot-melt adhesive layer is bonded with a high-pressure polyethylene layer, and the lower surface of the high-pressure polyethylene layer is bonded with a polyvinyl chloride layer; the processing technology comprises the following steps: S1: melting polymer raw materials; melting copolymerized polypropylene, linear low-density polyethylene, sealing hot-melt adhesive, high-pressure polyethylene, polyvinyl chloride and radiation cross-linked polyolefin heat shrinkable material respectively. The high-toughness anti-rust protective film enhances the waterproof ability of the composite film by setting the copolymerized polypropylene layer, and cooperates with anti-rust oil to improve the protection of the composite film to metal objects and reduce the possibility of rusting of metal objects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of protective films, and in particular to a high-toughness anti-rust protective film and a processing technology thereof. Background Art

[0002] Protective film is used in the industrial field to protect product surfaces, product production activities, product shipments, product circulation and other links. It not only improves the product yield, but also effectively enhances the product value.

[0003] The existing protective films are mainly used to protect objects, mainly dust and rain, and some protective films have fire resistance and anti-static capabilities. For metal products, anti-rust is the most critical.

[0004] Rust is a chemical reaction, essentially an oxidation reaction of metals. The most common rust phenomenon is that iron products are exposed to the air for a long time and undergo an oxidation reaction with oxygen, or are corroded by oxygen in water to become oxides.

[0005] Existing metal products are mostly treated with rust inhibitors. However, for metal products that have not been processed and need to be stored, applying rust inhibitors is obviously not reasonable. Protective films are often used to isolate the contact between external oxygen and moisture and the metal. However, after long-term storage, metal products will still suffer from small-scale rust.

[0006] After searching, the Chinese patent application number CN201110189434.7 discloses a peelable heat-resistant and rust-proof protective film coating and a preparation method thereof, comprising a paint and a curing agent, the weight ratio of the paint and the curing agent being 100:(25-40); the paint comprises the following components and their weight contents: 88-96 of a hydroxyl-containing straight-chain polyester resin or acrylic resin; 2.0-5.0 of a peeling accelerator; 1.0-3.0 of a film-forming accelerator; 0.5-2.0 of a defoaming agent; and 0.5-2.0 of a leveling agent; and the curing agent is an isocyanate polymer.

[0007] The device in the above patent has the following deficiencies: the protective film is a liquid protective film, which is sprayed on the metal surface and forms a protective film after solidification, and has a certain anti-rust ability;

[0008] However, the toughness of the liquid protective film itself is relatively low, and its resistance to external impact is relatively weak. Summary of the invention

[0009] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a high-toughness anti-rust protective film and a processing technology thereof.

[0010] In order to achieve the above object, the present invention adopts the following technical solutions:

[0011] A high-toughness anti-rust protective film, comprising:

[0012] A co-polypropylene layer, a linear low-density polyethylene layer is bonded to the lower surface of the co-polypropylene layer, a sealing hot-melt adhesive layer is bonded to the lower surface of the linear low-density polyethylene layer, a high-pressure polyethylene layer is bonded to the lower surface of the sealing hot-melt adhesive layer, and a polyvinyl chloride layer is bonded to the lower surface of the high-pressure polyethylene layer;

[0013] A radiation cross-linked polyolefin heat shrinkable material thread braided layer is arranged inside the sealing hot melt adhesive layer, anti-rust oil is arranged on the lower surface of the polyvinyl chloride layer, and a polypropylene film is arranged on the lower surface of the polyvinyl chloride layer to prevent the anti-rust oil from failing or contaminating the co-polypropylene layer.

[0014] As a preferred embodiment of the present invention, the copolymerized polypropylene layer, the linear low-density polyethylene layer, the high-pressure polyethylene layer and the polyvinyl chloride layer are extruded into a film.

[0015] As a preferred embodiment of the present invention, the radiation cross-linked polyolefin heat shrinkable material thread braided layer is woven from a plurality of radiation cross-linked polyolefin heat shrinkable material warps and wefts, and two adjacent radiation cross-linked polyolefin heat shrinkable material warps or wefts are equidistantly arranged.

[0016] As a preferred embodiment of the present invention, the sealing hot melt adhesive layer is provided as two layers of upper and lower hot melt adhesive films, and the radiation cross-linked polyolefin heat shrinkable material wire braided layer is provided between the two hot melt adhesive films.

[0017] A processing technology for a high-toughness anti-rust protective film comprises the following steps:

[0018] S1: Melting polymer raw materials; melting copolymer polypropylene, linear low-density polyethylene, sealing hot melt adhesive, high-pressure polyethylene, polyvinyl chloride and radiation cross-linked polyolefin heat shrinkable materials respectively;

[0019] S2: extrusion film forming; extruding co-polypropylene, linear low-density polyethylene, sealing hot melt adhesive, high-pressure polyethylene, and polyvinyl chloride into films respectively, and pre-treating them; extruding radiation cross-linked polyolefin heat shrinkable material and weaving it according to warp and weft arrangement, and compounding it with the sealing hot melt adhesive film;

[0020] S3: multi-film bonding; bonding a co-polypropylene film, a linear low-density film, a sealing hot-melt adhesive film, a high-pressure polyethylene film and a polyvinyl chloride film to form a composite film;

[0021] S4: Anti-rust oil spraying: spray anti-rust oil on the surface of the polyvinyl chloride film of the composite film;

[0022] S5: film coating and rolling; covering the surface of the polyvinyl chloride film with a polypropylene film, and then rolling it up.

[0023] On the basis of the above scheme: the extrusion film forming comprises the following steps;

[0024] S21: extrusion molding; extruding various raw materials in a molten state into films or extrusion wires as needed;

[0025] S22: film pretreatment; irradiating a copolypropylene film, a linear low-density film, a high-pressure polyethylene film and a polyvinyl chloride film with Co60 gamma rays, and then biaxially stretching the film at a temperature of 150°C;

[0026] S23: weaving radiation cross-linked polyolefin heat shrinkable material threads; extruding and drawing the radiation cross-linked polyolefin heat shrinkable material and arranging the threads according to warp and weft to weave into a layer;

[0027] S24: hot melt lamination; covering the upper and lower surfaces of the radiation cross-linked polyolefin heat shrinkable material wire braided layer with two sealing hot melt adhesive films, and heating the two sealing hot melt adhesive films to fuse them and fix them to the radiation cross-linked polyolefin heat shrinkable material wire braided layer.

[0028] On the basis of the above scheme: the multi-film bonding comprises the following steps;

[0029] S31: Glue coating on film surface; introducing co-polypropylene film, linear low-density film, sealing hot melt adhesive film, high-pressure polyethylene film and polyvinyl chloride film into a five-layer co-extrusion film blowing machine, and applying adhesive on the film surface;

[0030] S32: co-extrusion film blowing; extruding the plurality of films mentioned above through a five-layer co-extrusion film blowing machine, and finally forming a composite film;

[0031] S33: trimming into a roll; trimming the edge of the composite film and rolling it up.

[0032] The beneficial effects of the present invention are:

[0033] 1. The high-toughness anti-rust protective film enhances the waterproof ability of the composite film by setting a copolymerized polypropylene layer, and cooperates with anti-rust oil to improve the protection of the composite film to metal objects and reduce the possibility of rust on metal objects.

[0034] 2. This high-toughness anti-rust protective film is formed by mixing a variety of polymer materials and mixing multiple materials into a film. When combined with anti-rust oil to ensure the anti-rust ability of the film, it also takes into account toughness, flexibility, electrical insulation and other capabilities to comprehensively improve the performance of the film. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a schematic diagram of the cross-sectional structure of the protective film of the present invention;

[0036] Figure 2 It is a schematic diagram of the preparation process of the protective film of the present invention.

[0037] In the figure: 1. Co-polypropylene layer; 2. Linear low-density polyethylene layer; 3. Sealing hot-melt adhesive layer; 4. Radiation cross-linked polyolefin heat shrinkable material wire braided layer; 5. High-pressure polyethylene layer; 6. Polyvinyl chloride layer. DETAILED DESCRIPTION

[0038] The technical solution of this patent is further described in detail below in conjunction with specific implementation methods.

[0039] The embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0040] Embodiment 1;

[0041] A high-toughness anti-rust protective film and its processing technology, such as Figure 1 As shown, including:

[0042] A co-polypropylene layer 1, a linear low-density polyethylene layer 2 is bonded to the lower surface of the co-polypropylene layer 1, a sealing hot-melt adhesive layer 3 is bonded to the lower surface of the linear low-density polyethylene layer 2, a high-pressure polyethylene layer 5 is bonded to the lower surface of the sealing hot-melt adhesive layer 3, and a polyvinyl chloride layer 6 is bonded to the lower surface of the high-pressure polyethylene layer 5;

[0043] The inside of the sealing hot melt adhesive layer 3 is provided with a radiation cross-linked polyolefin heat shrinkable material wire braided layer 4, the lower surface of the polyvinyl chloride layer 6 is provided with anti-rust oil, and the lower surface of the polyvinyl chloride layer 6 is provided with a polypropylene film;

[0044] When the film is in use, the side of the polyvinyl chloride layer 6 coated with the anti-rust oil directly contacts the surface of the metal object; the polypropylene film has good flexibility and is coated on the lower surface of the polyvinyl chloride layer 6, so as to maintain the anti-rust effect of the anti-rust oil.

[0045] The copolymerized polypropylene layer 1, the linear low-density polyethylene layer 2, the high-pressure polyethylene layer 5 and the polyvinyl chloride layer 6 are extruded into a film with a thickness of 0.05 mm. The sealing hot-melt adhesive layer 3 has a thickness of 0.05 mm.

[0046] The co-polypropylene film is made of polypropylene random copolymer, which improves the optical properties (increases transparency and reduces haze), improves impact resistance, increases flexibility, reduces melting temperature, and thus also reduces the hot-melt temperature;

[0047] At the same time, the chemical stability, water vapor barrier properties and organoleptic properties (low odor and taste) are basically the same as homopolymers, reducing the possibility of water vapor passing through the film and contacting the surface of metal objects, reducing the probability of rust.

[0048] Linear low-density polyethylene is a molecular structure formed by copolymerization of ethylene and a small amount of α-olefin on the main chain of linear ethylene with very short comonomer side chains. In addition to the properties of general polyolefin resins, it has particularly excellent tensile strength, tear strength, environmental stress cracking resistance, low temperature resistance, heat resistance and puncture resistance.

[0049] After the linear low-density polyethylene is formed into a film, it is combined with a copolymerized polypropylene film to effectively improve the toughness of the film, enhance the film's ability to resist external impact, and reduce damage to the surface of the metal object wrapped by the film caused by external objects.

[0050] High-pressure polyethylene, also known as low-density polyethylene (LDPE), has excellent electrical insulation, good softness, good impact resistance and transparency, and good air permeability;

[0051] High-pressure polyethylene film can effectively reduce the adhesion of external free electrons and prevent free electrons from gathering on the surface of metal objects.

[0052] Polyvinyl chloride is a polymer formed by the polymerization of vinyl chloride monomer (VCM) in the presence of initiators such as peroxides and azo compounds or under the action of light or heat according to the free radical polymerization mechanism;

[0053] It has no fixed melting point, starts to soften at 80-85℃, becomes viscoelastic at 130℃, and turns into viscous flow at 160-180℃; it has good mechanical properties, with a tensile strength of about 60MPa and an impact strength of 5-10kJ / m 2 ; Excellent dielectric properties;

[0054] The polyvinyl chloride film is in direct contact with the surface of the metal object. During the heat shrinkage process, a certain adhesive connection can be established with the surface of the metal object to ensure the stability of the overall heat shrinkage of the film.

[0055] The radiation cross-linked polyolefin heat shrinkable material thread braided layer 4 is woven by multiple radiation cross-linked polyolefin heat shrinkable material warp threads and weft threads, and two adjacent radiation cross-linked polyolefin heat shrinkable material warp threads or weft threads are equidistantly arranged; the radiation cross-linked polyolefin heat shrinkable material has good heat shrinkage memory ability. After drawing, it is woven in the vertical and horizontal arrangements to effectively enhance the toughness of the overall film.

[0056] The sealing hot melt adhesive layer 3 is provided as two layers of hot melt adhesive films, the radiation cross-linked polyolefin heat shrinkable material thread braided layer 4 is provided between the two hot melt adhesive films, the thickness of the single layer of hot melt adhesive film is 0.03 mm, and the diameter of the radiation cross-linked polyolefin heat shrinkable material thread is 0.025 mm;

[0057] When the hot melt adhesive film is compounded with the radiation cross-linked polyolefin heat shrinkable material thread braided layer 4, one side surface of the hot melt adhesive is heated, and the heated surfaces of the two hot melt adhesive films are directly attached to the radiation cross-linked polyolefin heat shrinkable material thread braided layer 4, wrapping the radiation cross-linked polyolefin heat shrinkable material thread braided layer 4.

[0058] Embodiment 2:

[0059] A high-toughness anti-rust protective film processing technology, used to process a high-toughness anti-rust protective film described in Example 1, such as Figure 2 As shown, the following steps are included:

[0060] S1: Melting polymer raw materials; melting copolymer polypropylene, linear low-density polyethylene, sealing hot melt adhesive, high-pressure polyethylene, polyvinyl chloride and radiation cross-linked polyolefin heat shrinkable materials respectively;

[0061] The raw material melting includes the following steps;

[0062] S11: Co-polypropylene, linear low-density polyethylene, sealing hot melt adhesive, high-pressure polyethylene, polyvinyl chloride and radiation cross-linked polyolefin heat shrink materials are melted separately according to their own properties;

[0063] S12: After melting, filtering is performed to remove impurities;

[0064] S2: extrusion film forming; extruding co-polypropylene, linear low-density polyethylene, sealing hot melt adhesive, high-pressure polyethylene, and polyvinyl chloride into films respectively, and pre-treating them; extruding radiation cross-linked polyolefin heat shrinkable material and weaving it according to warp and weft arrangement, and compounding it with the sealing hot melt adhesive film;

[0065] Extrusion film forming comprises the following steps:

[0066] S21: extrusion molding; extruding various raw materials in a molten state into films or extrusion wires as needed;

[0067] S22: film pretreatment; irradiating a copolypropylene film, a linear low-density film, a high-pressure polyethylene film and a polyvinyl chloride film with Co60 gamma rays, and then biaxially stretching the film at a temperature of 150°C;

[0068] S23: weaving radiation cross-linked polyolefin heat shrinkable material threads; extruding and drawing the radiation cross-linked polyolefin heat shrinkable material and arranging the threads according to warp and weft to weave into a layer;

[0069] S24: hot melt lamination; covering the upper and lower surfaces of the radiation cross-linked polyolefin heat shrinkable material wire braided layer with two sealing hot melt adhesive films, and heating the two sealing hot melt adhesive films to fuse them and fix them to the radiation cross-linked polyolefin heat shrinkable material wire braided layer.

[0070] S3: multi-film bonding; bonding a co-polypropylene film, a linear low-density film, a sealing hot-melt adhesive film, a high-pressure polyethylene film and a polyvinyl chloride film to form a composite film;

[0071] Multi-film bonding includes the following steps:

[0072] S31: Glue coating on film surface; introducing co-polypropylene film, linear low-density film, sealing hot melt adhesive film, high-pressure polyethylene film and polyvinyl chloride film into a five-layer co-extrusion film blowing machine, and applying adhesive on the film surface;

[0073] S32: co-extrusion film blowing; extruding the plurality of films mentioned above through a five-layer co-extrusion film blowing machine, and finally forming a composite film;

[0074] S33: trimming into a roll; trimming the edge of the composite film and rolling it up.

[0075] S4: Anti-rust oil spraying: spray anti-rust oil evenly on the surface of the polyvinyl chloride film of the composite film;

[0076] S5: film coating and winding; covering the surface of the polyvinyl chloride film with a polypropylene film, and then winding it through a winding device.

[0077] Embodiment three;

[0078] On the basis of the first and second embodiments, the various raw materials of the first embodiment are removed from the sealing hot melt adhesive, mixed in a certain proportion, and then melted, co-extruded, blown film, treated, sprayed with anti-rust oil, etc., and then rolled;

[0079] A variety of polymer raw materials are mixed to form a film with a thickness of 0.05 mm to 0.3 mm, which fully guarantees the high toughness and waterproof ability of the mixed film. Combined with anti-rust oil, it reduces the possibility of rust on metal objects.

[0080] The mass percentages of the various raw materials mixed into the film are: 20-30% copolymerized polypropylene, 10-20% linear low-density polyethylene, 15-35% radiation cross-linked polyolefin heat shrinkable material, 15-30% high-pressure polyethylene, and 10-35% polyvinyl chloride;

[0081] Material ratio scheme 1: 30% co-polypropylene, 10% linear low-density polyethylene, 20% radiation cross-linked polyolefin heat shrink material, 20% high-pressure polyethylene, 20% polyvinyl chloride; co-polypropylene accounts for the highest proportion, and the film formation improves the impact resistance and flexibility, while ensuring the heat shrinkage ability, flexibility and toughness of the film formation;

[0082] Material ratio scheme 2: 15% copolymerized polypropylene, 20% linear low-density polyethylene, 25% radiation cross-linked polyolefin heat shrinkable material, 30% high-pressure polyethylene, and 10% polyvinyl chloride; high-pressure polyethylene accounts for the highest proportion, and the film formation ensures electrical insulation and softness, while combined with linear low-density polyethylene and radiation cross-linked polyolefin heat shrinkable material, tensile strength and toughness are taken into account.

[0083] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A high-toughness anti-rust protective film, characterized in that: include: A copolymerized polypropylene layer (1), the lower surface of the copolymerized polypropylene layer (1) being bonded with a linear low-density polyethylene layer (2), the lower surface of the linear low-density polyethylene layer (2) being bonded with a sealing hot-melt adhesive layer (3), the lower surface of the sealing hot-melt adhesive layer (3) being bonded with a high-pressure polyethylene layer (5), and the lower surface of the high-pressure polyethylene layer (5) being bonded with a polyvinyl chloride layer (6); A radiation cross-linked polyolefin heat shrinkable material thread braided layer (4) is arranged inside the sealing hot melt adhesive layer (3), anti-rust oil is arranged on the lower surface of the polyvinyl chloride layer (6), and a polypropylene film is arranged on the lower surface of the polyvinyl chloride layer (6), and the polypropylene film prevents the anti-rust oil from becoming ineffective or contaminating the co-polypropylene layer (1).

2. The high-toughness anti-rust protective film according to claim 1, characterized in that: The copolymerized polypropylene layer (1), the linear low-density polyethylene layer (2), the high-pressure polyethylene layer (5) and the polyvinyl chloride layer (6) are extruded into a film.

3. The high-toughness anti-rust protective film according to claim 1, characterized in that: The radiation cross-linked polyolefin heat shrinkable material thread braided layer (4) is woven from a plurality of radiation cross-linked polyolefin heat shrinkable material warps and wefts, and two adjacent radiation cross-linked polyolefin heat shrinkable material warps or wefts are arranged at equal distances.

4. The high-toughness anti-rust protective film according to claim 1, characterized in that: The sealing hot melt adhesive layer (3) is provided as two layers of upper and lower hot melt adhesive films, and the radiation cross-linked polyolefin heat shrinkable material thread braided layer (4) is provided between the two hot melt adhesive films.

5. A processing technology for high-toughness anti-rust protective film, characterized in that: The following steps are involved: S1: Melting polymer raw materials; melting copolymer polypropylene, linear low-density polyethylene, sealing hot melt adhesive, high-pressure polyethylene, polyvinyl chloride and radiation cross-linked polyolefin heat shrinkable materials respectively; S2: extrusion film forming; extruding co-polypropylene, linear low-density polyethylene, sealing hot melt adhesive, high-pressure polyethylene, and polyvinyl chloride into films respectively, and pre-treating them; extruding radiation cross-linked polyolefin heat shrinkable material and weaving it according to warp and weft arrangement, and compounding it with the sealing hot melt adhesive film; S3: multi-film bonding; bonding a co-polypropylene film, a linear low-density film, a sealing hot-melt adhesive film, a high-pressure polyethylene film and a polyvinyl chloride film to form a composite film; S4: Anti-rust oil spraying: spray anti-rust oil on the surface of the polyvinyl chloride film of the composite film; S5: film coating and rolling; covering the surface of the polyvinyl chloride film with a polypropylene film, and then rolling it up.

6. The processing technology of a high-toughness anti-rust protective film according to claim 5 is characterized in that: The extrusion film forming comprises the following steps: S21: extrusion molding; extruding various raw materials in a molten state into films or extrusion wires as needed; S22: film pretreatment; irradiating a copolypropylene film, a linear low-density film, a high-pressure polyethylene film and a polyvinyl chloride film with Co60 gamma rays, and then biaxially stretching the film at a temperature of 150°C; S23: weaving radiation cross-linked polyolefin heat shrinkable material threads; extruding and drawing the radiation cross-linked polyolefin heat shrinkable material and arranging the threads according to warp and weft to weave into a layer; S24: hot melt lamination; covering the upper and lower surfaces of the radiation cross-linked polyolefin heat shrinkable material wire braided layer with two sealing hot melt adhesive films, and heating the two sealing hot melt adhesive films to fuse them and fix them to the radiation cross-linked polyolefin heat shrinkable material wire braided layer.

7. The processing technology of a high-toughness anti-rust protective film according to claim 5 is characterized in that: The multi-film bonding comprises the following steps: S31: Glue coating on film surface; introducing co-polypropylene film, linear low-density film, sealing hot melt adhesive film, high-pressure polyethylene film and polyvinyl chloride film into a five-layer co-extrusion film blowing machine, and applying adhesive on the film surface; S32: co-extrusion film blowing; extruding the plurality of films mentioned above through a five-layer co-extrusion film blowing machine, and finally forming a composite film; S33: trimming into a roll; trimming the edge of the composite film and rolling it up.

Citation Information

Patent Citations

  • Strippable heat-proof antirust protective film coating and preparation method thereof

    CN102863888A

  • Color film antirust film

    CN209065816U

  • Stretch-proof polyethylene film

    CN216639357U