A low-cost carbon fiber reinforced metal-ceramic matrix composite material for aerospace thermal protection system and a preparation method thereof

By infiltrating Cu metal alloy powder into carbon fiber reinforced carbon aerogel preforms, the preparation process was simplified and a uniform distribution of metal and ceramic matrices was achieved, solving the problem of insufficient ablation resistance of composite materials and improving the thermal protection performance of the materials.

CN116219329BActive Publication Date: 2024-11-19INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310008951.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-04
Publication Date
2024-11-19
Estimated Expiration
2043-01-04

AI Technical Summary

Technical Problem

The existing carbon fiber reinforced metal-ceramic matrix composites have complex preparation processes and uneven distribution of ceramic and metal matrices, resulting in insufficient ablation resistance.

Method used

A one-step reactive melting method was used to melt-infiltrate Cu-containing alloy powder into carbon fiber reinforced carbon aerogel preforms with a three-dimensional interconnected nanoporous structure, simplifying the preparation process and achieving uniform distribution of the metal matrix and ceramic matrix.

Benefits of technology

It significantly reduced the material surface temperature and ablation rate, improved the material's ablation resistance, and achieved a perfect combination of active and passive cooling thermal protection mechanisms.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004037094590000011
    Figure HDA0004037094590000011
  • Figure HDA0004037094590000012
    Figure HDA0004037094590000012
  • Figure HDA0004037094590000021
    Figure HDA0004037094590000021
Patent Text Reader

Abstract

The present invention discloses a low-cost carbon fiber reinforced metal-ceramic matrix composite material for aerospace thermal protection system and a preparation method thereof, belonging to the technical field of composite material preparation. The method comprises: 1) preparation of a preform; 2) pretreatment of the preform; 3) powder spreading; 4) infiltration. The present invention simultaneously introduces a metal-ceramic matrix into the preform by a one-step reaction infiltration method, and obtains a composite material with a uniformly dispersed two-phase matrix; during the ablation process, the metal and the ceramic matrix respectively reduce the ablation temperature of the material surface through phase change heat absorption and radiation heat dissipation mechanisms, realizing an effective combination of active cooling and passive cooling thermal protection mechanisms, giving the carbon fiber reinforced metal-ceramic matrix composite material excellent ablation resistance, greatly improving the use temperature limit of the carbon fiber reinforced ceramic matrix composite material, and is expected to be used as a new type of high-temperature thermal protection material in aerospace thermal protection systems.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite material preparation, and in particular to a low-cost carbon fiber reinforced metal-ceramic matrix composite material for aerospace thermal protection system and a preparation method thereof. Background Art

[0002] When high-speed aircraft engines are working, the combustion of propellants produces high-temperature gas flow, with a temperature of more than 3000℃. The injector panel, combustion thrust chamber inner wall, throat lining, nozzle and other parts of the engine are subjected to the scouring and erosion of the high-temperature gas flow, which puts higher requirements on the thermal protection materials of aircraft. Radiation heat protection (passive cooling) refers to the fact that most of the heat conducted to the material under the action of high-temperature and high-speed airflow is dissipated through convection and re-radiation, accompanied by a series of physical and chemical changes such as material oxidation, evaporation and mechanical erosion. Carbon fiber reinforced silicon carbide composite material (C / SiC) is a typical radiation-type thermal protection material with the advantages of low density, low thermal expansion coefficient, high strength and excellent thermal shock resistance. It is widely used in key thermal protection structures such as aircraft nose cones and wing leading edges, engine combustion chamber linings and nozzles. However, in an oxygen environment above 1650℃, the SiC matrix of C / SiC changes from passive oxidation to active oxidation. In addition, the thermal stability of the SiO2 oxide film under this condition decreases sharply, and the material suffers serious ablation damage. Sweating heat protection (active cooling) is another heat protection method, which means that when the material is in high-temperature service, it sweats to reduce the temperature of the material itself to achieve heat protection. For example, in the ablation environment, the copper in the tungsten-copper composite material evaporates and absorbs a lot of heat, thereby providing a good cooling effect for the tungsten skeleton, making the use temperature of the tungsten-copper composite material as high as 2700℃. However, the material has a high density (16-18g / cm 3 ), long preparation cycle, high cost, and limited application in thermal protection systems. It can be seen that a single radiation-type or sweat-type thermal protection material system still has deficiencies in terms of high-temperature physical and chemical stability, energy dissipation efficiency, and effective service temperature. It is necessary to explore ways to improve the service capabilities of materials in extreme environments, develop new thermal protection material systems, and provide material reserves and technical support for the new generation of aerospace thermal protection systems.

[0003] The effective combination of active cooling and passive cooling thermal protection mechanisms can give the material more excellent ablation resistance and further improve the service ability of the material in extreme environments. For example, Wang QK et al. mixed Cu powder with polycarbosilane solution and prepared C / SiC-Cu composite materials by precursor impregnation pyrolysis method. After ablation in oxyacetylene flame at 3000℃ for 35s, the mass ablation rate of the material was 0.012g / s and the line ablation rate was 7μm / s, which was only 1 / 7 of the line ablation rate of C / SiC composite materials under the same ablation conditions (Wang QK, Hu HF, Chen ZH, Preparation of 3D C / SiC-Cu composites via precursor pyrolysis and property investigation, Key Engineering Materials, 2008, 368–372: 1031–1033.). Wang P et al. first used chemical deposition technology to prepare porous C / C-SiC composites, and then melt-infiltrated Cu-Sn alloy to prepare C / SiC-Cu composites. During oxyacetylene ablation (the center temperature of the sample surface was 2500℃ / 30s), a continuous and dense SiO2 ablation-resistant layer was formed on the surface of the sample. Combined with the evaporative cooling effect of the copper alloy, the mass ablation rate was 4.23 mg / s and the line ablation rate was 6 μm / s, showing excellent ablation resistance. However, the characteristics of the preparation process itself determine that the distribution of SiC and Cu-Sn alloy in the composite material is uneven (Wang P, Guo Y, Du S, et al, Microstructure, mechanical and ablation properties of transpiration cooling applied to C / C-SiC composite for novel anti-ablation material, Applied Composite Materials, 2022, 29: 2147–2163.). Weng YQ et al. prepared C / SiC-ZrC-Cu composites by combining chemical vapor deposition, precursor impregnation cracking and melt infiltration technology. After ablation in an oxyacetylene flame at a temperature of 2500°C for 20 seconds, the mass ablation rate of the material was 3.4 mg / s and the line ablation rate was 3.5 μm / s; after ablation in an oxyacetylene flame at a temperature of 3000°C for 20 seconds, the mass ablation rate was 21 mg / s and the line ablation rate was 7.3 μm / s. In addition, the composite material prepared by this process has a low density (2.11 g / cm 3), the metal phase is mainly concentrated in the large-sized pores around the fiber, and the ceramic phase is mainly distributed between the fiber and the metal phase (Weng YQ, Yang X, Chen FX, et al, Effect of CVI SiC content on ablation and mechanism of C / C-SiC-ZrC-Cu composites, Ceramics International, 2022, 48: 7937–7950.). Yin Jian et al. used chemical vapor infiltration to obtain a C / C-SiC porous composite material, and then prepared a C / C-SiC-Cu composite material by pressure infiltration. However, its porosity reached 20% to 35%, and its ablation resistance was not ideal (Yin Jian, Xiong Xiang, Zhang Hongbo et al., A C / C-SiC-Cu composite material and its preparation method and application, CN 110983208 B, 2021.08.31.). Long Xianhai et al. combined the vapor-deposited silicon carbide on the surface of the carbon substrate with the copper-zirconium alloy infiltration technology to form a spontaneous infiltration system that does not require a high-pressure environment, and prepared a C / C-SiC-Cu composite material (open porosity of 3%-8%), in which the outer layer of the carbon fiber preform is wrapped by the matrix carbon, the outer layer of the matrix carbon is the matrix silicon carbide layer, the outer layer of the matrix silicon carbide is a mixture layer of zirconium carbide and zirconium silicon compounds, and the outer layer of the mixture of zirconium carbide and zirconium silicon compounds is a copper-zirconium alloy. In other words, the metal phase and ceramic phase in the matrix of the composite material are not evenly distributed, which to a certain extent affects the active / passive cooling synergistic thermal protection effect. After 60s of ablation in an oxyacetylene flame, the linear ablation rate of the material is 0.4μm / s (Long Xianhai, Zhou Feng, He Jiaqi, et al., A C / C-SiC-Cu composite material and its preparation method, CN112573937A, 2021.03.30.). It can be seen that the existing publicly reported carbon fiber reinforced metal-ceramic matrix composites (such as C / SiC-Cu) benefit from the two thermal protection mechanisms of active cooling and passive cooling, and show better ablation resistance than carbon fiber reinforced ceramic matrix composites (such as C / SiC). However, due to the complexity of the preparation process and its own characteristics, the metal matrix and the ceramic matrix are unevenly distributed, and the advantages of the combination of active and passive cooling thermal protection mechanisms cannot be fully utilized. The ablation resistance of the composite material still has room for improvement. Therefore, simplifying the preparation process of the composite material, obtaining a high-density composite material and ensuring the uniform dispersion of the metal matrix and the ceramic matrix is ​​the key to achieving a perfect and effective combination of active and passive cooling thermal protection mechanisms and further improving the ablation resistance of carbon fiber reinforced metal-ceramic matrix composites. Summary of the invention

[0004] The purpose of the present invention is to provide a low-cost carbon fiber reinforced metal-ceramic matrix composite material for aerospace thermal protection system and a preparation method thereof, that is, to infiltrate an alloy powder containing Cu metal into a carbon fiber reinforced carbon aerogel preform with a three-dimensional interconnected nanoporous structure through a one-step reaction infiltration method, so as to solve the problems of complex composite material preparation process, uneven distribution of ceramic matrix and metal matrix, and high ablation rate.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] A method for preparing a low-cost carbon fiber reinforced metal-ceramic matrix composite material for an aerospace thermal protection system, the method comprising the following steps:

[0007] (1) Preform preparation: The carbon fiber preform with the interface layer is placed in a precursor solution for high pressure impregnation, followed by curing and carbonization treatment;

[0008] (2) Repeat step (1) of impregnation-curing-carbonization process multiple times to obtain a density of 0.8-1.5 g / cm 3 Carbon fiber reinforced carbon aerogel preform;

[0009] (3) Preform polishing: The carbon fiber reinforced carbon aerogel preform obtained in step (1) is polished with 200# and 800# silicon carbide sandpapers to remove the surface crust of the preform;

[0010] (4) Ultrasonic cleaning: The carbon fiber reinforced carbon aerogel preform polished in step (2) is placed in anhydrous ethanol for ultrasonic cleaning for 10 minutes;

[0011] (5) Drying: The carbon fiber reinforced carbon aerogel preform after cleaning in step (3) is placed in a 120° C. oven for 5 h for drying;

[0012] (6) Powder spreading: Weigh a certain mass of alloy powder and evenly spread it on the surface of the carbon fiber reinforced carbon aerogel preform after the drying treatment in step (4);

[0013] (7) Infiltration: placing the carbon fiber reinforced carbon aerogel preform with powder on the surface in step (6) in a vacuum environment for high-temperature heat treatment to obtain the carbon fiber reinforced metal-ceramic matrix composite material.

[0014] In the above step (1), the interface layer is one or a combination of two of pyrolytic carbon, silicon carbide and boron nitride.

[0015] In the above step (1), the precursor solution is prepared by mixing a phenolic resin, a pore-forming agent and a curing agent in a weight ratio of (5-15):(8-20):(1-5); wherein the pore-forming agent is one or more of ethanol, ethylene glycol and propylene glycol, and the curing agent is one or more of benzenesulfonyl chloride, hexamethylenetetramine and hydroxymethyl urea.

[0016] In the above step (1), the pressure of the high-pressure impregnation is 2-8 MPa, and the time is 0.5-5 h; the curing treatment temperature is 100-250° C., and the curing time is 10-20 h; the carbonization treatment temperature is 600-1200° C., and the carbonization time is 0.5-5 h.

[0017] In the above step (1), the carbon fiber reinforced carbon aerogel preform is composed of carbon fiber, an interface layer and a carbon aerogel matrix with a three-dimensional interconnected nanopore structure, and the weight ratio of the carbon fiber, the interface layer and the carbon aerogel matrix with a three-dimensional interconnected nanopore structure is (1-5):(1-4):(1-8).

[0018] In the above step (6), the powder spreading process is to mix the alloy powder with an appropriate amount of alcohol to a paste, and evenly spread the powder on the surface of the carbon fiber reinforced carbon aerogel preform.

[0019] The average particle size of the alloy powder is 1-500 μm.

[0020] The alloy powder contains the Cu element and also contains one or more of the refractory metal elements Si, Zr, Hf, Ta, Ti, Nb, V and Mo.

[0021] The weight content of Cu element in the alloy powder is preferably 10-50wt.%.

[0022] In the above step (6), the alloy powder is composed of single-element Cu powder and refractory metal powder; or, the alloy powder is composed of binary Cu-based alloy powder and refractory metal powder; the alloy powder is ternary or multi-element Cu-based alloy powder; the refractory metal powder is one or more of single-element Si powder, single-element Zr powder, single-element Hf powder, single-element Ta powder, single-element Ti powder, single-element Nb powder, single-element V powder and single-element Mo powder.

[0023] In the above step (6), the temperature of the high temperature heat treatment is 1000-2200°C, and the insulation time is 0.5-4h.

[0024] The effective effects and advantages of the present invention are as follows:

[0025] 1. The carbon fiber reinforced carbon aerogel preform of the present invention is composed of carbon fiber, an interface layer and a carbon aerogel matrix, wherein the carbon aerogel has three-dimensionally interconnected nano-mesh pores and a nano-sized carbon skeleton, which is conducive to the alloy infiltrated into the matrix to react with the carbon matrix to the greatest extent, fully realizing the ceramic transformation, thereby forming a dense matrix, and at the same time, it is conducive to the maximum extent of uniform dispersion distribution of the metal matrix and the ceramic matrix, thereby ensuring the effective play of the synergistic effect of the active and passive cooling thermal protection mechanisms to the greatest extent, and giving the composite material excellent ablation resistance.

[0026] 2. Compared with carbon fiber reinforced ceramic matrix composites, the surface temperature of carbon fiber reinforced metal-ceramic matrix composites under the same ablation conditions is significantly reduced (down 200-850℃), and the ablation rate is significantly reduced (close to zero ablation). BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the bending stress-displacement curve of the C / SiC-Cu composite material in Example 1.

[0028] Figure 2 This is the SEM microstructure morphology of the C / SiC-Cu composite material in Example 1.

[0029] Figure 3 This is the SEM microstructure morphology of the C / SiC-Cu composite material in Example 2.

[0030] Figure 4 This is the SEM microstructure morphology of the C / SiC-Cu composite material in Example 3.

[0031] Figure 5 is the surface temperature of the C / SiC-Cu composite material and the C / SiC composite material in Example 3 under the same ablation conditions.

[0032] Figure 6 The microstructure and element distribution of the C / SiC-ZrC-Cu composite material in Example 4; wherein: (a) SEM microstructure morphology; (b) element distribution. DETAILED DESCRIPTION

[0033] In order to further understand the present invention, the present invention is described below in conjunction with examples, but the examples are only for further elaboration of the features and advantages of the present invention, rather than for limitation of the claims of the present invention.

[0034] In the following implementation cases, carbon fiber reinforced metal-ceramic matrix composites are prepared by infiltrating silicon-copper alloy powder, copper powder + silicon powder, silicon-copper alloy powder + silicon powder, silicon-copper alloy powder + silicon-zirconium alloy powder, silicon-zirconium-copper alloy powder or silicon-zirconium-hafnium-copper alloy powder in a carbon fiber reinforced carbon aerogel preform in one step.

[0035] The method of the present invention specifically comprises the following steps:

[0036] (1) Preform preparation: The carbon fiber preform with the interface layer is placed in the precursor solution for high pressure impregnation, followed by curing and carbonization. The density of 0.8-1.5 g / cm is obtained by repeating the impregnation-curing-carbonization process. 3 Carbon fiber reinforced carbon aerogel preform;

[0037] (2) Preform polishing: The carbon fiber reinforced carbon aerogel preform obtained in step (1) is polished with 200# and 800# silicon carbide sandpapers in turn;

[0038] (3) Ultrasonic cleaning: The carbon fiber reinforced carbon aerogel preform obtained in step (2) is placed in anhydrous ethanol and ultrasonically cleaned for 10 min;

[0039] (4) Drying: placing the carbon fiber reinforced carbon aerogel preform obtained in step (3) in an oven at 120° C. for 5 h for drying;

[0040] (5) Powder spreading: Weigh a certain mass of alloy powder and evenly spread it on the surface of the carbon fiber reinforced carbon aerogel preform obtained in step (4);

[0041] (6) Infiltration: The surface-powdered carbon fiber-reinforced carbon aerogel preform obtained in step (5) is placed in a vacuum environment for high-temperature heat treatment to obtain the carbon fiber-reinforced metal-ceramic matrix composite material.

[0042] Preferably, in step (1), the interface layer is pyrolytic carbon, silicon carbide, boron nitride or a combination of two thereof.

[0043] Preferably, in step (1), the precursor solution is composed of phenolic resin, pore-forming agent and curing agent in a weight ratio of (5-15):(8-20):(1-5); wherein the pore-forming agent is one or more of ethanol, ethylene glycol and propylene glycol, and the curing agent is one or more of benzenesulfonyl chloride, hexamethylenetetramine and hydroxymethyl urea.

[0044] Preferably, in step (1), the pressure of the high-pressure impregnation is 2-8 MPa, and the time is 0.5-5 h; the curing temperature is 100-250° C., and the curing time is 10-20 h; the carbonization temperature is 600-1200° C., and the carbonization time is 0.5-5 h.

[0045] Preferably, in step (1), the carbon fiber reinforced carbon aerogel preform is composed of carbon fibers, an interface layer and a carbon aerogel matrix having a three-dimensional interconnected nanoporous structure, and the weight ratio thereof is (1-5):(1-4):(1-8).

[0046] Preferably, in step (2), the grinding is to remove the surface crust of the preform.

[0047] Preferably, in step (5), the powder spreading is to mix the alloy powder with an appropriate amount of alcohol to a paste, and evenly spread it on the surface of the carbon fiber reinforced carbon aerogel preform.

[0048] Preferably, in step (5), the average particle size of the alloy powder is 1-500 μm.

[0049] Preferably, in step (5), the alloy powder contains Cu element and one or more refractory metal elements of Si, Zr, Hf, Ta, Ti, Nb, V, and Mo.

[0050] Preferably, in step (5), the weight ratio of Cu element in the alloy powder is 10-50.

[0051] Preferably, in step (5), the alloy powder is composed of one or more powders of elemental Cu powder and refractory metal powders such as elemental Si powder, elemental Zr powder, elemental Hf powder, elemental Ta powder, elemental Ti powder, elemental Nb powder, elemental V powder, and elemental Mo powder; or is composed of a binary Cu-based alloy and one or more powders of refractory metal powders such as elemental Si powder, elemental Zr powder, elemental Hf powder, elemental Ta powder, elemental Ti powder, elemental Nb powder, elemental V powder, and elemental Mo powder; or is a ternary or multinary Cu-based alloy powder.

[0052] Preferably, in step (6), the temperature of the high temperature heat treatment is 1000-2200°C, and the holding time is 0.5-4h.

[0053] Embodiment 1:

[0054] In this embodiment, silicon-copper alloy powder is infiltrated into a carbon fiber reinforced carbon aerogel preform, and the specific process steps are as follows:

[0055] 1) A precursor solution was prepared with ethylene glycol and hexamethylenetetramine as pore former and curing agent, respectively, wherein the weight ratio of phenolic resin: pore former: curing agent was 6:10:3, and a carbon fiber preform with a pyrolytic carbon interface layer was placed in the precursor solution for 7 h under 5 MPa conditions, then cured at 150 ° C for 15 h, and finally carbonized at 800 ° C for 2 h. By repeating the impregnation-curing-carbonization process, a carbon fiber preform with a density of 1.20 g / cm 3 A carbon fiber reinforced carbon aerogel preform, wherein the weight ratio of the carbon fiber, the interface layer and the carbon aerogel matrix is ​​2:1:2;

[0056] 2) The preform is polished with 200# and 800# silicon carbide sandpaper to remove the surface crust;

[0057] 3) Place the treated preform in anhydrous ethanol and ultrasonically clean it for 10 minutes;

[0058] 4) placing the preform in an oven at 120°C for 5 hours for drying;

[0059] 5) Mix silicon-copper alloy powder with a particle size of 200 μm and a weight ratio of Cu element of 20% with an appropriate amount of alcohol to a paste, and evenly spread it on the surface of the carbon fiber reinforced carbon aerogel preform;

[0060] 6) The carbon fiber reinforced carbon aerogel preform with powder on the surface is placed in a vacuum environment and heat treated at 1350° C. for 1 h to obtain a C / SiC-Cu composite material.

[0061] The density of the C / SiC-Cu composite material prepared in this example is 2.86 g / cm 3 , its bending mechanics-displacement curve is as follows Figure 1 As shown in Figure 1, after the bending stress reaches the maximum value (~160MPa), it slowly decreases, and the composite material exhibits pseudoplastic fracture. The SEM microstructure morphology of the composite material is shown in Figure 1. Figure 2 As shown in the figure, due to the protective effect of the pyrolytic carbon interface layer, the carbon fibers are intact; the ceramic matrix and the metal matrix around the fibers are well dispersed. Under oxyacetylene flame ablation, when the surface temperature of the C / SiC composite material is 1900°C, the surface temperature of the C / SiC-Cu composite material prepared in this embodiment is 1750°C (150°C lower than the surface temperature of the C / SiC composite material), and the mass ablation rate after ablation for 600s is 0.064mg / cm 2 / s, and the linear ablation rate is -0.157μm / s.

[0062] Embodiment 2:

[0063] In this embodiment, a mixture of copper powder and silicon powder is infiltrated into a carbon fiber reinforced carbon aerogel preform, and the specific process steps are as follows:

[0064] 1) A precursor solution was prepared with ethanol and hexamethylenetetramine as pore former and curing agent, respectively, wherein the weight ratio of phenolic resin: pore former: curing agent was 5:9:3, and a carbon fiber preform with a pyrolytic carbon interface layer was placed in the precursor solution for immersion at 8 MPa for 2 h, then cured at 100 ° C for 18 h, and finally carbonized at 800 ° C for 2 h. By repeating the immersion-curing-carbonization process, a carbon fiber preform with a density of 1.10 g / cm 3 A carbon fiber reinforced carbon aerogel preform, wherein the weight ratio of the carbon fiber, the interface layer and the carbon aerogel matrix is ​​9:4:7;

[0065] 2) The preform is polished with 200# and 800# silicon carbide sandpaper to remove the surface crust;

[0066] 3) Place the treated preform in anhydrous ethanol and ultrasonically clean it for 10 minutes;

[0067] 4) placing the preform in an oven at 120°C for 5 hours for drying;

[0068] 5) Mix a mixture of copper powder and silicon powder with a particle size of 120 μm and a weight ratio of Cu element of 15% with an appropriate amount of alcohol until it becomes a paste, and evenly spread it on the surface of the carbon fiber reinforced carbon aerogel preform;

[0069] 6) The carbon fiber reinforced carbon aerogel preform with powder on the surface is placed in a vacuum environment and heat treated at 1450° C. for 1 h to obtain a C / SiC-Cu composite material.

[0070] The density of the C / SiC-Cu composite material prepared in this example is 2.78 g / cm 3 Its SEM microstructure morphology is as follows Figure 3 As shown in the figure, the material is relatively dense, the metal matrix and the ceramic matrix are relatively evenly dispersed around the fiber, and no obvious pores and cracks are observed. Under oxyacetylene flame ablation, when the surface temperature of the C / SiC composite material is 2200°C, the surface temperature of the C / SiC-Cu composite material prepared in this embodiment is 1750°C (450°C lower than the surface temperature of the C / SiC composite material), and the mass ablation rate after ablation for 600s is 0.054mg / cm 2 / s, and the linear ablation rate is 0.018μm / s.

[0071] Embodiment 3:

[0072] In this embodiment, a mixture of silicon powder and silicon-copper alloy powder is infiltrated into a carbon fiber reinforced carbon aerogel preform. The specific process steps are as follows:

[0073] 1) Precursor solutions were prepared with glycerol and hydroxymethyl urea as pore formers and curing agents, respectively, wherein the weight ratio of phenolic resin: pore former: curing agent was 11:15:4, and a carbon fiber preform with a silicon carbide interface layer was placed in the precursor solution for immersion at 2 MPa for 10 h, then cured at 180 ° C for 12 h, and finally carbonized at 900 ° C for 2 h. By repeating the immersion-curing-carbonization process, a carbon fiber preform with a density of 1.20 g / cm 3 A carbon fiber reinforced carbon aerogel preform, wherein the weight ratio of the carbon fiber, the interface layer and the carbon aerogel matrix is ​​2:1:2;

[0074] 2) The preform is polished with 200# and 800# silicon carbide sandpaper to remove the surface crust;

[0075] 3) Place the treated preform in anhydrous ethanol and ultrasonically clean it for 10 minutes;

[0076] 4) placing the preform in an oven at 120°C for 5 hours for drying;

[0077] 5) A mixture of silicon powder and silicon-copper alloy powder with a particle size of 80 μm and a weight ratio of Cu element of 20% is mixed with an appropriate amount of alcohol to a paste, and evenly spread on the surface of the carbon fiber reinforced carbon aerogel preform;

[0078] 6) The carbon fiber reinforced carbon aerogel preform with powder on the surface is placed in a vacuum environment and heat treated at 1500°C for 1 hour to obtain a C / SiC-Cu composite material.

[0079] The density of the C / SiC-Cu composite material prepared in this example is 2.62 g / cm 3 Its microstructure morphology is as follows Figure 4 As shown in FIG. 1 , the dark gray and light gray regions are evenly distributed alternately, indicating that the ceramic matrix and the metal matrix in the composite material are evenly distributed. The surface temperatures of the C / SiC-Cu composite material and the C / SiC composite material prepared in this embodiment under the same ablation conditions are shown in FIG. Figure 5 As shown in the figure, under the same ablation conditions, the surface temperatures of C / SiC-Cu and C / SiC composite materials are 1750°C and 2500°C respectively, and the former is 750°C lower than the latter, showing a good cooling effect; after ablation for 600s, the mass ablation rate of the C / SiC-Cu composite material prepared in this embodiment is 0.060mg / cm 2 / s, and the linear ablation rate is -0.012μm / s.

[0080] Embodiment 4:

[0081] In this embodiment, a mixture of silicon-zirconium alloy powder and silicon-copper alloy powder is infiltrated into a carbon fiber reinforced carbon aerogel preform. The specific process steps are as follows:

[0082] 1) A precursor solution was prepared with ethylene glycol and benzenesulfonyl chloride as pore former and curing agent, respectively, wherein the weight ratio of phenolic resin: pore former: curing agent was 8:10:4, and a carbon fiber preform with a silicon carbide interface layer was placed in the precursor solution for immersion at 3 MPa for 5 h, then cured at 150 ° C for 16 h, and finally carbonized at 900 ° C for 2 h. By repeating the immersion-curing-carbonization process, a carbon fiber preform with a density of 1.20 g / cm 3 A carbon fiber reinforced carbon aerogel preform, wherein the weight ratio of the carbon fiber, the interface layer and the carbon aerogel matrix is ​​8:4:9;

[0083] 2) The preform is polished with 200# and 800# silicon carbide sandpaper to remove the surface crust;

[0084] 3) Place the treated preform in anhydrous ethanol and ultrasonically clean it for 10 minutes;

[0085] 4) placing the preform in an oven at 120°C for 5 hours for drying;

[0086] 5) A mixture of silicon-zirconium alloy powder and silicon-copper alloy powder with a particle size of 300 μm and a weight ratio of Cu element of 30% is mixed with an appropriate amount of alcohol to a paste, and evenly spread on the surface of the carbon fiber reinforced carbon aerogel preform;

[0087] 6) The carbon fiber reinforced carbon aerogel preform with powder on the surface is placed in a vacuum environment and heat treated at 1700°C for 2 hours to obtain a C / SiC-ZrC-Cu composite material.

[0088] The density of the C / SiC-ZrC-Cu composite material prepared in this example is 2.96 g / cm 3 Its SEM microstructure morphology is as follows Figure 6 As shown in (a), the dark gray and light gray areas are evenly dispersed, indicating that the ceramic matrix and the metal matrix in the composite material are evenly distributed; the distribution of the three elements Si, Zr and Cu is shown in Figure 6 (b) shows that the ceramic and metal phases in the composite matrix are relatively uniformly distributed. Under oxyacetylene flame ablation, when the surface temperature of the C / SiC composite material is 2200°C, the surface temperature of the C / SiC-ZrC-Cu composite material prepared in this embodiment is 1900°C (300°C lower than the surface temperature of the C / SiC composite material). After ablation for 600s, the mass ablation rate is 0.046mg / cm 2 / s, and the linear ablation rate is 0.012μm / s.

[0089] Embodiment 5:

[0090] In this embodiment, silicon-zirconium-copper alloy powder is infiltrated into a carbon fiber reinforced carbon aerogel preform, and the specific process steps are as follows:

[0091] 1) A precursor solution was prepared with propylene glycol and benzenesulfonyl chloride as pore former and curing agent, respectively, wherein the weight ratio of phenolic resin: pore former: curing agent was 5:8:2, and a carbon fiber preform with a pyrolytic carbon interface layer was placed in the precursor solution for immersion at 7 MPa for 3 h, then cured at 200 ° C for 10 h, and finally carbonized at 900 ° C for 2 h. By repeating the immersion-curing-carbonization process, a carbon fiber preform with a density of 1.26 g / cm 3 A carbon fiber reinforced carbon aerogel preform, wherein the weight ratio of the carbon fiber, the interface layer and the carbon aerogel matrix is ​​7:4:8;

[0092] 2) The preform is polished with 200# and 800# silicon carbide sandpaper to remove the surface crust;

[0093] 3) Place the treated preform in anhydrous ethanol and ultrasonically clean it for 10 minutes;

[0094] 4) placing the preform in an oven at 120°C for 5 hours for drying;

[0095] 5) Mix silicon-zirconium-copper alloy powder with a particle size of 180 μm and a weight ratio of Cu element of 35% with an appropriate amount of alcohol until it becomes a paste, and evenly spread it on the surface of the carbon fiber reinforced carbon aerogel preform;

[0096] 6) The carbon fiber reinforced carbon aerogel preform with powder on the surface was placed in a vacuum environment and heat treated at 1650° C. for 1.5 h to obtain a C / SiC-ZrC-Cu composite material.

[0097] The density of the C / SiC-ZrC-Cu composite material prepared in this example is 3.17 g / cm 3 , wherein the metal matrix and the ceramic matrix are uniformly dispersed. Under oxyacetylene flame ablation, when the surface temperature of the C / SiC composite material is 2300°C, the surface temperature of the C / SiC-ZrC-Cu composite material prepared in this embodiment is 1800°C (500°C lower than the surface temperature of the C / SiC composite material).

[0098] Embodiment 6:

[0099] In this embodiment, silicon-zirconium-hafnium-copper alloy powder is infiltrated into a carbon fiber reinforced carbon aerogel preform, and the specific process steps are as follows:

[0100] 1) A precursor solution was prepared with ethylene glycol and hydroxymethyl urea as pore former and curing agent, respectively, wherein the weight ratio of phenolic resin: pore former: curing agent was 14:19:5, and a carbon fiber preform with a silicon carbide interface layer was placed in the precursor solution for immersion at 5 MPa for 6 h, then cured at 160 ° C for 10 h, and finally carbonized at 1000 ° C for 2 h. By repeating the immersion-curing-carbonization process, a carbon fiber preform with a density of 1.30 g / cm 3 A carbon fiber reinforced carbon aerogel preform, wherein the weight ratio of the carbon fiber, the interface layer and the carbon aerogel matrix is ​​7:4:9;

[0101] 2) The preform is polished with 200# and 800# silicon carbide sandpaper to remove the surface crust;

[0102] 3) Place the treated preform in anhydrous ethanol and ultrasonically clean it for 10 minutes;

[0103] 4) placing the preform in an oven at 120°C for 5 hours for drying;

[0104] 5) Mix silicon-zirconium-hafnium-copper alloy powder with a particle size of 200 μm and a weight ratio of Cu element of 40 with an appropriate amount of alcohol until it becomes a paste, and evenly spread it on the surface of the carbon fiber reinforced carbon aerogel preform;

[0105] 6) The carbon fiber reinforced carbon aerogel preform with powder on the surface is placed in a vacuum environment and heat treated at 1800°C for 1 hour to obtain a C / SiC-ZrC-HfC-Cu composite material.

[0106] The density of the C / SiC-ZrC-HfC-Cu composite material prepared in this example is 3.36 g / cm 3 , wherein the metal matrix and the ceramic matrix are uniformly dispersed. Under oxyacetylene flame ablation, when the surface temperature of the C / SiC composite material is 2500°C, the surface temperature of the C / SiC-ZrC-HfC-Cu composite material prepared in this embodiment is 1850°C (650°C lower than the surface temperature of the C / SiC composite material).

Claims

1. A method for preparing a low-cost carbon fiber reinforced metal-ceramic matrix composite material for aerospace thermal protection system, characterized in that: The method specifically comprises the following steps: (1) Preform preparation: The carbon fiber preform with the interface layer is placed in a precursor solution for high pressure impregnation, followed by curing and carbonization treatment; (2) Repeat step (1) of impregnation-curing-carbonization process for many times to obtain a density of 0.8-1.5 g / cm 3 Carbon fiber reinforced carbon aerogel preform; (3) Preform polishing: polish the carbon fiber reinforced carbon aerogel preform obtained in step (1) with 200# and 800# silicon carbide sandpaper in turn to remove the surface crust of the preform; (4) Ultrasonic cleaning: The polished carbon fiber reinforced carbon aerogel preform in step (2) is placed in anhydrous ethanol and ultrasonically cleaned for 10 min; (5) Drying: The carbon fiber reinforced carbon aerogel preform after cleaning in step (3) is placed in a 120°C oven for 5 h for drying; (6) Powder spreading: Weigh a certain mass of alloy powder and evenly spread it on the surface of the carbon fiber reinforced carbon aerogel preform after the drying treatment in step (4); (7) Infiltration: placing the carbon fiber reinforced carbon aerogel preform with powder on the surface in step (6) in a vacuum environment and subjecting it to high temperature heat treatment to obtain the carbon fiber reinforced metal-ceramic matrix composite material; The alloy powder contains Cu and Si elements, and also contains one or more of the simple refractory metal elements of Zr, Hf, Ta, Ti, Nb, V and Mo; In step (1), the interface layer is one or a combination of two of pyrolytic carbon, silicon carbide and boron nitride; the pressure of the high-pressure impregnation is 2-8 MPa, and the time is 0.5-5 h; the temperature of the curing treatment is 100-250 ° C, and the curing time is 10-20 h; the temperature of the carbonization treatment is 600-1200 ° C, and the carbonization time is 0.5-5 h; In step (2), the carbon fiber reinforced carbon aerogel preform is composed of carbon fiber, an interface layer and a carbon aerogel matrix with a three-dimensional interconnected nanoporous structure, and the weight ratio of the carbon fiber, the interface layer and the carbon aerogel matrix with a three-dimensional interconnected nanoporous structure is (1-5):(1-4):(1-8); In step (6), the weight proportion of the Cu element in the alloy powder is 10-50 wt.%.

2. The method for preparing a carbon fiber reinforced metal-ceramic matrix composite material according to claim 1, characterized in that: In step (1), the precursor solution is prepared by mixing a phenolic resin, a pore former and a curing agent in a weight ratio of (5-15):(8-20):(1-5); wherein the pore former is one or more of ethanol, ethylene glycol and propylene glycol, and the curing agent is one or more of benzenesulfonyl chloride, hexamethylenetetramine and hydroxymethyl urea.

3. The method for preparing a carbon fiber reinforced metal-ceramic matrix composite material according to claim 1, characterized in that: In step (6), the powder spreading process includes mixing the alloy powder with an appropriate amount of alcohol to form a paste, and evenly spreading the powder on the surface of the carbon fiber reinforced carbon aerogel preform; the average particle size of the alloy powder is 1-500 μm.

4. The method for preparing a carbon fiber reinforced metal-ceramic matrix composite material according to claim 1, characterized in that: In step (7), the temperature of the high temperature heat treatment is 1000-2200°C, and the holding time is 0.5-4 h.

5. A carbon fiber reinforced metal-ceramic matrix composite material prepared according to any one of claims 1 to 4, characterized in that: The carbon fiber reinforced metal-ceramic matrix composite material has a density of 2.5-4.0 g / cm 3 ; The material consists of a carbon fiber reinforcement with an interface layer and a ceramic matrix and a metal matrix that are evenly dispersed with each other; the ceramic matrix includes one or more of SiC and ZrC, HfC, TaC, TiC, NbC, VC, and MoC; the metal matrix is ​​a mixture of copper and copper alloys; under the same ablation conditions, compared with the carbon fiber reinforced ceramic matrix composite material, the surface temperature of the carbon fiber reinforced metal-ceramic matrix composite material decreases by 200-850 ℃, and the ablation resistance is better.