A low-cost low-alloy ultra-high-strength steel bar and production method thereof

By designing appropriate alloy composition and smelting technology, the problems of high production costs and complex processes of low alloy ultra-high strength steel are solved, and the production of low alloy ultra-high strength steel is achieved efficiently, with high tensile strength, high impact strength and excellent Fracture toughness reduces production costs and improves efficiency.

CN116219262BActive Publication Date: 2024-11-29CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211529428.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-30
Publication Date
2024-11-29
Estimated Expiration
2042-11-30

AI Technical Summary

Technical Problem

The existing low-alloy ultra-high strength steel has high production costs, complex processes and low production efficiency, and the alloy composition design requires expensive metal elements to be considered, which limits its application scenarios.

Method used

By designing suitable alloy composition and smelting technology, low-carbon and low-sulfur content steel is used for smelting, refining, deoxidation, vacuum degassing, continuous casting, annealing and vacuum self-consumption smelting to form low-alloy ultra-high strength steel rods.

Benefits of technology

Low-alloy ultra-high strength steel finished products with high tensile strength, high impact strength and excellent fracture toughness have been achieved, reducing production costs, improving production efficiency, and no additional equipment investment is required.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116219262B_ABST
    Figure CN116219262B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for producing low-cost low-alloy ultra-high-strength steel bars, which comprises the following steps: smelting alloy raw materials to obtain molten steel with low carbon and low sulfur content; refining the molten steel, and performing deoxidation treatment and alloy composition adjustment during the refining process; vacuum degassing the adjusted molten steel; continuously casting the molten steel after vacuum degassing to form bars; annealing and surface grinding the bars; vacuum consumable smelting the polished bars; and heat treating the bars after vacuum consumable smelting to obtain low-alloy ultra-high-strength steel bars. In the above manner, the present invention realizes continuous casting production of low-alloy ultra-high-strength steel products that do not contain high-cost alloy elements, have high tensile strength, high impact strength, and excellent fracture toughness without the need for additional equipment investment, which greatly reduces the production cost of existing low-alloy ultra-high-strength steel and improves production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of iron and steel metallurgy, and in particular to a low-cost low-alloy ultra-high-strength steel bar and a production method thereof. Background Art

[0002] Ultra-high strength steel has excellent mechanical properties, ultra-high strength and excellent toughness, and has always been widely used in national defense and civilian applications. As early as the 1940s, the United States took the lead in developing ultra-high strength steel to replace ordinary steel in order to save military expenses. In addition to high strength and good toughness, ultra-high strength steel also has different special properties according to its different use environments, such as high fatigue resistance and good welding performance. According to different chemical composition and organizational properties, ultra-high strength steel is generally divided into three categories: low-alloy ultra-high strength steel, medium-high alloy secondary hardening ultra-high strength steel and ultra-low carbon martensitic aging ultra-high strength steel. At present, because medium-high alloy secondary hardening ultra-high strength steel contains a large amount of very expensive alloy elements such as cobalt and nickel, although it has excellent mechanical properties and high corrosion resistance, it is expensive and is generally only used in high-end parts such as fighter landing gear. In order to ensure the martensitic strength, a considerable amount of cobalt and nickel are added to ultra-low carbon maraging ultra-high strength steel. As metal elements in serious shortage worldwide, cobalt and nickel have significantly increased the cost of this type of steel, limiting its application scenarios. Low-alloy ultra-high strength steel has excellent strength and toughness matching while taking into account the cost. Existing low-alloy ultra-high strength steel generally adopts special smelting methods. Although the product performance is good, the cost is high, the process is complicated, and the production efficiency is low; and its alloy composition design often requires the participation of high-cost metal elements, or needs to consider different application scenarios, so the application effect is limited.

[0003] Therefore, in view of the many deficiencies in the existing production of low-alloy ultra-high strength steel, it is necessary to provide a method for producing high-performance low-alloy ultra-high strength steel with improved alloy composition and more efficiently and at low cost. Summary of the invention

[0004] The purpose of the present invention is to achieve efficient continuous casting production of low-alloy ultra-high strength steel products with low cost, high tensile strength, high impact strength and excellent fracture toughness by designing appropriate alloy composition and smelting process.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A method for producing low-cost low-alloy ultra-high strength steel bars, the method comprising:

[0007] The alloy raw materials are melted to obtain molten steel with low carbon and low sulfur content;

[0008] Refining the molten steel, and performing deoxidation treatment and alloy composition adjustment during the refining process;

[0009] The molten steel after adjustment is subjected to vacuum degassing treatment;

[0010] Continuously casting the molten steel after vacuum degassing to form rods;

[0011] Performing annealing and surface grinding on the rod;

[0012] The polished bars are subjected to vacuum consumable melting;

[0013] The rods after vacuum consumable melting are heat treated to obtain low alloy ultra-high strength steel rods.

[0014] As a further improvement of the present invention, the composition of the molten steel is adjusted to C: 0.30% ~ 0.35%, Si: 0.90% ~ 1.10%, Mn: 0.30% ~ 0.50%, Ni: 0.70% ~ 1.00%, Cr: 2.80% ~ 3.00%, Nb + Ta ≤ 0.1%, and the remainder is Fe and impurities.

[0015] As a further improvement of the present invention, in the molten steel with low carbon and low sulfur content: P: ≤0.020%, S: ≤0.005%.

[0016] As a further improvement of the present invention, the process of smelting the alloy raw materials to obtain molten steel with low carbon and low sulfur content comprises:

[0017] Oxygen is blown into the molten steel at a temperature of 1580°C or above after melting, and the molten steel is thoroughly mixed.

[0018] As a further improvement of the present invention, the deoxidation treatment comprises:

[0019] The deoxidation treatment conditions of Si-Ca line are controlled to be 90m / furnace-100m / furnace;

[0020] The addition amount of Si-Ca alloy particles is controlled to be 15kg / furnace to 20kg / furnace.

[0021] As a further improvement of the present invention, the slag composition after the deoxidation treatment is controlled to include: 43.5% to 45% CaO, 34.5% to 38.5% Al2O3, 8% to 12% SiO2, 6 to 9% MgO, 3% to 7% CaF2 and 2.4% to 2.7% K2O.

[0022] As a further improvement of the present invention, the alloy composition adjustment includes:

[0023] Niobium-tantalum alloy is added to molten steel at a refining temperature above 1550°C.

[0024] As a further improvement of the present invention, the temperature of the molten steel before vacuum degassing is controlled to be ≥1580°C; and the vacuum degassing treatment time is 45 to 60 minutes.

[0025] As a further improvement of the present invention, the diameter of the rod is 300-350 mm.

[0026] As a further improvement of the present invention, the continuous casting of the molten steel after vacuum degassing to form the rod comprises:

[0027] Set the pouring superheat to 25℃~30℃; the casting machine pulling speed to 2.0~2.5m / min.

[0028] As a further improvement of the present invention, the vacuum consumable melting conditions are set as follows: smelting voltage 78±3V; smelting current 7500~11500A; smelting current fluctuation range does not exceed ±500A; smelting vacuum degree ≤1Pa; filling time ≥35min; furnace cooling time 50~60min; vacuum consumable melting rate 4.9~6kg / min; smelting crystallizer water outlet temperature 40~58 degrees; and slow cooling time ≥48h.

[0029] The present invention also provides a low-cost low-alloy ultra-high strength steel bar, which is prepared by any of the preparation methods described above.

[0030] Technical effects and advantages of the present invention:

[0031] The method for producing low-cost low-alloy ultra-high-strength steel bars of the present invention comprises the following steps: smelting alloy raw materials to obtain molten steel with low carbon and low sulfur content; refining the molten steel, and performing deoxidation treatment and alloy composition adjustment during the refining process; vacuum degassing the adjusted molten steel; continuously casting the molten steel after vacuum degassing to form bars; annealing and surface grinding the bars; vacuum consumable smelting the polished bars; and heat treating the bars after vacuum consumable smelting to obtain low-alloy ultra-high-strength steel bars. In the above manner, the present invention realizes continuous casting production of low-alloy ultra-high-strength steel products that do not contain high-cost alloy elements, have high tensile strength, high impact strength, and excellent fracture toughness without the need for additional equipment investment, greatly reducing the production cost of existing low-alloy ultra-high-strength steel and improving production efficiency.

[0032] Other features and advantages of the present invention will be described in the following description, and partly become obvious from the description, or be understood by implementing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The present invention is a flow chart of the method for producing low-cost low-alloy ultra-high strength steel bars. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] In order to solve the deficiencies of the prior art, the present invention designs appropriate alloy composition and smelting process to produce a low-cost, high tensile strength, high impact strength and excellent fracture toughness low alloy ultra-high strength steel product. The specific content of the invention is as follows:

[0036] The low alloy ultra-high strength steel involved in the present invention is mainly composed of the following chemical components by mass percentage: C: 0.30% to 0.35%, Si: 0.90% to 1.10%, Mn: 0.30% to 0.50%, Ni: 0.70% to 1.00%, Cr: 2.80% to 3.00%, Nb+Ta≤0.1%, and the remainder of Fe and impurities. The appropriate content of carbon element ensures that the steel can form martensite and has sufficient strength. The addition of Si element significantly improves the elastic limit, yield strength and yield strength ratio of the steel, and improves the fatigue strength and fatigue ratio. The addition of Mn element is also to increase the strength and improve the hardenability of the steel. The addition of Ni element can obtain comprehensive mechanical properties with good matching of strength and toughness, and at the same time increase the corrosion resistance of the steel. The addition of Cr element improves the strength and hardness of the steel and improves the wear resistance of the steel. The addition of Nb and Ta elements can significantly refine the grains and improve the yield strength and impact toughness of steel. At the same time, the use of niobium-tantalum alloy is cheaper than traditional niobium-iron alloy because of its high purity and small usage. In addition, since niobium and tantalum generally coexist in niobium-tantalum ore, the cost of separating the elements is low.

[0037] The furnace is smelted by electric furnace, with lime padding at the bottom. High-quality scrap steel, ferroalloy, low-phosphorus and low-sulfur pig iron are added to the furnace and then powered for melting. After melting, the temperature is measured and controlled above 1580℃. Oxygen is blown deep into the furnace at low pressure through a single tube. After sufficient stirring, the components are sampled and analyzed to generate molten steel with low carbon and low sulfur content (P: ≤0.020%, S: ≤0.005%).

[0038] LF furnace refining is adopted, Si-Ca line is used for deoxidation treatment, 90m / furnace-100m / furnace. According to the sampling and analysis results, the chemical composition is adjusted according to the relevant requirements of the chemical composition control of the steel grade, the alloy is adjusted, and the power is sent to increase the temperature. The sampling is fully analyzed and the chemical composition and mass percentage of ultra-high strength steel C: 0.30%~0.35%, Si: 0.90%~1.10%, Mn: 0.30%~0.50%, Ni: 0.70%~1.00%, Cr: 2.80%~3.00%, P: ≤0.010%, S: ≤0.003% of the remaining Fe and impurities are fine-tuned. Add Si-Ca alloy particles for final deoxidation, Si-Ca alloy particles are 15kg / furnace to 20kg / furnace, and control the composition range (mass percentage) of LF smelting end slag to: 43.5% to 45% CaO, 34.5% to 38.5% Al2O3, 8% to 12% SiO2, 6% to 9% MgO, 3% to 7% CaF2, about 2.5% K2O. Temperature measurement, the temperature is controlled above 1550℃, and a trace amount of 5kg / furnace of niobium-tantalum alloy can be added to fine-tune the alloy composition. Temperature measurement, the temperature is controlled above 1580℃ and the package can be hung.

[0039] In the VD stage, argon soft blowing is used to make the inclusions fully float up and be removed. The argon soft blowing time is controlled between 45 minutes and 60 minutes. In the early stage of VD, a large flow of argon is blown and the flow rate is controlled below 180L / min to prevent the molten steel from rolling violently.

[0040] After that, continuous casting is carried out. Since the carbon content is about 0.30% and the rod diameter is between 300-350mm, the tundish pouring overheat ΔT is strictly controlled between 25℃ and 30℃, the casting machine pulling speed is set to 2.0-2.5m / min, and the secondary cooling water ratio is about 2.5L / kg; the secondary cooling water ratio: about 150L / m in the first zone, about 175L / m in the second zone, and about 50L / m in the third zone. After the continuous casting rod product is annealed, its surface is rolled.

[0041] Finally, the consumable electrode rods produced by continuous casting are vacuum consumable to further remove inclusions. The smelting voltage setting value is 78±3V; the smelting current setting value is 7500~11500A; the maximum smelting fluctuation range is ±500A; the smelting vacuum degree is ≤1Pa; the filling time is ≥35min; the furnace cooling time is 50~60min; the vacuum consumable melting rate is 4.9~6kg / min; the bottom is Bengang or similar steel grades; the smelting crystallizer outlet water temperature is 40~58 degrees; slow cooling: ≥48h.

[0042] The bars are forged and heat treated according to customer needs to obtain ultra-high strength steel with a microstructure dominated by martensite, a tensile strength ≥1350MPa, and a fracture toughness KIC ≥65MPa·m 1 / 2, Charpy impact energy ≥55J.

[0043] The production method of low-cost low-alloy ultra-high-strength steel bars provided by the present invention is described below with reference to specific embodiments 1 to 3:

[0044] Example 1

[0045] The low alloy ultra-high strength steel involved in the present invention is mainly composed of the following chemical components by mass percentage: C: 0.33%, Si: 0.95%, Mn: 0.36%, Ni: 0.79%, Cr: 2.89%, Nb+Ta=0.09%, and the remainder Fe and impurities.

[0046] The furnace is smelted in an electric furnace, with lime at the bottom. High-quality scrap steel, ferroalloys, low-phosphorus and low-sulfur pig iron are added to the furnace and then powered for melting. After melting, the temperature is measured and controlled at 1600°C. Oxygen is blown deep into the furnace at low pressure. After sufficient stirring, samples are taken for component analysis to generate molten steel with low carbon and low sulfur content (P: = 0.018%, S: = 0.004%).

[0047] LF furnace refining is adopted, and Si-Ca wire is used for deoxidation treatment, 93m / furnace. According to the sampling and analysis results, the chemical composition is adjusted according to the relevant requirements of the chemical composition control of the steel grade, the alloy is adjusted, and the power is sent to increase the temperature. The sampling is fully analyzed and the alloy composition is fine-tuned according to the chemical composition and mass percentage of ultra-high strength steel C: 0.32%, Si: 0.99%, Mn: 0.38%, Ni: 0.90%, Cr: 2.98%, P: = 0.009%, S: = 0.002%, the remaining Fe and impurities. Si-Ca alloy particles are added for final deoxidation, Si-Ca alloy particles are 19kg / furnace, and the LF smelting end slag composition control range (mass percentage) is: 44.5% CaO, 36.5% Al2O3, 11.4% SiO2, 7.9% MgO, 3.8% CaF2, about 2.7% K2O. Temperature measurement, temperature control at 1592℃, add a small amount of niobium tantalum alloy of about 5.7kg / furnace to make the final fine adjustment of the alloy composition. Temperature measurement, temperature control above 1610℃, then the package can be hung.

[0048] In the VD (Vacuum Degassing) stage, argon soft blowing is used to make the inclusions fully float up and be removed. The argon soft blowing time is controlled at 58 minutes. At the initial stage of VD, a large flow rate of argon is blown, and the flow rate is controlled at 181L / min.

[0049] After that, continuous casting is carried out. Since the carbon content is about 0.32% and the rod diameter is between 330mm, the tundish pouring superheat ΔT is strictly controlled between 25℃, the casting machine pulling speed is set to 2.4m / min, the secondary cooling water ratio is 2.6L / kg; the secondary cooling water ratio: 151L / m in zone one, 173L / m in zone two, and 51L / m in zone three. After the finished continuous casting rod is annealed, its surface is rolled.

[0050] Finally, the consumable electrode rod produced by continuous casting is subjected to vacuum consumable to further remove inclusions. The smelting voltage setting value is 78V; the smelting current setting value is 10750A; the maximum smelting fluctuation range is ±465A; the smelting vacuum degree = 0.87Pa; the filling time = 45min; the furnace cooling time is 55min; the vacuum consumable melting rate is 5.3±0.4kg / min; the bottom: Bengang or similar steel grades; the smelting crystallizer outlet water temperature: 49 degrees; slow cooling: 53h.

[0051] The bars are forged and heat treated according to customer needs to obtain ultra-high strength steel with a microstructure dominated by martensite, a tensile strength of 1602MPa, and a fracture toughness KIC of 69MPa·m 1 / 2 , the Charpy impact energy is equal to 68J.

[0052] Example 2

[0053] The low alloy ultra-high strength steel involved in the present invention is mainly composed of the following chemical components by mass percentage: C: 0.31%, Si: 1.05%, Mn: 0.46%, Ni: 0.92%, Cr: 2.95%, Nb+Ta=0.089%, and the remainder Fe and impurities.

[0054] The furnace is smelted in an electric furnace, with lime at the bottom. High-quality scrap steel, ferroalloys, low-phosphorus and low-sulfur pig iron are added to the furnace and then powered for melting. After melting, the temperature is measured and controlled at 1593°C. Oxygen is blown deep into the furnace at low pressure through a single tube. After sufficient stirring, samples are taken for component analysis to generate molten steel with low carbon and low sulfur content (P: = 0.016%, S: = 0.0041%).

[0055] LF furnace refining is adopted, and Si-Ca wire is used for deoxidation treatment, 98m / furnace. According to the sampling and analysis results, the chemical composition is adjusted according to the relevant requirements of the chemical composition control of the steel grade, the alloy is adjusted, and the power is sent to heat up. The sampling is fully analyzed and the alloy composition is fine-tuned according to the chemical composition and mass percentage of ultra-high strength steel C: 0.33%, Si: 1.04%, Mn: 0.46%, Ni: 0.92%, Cr: 2.95%, P: = 0.0012%, S: = 0.0032%, and the remaining Fe and impurities. Si-Ca alloy particles are added for final deoxidation, and the Si-Ca alloy particles are 16kg / furnace. The control range (mass percentage) of the slag composition at the end of LF smelting is: 43.9% CaO, 38.4% Al2O3, 11.2% SiO2, 8.5% MgO, 6.8% CaF2, and about 2.7% K2O. Temperature measurement, temperature control at 1590℃, add a small amount of 4.8kg / furnace of niobium-tantalum alloy to make the final fine-tuning of the alloy composition. Temperature measurement, temperature control above 1605℃, then the package can be hung.

[0056] In the VD stage, argon soft blowing is used to make the inclusions fully float up and be removed. The argon soft blowing time is controlled at 58 minutes. In the early stage of VD, a large flow of argon is blown, and the flow rate is controlled at 155L / min.

[0057] After that, continuous casting is carried out. Since the carbon content is about 0.32% and the rod diameter is between 320mm, the tundish pouring superheat ΔT is strictly controlled between 27℃, the casting machine pulling speed is set to 2.5m / min, the secondary cooling water ratio is 2.5L / kg; the secondary cooling water ratio: 148L / m in the first zone, 177L / m in the second zone, and 52L / m in the third zone. After the continuous casting rod product is annealed, its surface is rolled.

[0058] Finally, the consumable electrode rod produced by continuous casting is subjected to vacuum consumable to further remove inclusions. The smelting voltage setting value is 79V; the smelting current setting value is 10800A; the maximum smelting fluctuation range is ±470A; the smelting vacuum degree = 0.9Pa; the filling time = 40min; the furnace cooling time is 52min; the vacuum consumable melting rate is 5.4±0.3kg / min; the bottom: Bengang or similar steel grades; the smelting crystallizer outlet water temperature: 47 degrees; slow cooling: 50h.

[0059] The bars are forged and heat treated according to customer needs to obtain ultra-high strength steel with a microstructure dominated by martensite, a tensile strength of 1570MPa, and a fracture toughness KIC of 77MPa·m 1 / 2 , the Charpy impact energy is equal to 61J.

[0060] Example 3

[0061] The low alloy ultra-high strength steel involved in the present invention is mainly composed of the following chemical components by mass percentage: C: 0.35%, Si: 1.05%, Mn: 0.50%, Ni: 0.99%, Cr: 2.96%, Nb+Ta=0.09%, and the remainder Fe and impurities.

[0062] The furnace is smelted in an electric furnace, with lime at the bottom. High-quality scrap steel, ferroalloys, low-phosphorus and low-sulfur pig iron are added to the furnace and then powered for melting. After melting, the temperature is measured and controlled at 1610°C. Oxygen is blown deep into the furnace at low pressure through a single tube. After sufficient stirring, the components are sampled and analyzed to generate molten steel with low carbon and low sulfur content (P: = 0.016%, S: = 0.003%).

[0063] LF furnace refining is adopted, and Si-Ca wire is used for deoxidation treatment, 92m / furnace. According to the sampling and analysis results, the chemical composition is adjusted according to the relevant requirements of the chemical composition control of the steel grade, the alloy is adjusted, and the power is sent to heat up. The sampling is fully analyzed and the alloy composition is fine-tuned according to the chemical composition of ultra-high strength steel and its mass percentage C: 0.35%, Si: 1.07%, Mn: 0.48%, Ni: 0.97%, Cr: 2.93%, P: = 0.008%, S: = 0.0016% of the remaining Fe and impurities. Si-Ca alloy particles are added for final deoxidation, and the Si-Ca alloy particles are 20kg / furnace. The control range (mass percentage) of the slag composition at the end of LF smelting is: 44.8% CaO, 35.3% Al2O3, 11.2% SiO2, 8.9% MgO, 6.2% CaF2, and about 2.4% K2O. Temperature measurement, temperature control at 1564℃, add a small amount of niobium tantalum alloy of about 5.8kg / furnace to make the final fine adjustment of the alloy composition. Temperature measurement, temperature control above 1583℃, then the package can be hung.

[0064] In the VD stage, argon soft blowing is used to make the inclusions fully float up and be removed. The argon soft blowing time is controlled at 60 minutes. In the early stage of VD, a large flow of argon is blown, and the flow rate is controlled at 169L / min.

[0065] After that, continuous casting is carried out. Since the carbon content is about 0.32% and the rod diameter is between 340mm, the tundish pouring superheat ΔT is strictly controlled between 28℃, the casting machine pulling speed is set to 2.3m / min, the secondary cooling water ratio is 2.4L / kg; the secondary cooling water ratio: 152L / m in the first zone, 178L / m in the second zone, and 48L / m in the third zone. After the continuous casting rod product is annealed, its surface is rolled.

[0066] Finally, the consumable electrode rod produced by continuous casting is subjected to vacuum consumable to further remove inclusions. The smelting voltage setting value is 81V; the smelting current setting value is 10650A; the maximum smelting fluctuation range is ±430A; the smelting vacuum degree = 0.75Pa; the filling time = 46min; the furnace cooling time is 58min; the vacuum consumable melting rate is 5.3±0.4kg / min; the bottom: Bengang or similar steel grades; the smelting crystallizer outlet water temperature: 57 degrees; slow cooling: 53h.

[0067] The bars are forged and heat treated according to customer needs to obtain ultra-high strength steel with a microstructure dominated by martensite, a tensile strength of 1558MPa, and a fracture toughness KIC of 75MPa·m 1 / 2 , the Charpy impact energy is equal to 64J.

[0068] In summary, the method for producing low-cost low-alloy ultra-high-strength steel bars of the present invention obtains molten steel with low carbon and low sulfur content by smelting alloy raw materials; refining the molten steel, and performing deoxidation treatment and alloy composition adjustment during the refining process; vacuum degassing the adjusted molten steel; continuously casting the molten steel after vacuum degassing to form bars; annealing and surface grinding the bars; vacuum consumable smelting the polished bars; heat treating the bars after vacuum consumable smelting to obtain low-alloy ultra-high-strength steel bars. In the above manner, the present invention realizes continuous casting production of low-alloy ultra-high-strength steel products that do not contain high-cost alloy elements, have high tensile strength, high impact strength and excellent fracture toughness without the need for additional equipment investment, greatly reducing the production cost of existing low-alloy ultra-high-strength steel and improving production efficiency.

[0069] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for producing low-cost low-alloy ultra-high strength steel bars, characterized in that: The method comprises: The alloy raw materials are melted to obtain molten steel with low carbon and low sulfur content; Refining the molten steel, and performing deoxidation treatment and alloy composition adjustment during the refining process; The molten steel after adjustment is subjected to vacuum degassing treatment; Continuously casting the molten steel after vacuum degassing to form rods; Performing annealing and surface grinding on the rod; The polished bars are subjected to vacuum consumable melting; The rods after vacuum consumable smelting are heat treated to obtain low alloy ultra-high strength steel rods; The composition of the molten steel is adjusted to be C: 0.30% to 0.35%, Si: 0.90% to 1.10%, Mn: 0.30% to 0.50%, Ni: 0.70% to 1.00%, Cr: 2.80% to 3.00%, Nb+Ta≤0.1%, and the remainder is Fe and impurities; In the molten steel with low carbon and low sulfur content: P: ≤0.020%, S: ≤0.005%; The deoxidation treatment comprises: The deoxidation treatment conditions of Si-Ca line are controlled to be 90m / furnace-100m / furnace; The amount of Si-Ca alloy particles added is controlled to be 15kg / furnace to 20kg / furnace; The slag composition after the deoxidation treatment is controlled to include: 43.5% to 45% CaO, 34.5% to 38.5% Al2O3, 8% to 12% SiO2, 6% to 9% MgO, 3% to 7% CaF2 and 2.4% to 2.7% K2O; The continuous casting of the molten steel after vacuum degassing to form a bar comprises: Set the pouring superheat to 25℃~30℃; the casting speed to 2.0~2.5m / min; The vacuum consumable melting conditions are set as follows: smelting voltage 78±3V; smelting current 7500~11500A; smelting current fluctuation range does not exceed ±500A; smelting vacuum degree ≤1Pa; filling time ≥35min; furnace cooling time 50~60min; vacuum consumable melting rate 4.9~6kg / min; smelting crystallizer water outlet temperature 40~58 degrees; and slow cooling time ≥48h.

2. The method for producing low-cost low-alloy ultra-high strength steel bars according to claim 1, characterized in that: The method of smelting the alloy raw materials to obtain molten steel with low carbon and low sulfur content comprises: Oxygen is blown into the molten steel at a temperature above 1580°C and the molten steel is thoroughly mixed.

3. The method for producing low-cost low-alloy ultra-high strength steel bars according to claim 1, characterized in that: The alloy composition adjustment includes: Niobium-tantalum alloy is added to molten steel at a refining temperature above 1550°C.

4. The method for producing low-cost low-alloy ultra-high strength steel bars according to claim 1, characterized in that: Control the temperature of molten steel before vacuum degassing to be ≥1580℃; the vacuum degassing treatment time is 45~60min.

5. The method for producing low-cost low-alloy ultra-high strength steel bars according to claim 1, characterized in that: The diameter of the rod is 300-350 mm.

6. A low-cost, low-alloy, ultra-high-strength steel bar, characterized in that: The low-cost low-alloy ultra-high-strength steel bar is produced by the production method described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Ultrahigh-strength low-alloy steel and manufacturing method thereof

    CN104726782A