Carbon dioxide solid recovery material and manufacturing method thereof

By supporting or granulating sodium ferrite on porous materials to form a high-concentration molded body, the problem of insufficient performance of existing carbon dioxide solid recovery materials in low-temperature environments is solved, and efficient carbon dioxide fixation and stabilization in the range from room temperature to 200°C is achieved. Recycling, suitable for small and medium-sized facilities.

CN116234625BActive Publication Date: 2024-10-11TODA KOGYO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180057894.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-10-29
Filing Date
2021-07-29
Publication Date
2024-10-11
Estimated Expiration
2041-07-29

AI Technical Summary

Technical Problem

Existing carbon dioxide solid recovery materials have insufficient carbon dioxide fixation and recovery performance in low-temperature environments, and sodium ferrite powder is prone to pressure loss during operation and filling, making it difficult to effectively apply in small and medium-sized facilities.

Method used

By loading sodium ferrite on porous materials or using porous materials to granulate, a molded body with a high concentration of sodium ferrite is formed to ensure efficient fixation and recovery of carbon dioxide in the temperature range from room temperature to 200°C, improve the morphological characteristics of the material, and Reduce pressure loss.

Benefits of technology

It achieves excellent carbon dioxide fixed recovery performance in the range of room temperature to 200°C, improves the formability and processability of the material, reduces energy costs, and is suitable for carbon dioxide recovery in small and medium-sized facilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116234625B_ABST
    Figure CN116234625B_ABST
Patent Text Reader

Abstract

The carbon dioxide solid recovery material of the present invention is a carbon dioxide solid recovery material containing 1 wt% to 99 wt% of sodium ferrite and 1 wt% to 99 wt% of porous material, with an average particle size of 1 mm to 10 mm and a specific surface area of ​​5 m 2 / g~1500m 2 / g, and the axial ratio of the average major axis diameter to the average minor axis diameter of the primary particles of the sodium ferrite is 1 to 2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a solid recovery material for fixing carbon dioxide and a method for making the same, in particular to a solid recovery material containing sodium ferrite and a method for making the same. Background Art

[0002] In the past, in order to reduce the amount of carbon dioxide emitted into the atmosphere, research has been conducted on the recovery, storage, and recycling of carbon dioxide. As large-scale sources of carbon dioxide, there are thermal power plants, boilers in manufacturing plants, and kilns in cement plants that use coal, heavy oil, natural gas, etc. as fuels. In addition, there are blast furnaces in iron and steel plants that use coke to reduce iron oxide, or transportation equipment such as automobiles, ships, and airplanes that use gasoline, heavy oil, and light oil as fuels.

[0003] Currently, in large facilities such as thermal power plants, amine aqueous solutions are used to fix and recover carbon dioxide. Since this method uses liquid recovery materials, it has the advantage that the recovery materials can be transported by pumps.

[0004] However, since liquids containing dangerous goods are used in the above method, it is difficult to apply it to small and medium-sized facilities such as waste incineration plants. As a result, the current situation is that it is almost impossible to complete the fixation and recovery of carbon dioxide. Therefore, solid carbon dioxide solid recovery materials made of solid, especially non-hazardous inorganic materials are expected. As existing solid carbon dioxide recovery materials, carbon dioxide recovery materials containing sodium ferrite are disclosed in Patent Documents 1 and 2. Among them, α-sodium ferrite with a layered rock salt structure (trigonal system) causes carbon dioxide to react with sodium by topological chemical reaction. That is, α-sodium ferrite forms Na in the reaction with carbon dioxide. 1-x A mixed phase of FeO2 and sodium carbonate. Therefore, the reaction rate is reported to be fast and the reaction has excellent repetitive performance for carbon dioxide absorption / release. On the other hand, since orthorhombic β-sodium ferrite reacts sodium with carbon dioxide, the crystalline phase of β-sodium ferrite is reported to absorb more carbon dioxide than the crystalline phase of α-sodium ferrite.

[0005] Generally, the reaction formula of sodium ferrite and carbon dioxide is NaFeO2+1 / 2CO2→1 / 2Na2CO3+1 / 2Fe2O3 when there is no water vapor in the gas, and NaFeO2+CO2+1 / 2H2O→NaHCO3+1 / 2Fe2O3 when there is water vapor. Therefore, sodium ferrite theoretically has the ability to adsorb / desorb up to 18 to 28% by weight of carbon dioxide.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2016-3156

[0009] Patent Document 2: Japanese Patent Application Publication No. 2017-109198 Summary of the invention

[0010] -Problems to be solved by the invention-

[0011] The solid recovery material of carbon dioxide recorded in Patent Documents 1 and 2 contains sodium ferrite as described above, and is therefore considered to be a solid recovery material with good absorption performance of carbon dioxide in low temperature areas. However, there is still a need for a carbon dioxide recovery material with higher fixed recovery performance of carbon dioxide. In addition to improving the characteristics of sodium ferrite itself, it is also necessary to further improve the characteristics under the form installed in the carbon dioxide recovery device. Specifically, sodium ferrite powder is difficult to handle in a powder state, especially when sodium ferrite is filled into an adsorption tower for use, because the fine powder is dense and pressure loss is easily generated, so it is carried on a specified carrier or granulated into a specified shape for use. Therefore, the composition and physical properties of the carbon dioxide recovery material in the state where sodium ferrite is carried or granulated are also very important.

[0012] The present invention is completed in view of the above-mentioned problems, and its purpose is to provide a carbon dioxide solid recovery material and a method for manufacturing the same, wherein the carbon dioxide solid recovery material can fix carbon dioxide in a low temperature range from room temperature to 200°C, and can recover carbon dioxide by heating at 50 to 200°C, and has excellent fixation and recovery performance.

[0013] -Solutions to solve the problem-

[0014] In order to achieve the above-mentioned purpose, in the present invention, by supporting sodium ferrite on a porous material or granulating sodium ferrite using a porous material under specified conditions, carbon dioxide can be fixed in a temperature range of room temperature to 200°C, and the fixed carbon dioxide can be efficiently recovered by heating at 50 to 200°C.

[0015] Specifically, the carbon dioxide solid recovery material of the present invention is characterized in that it is a carbon dioxide solid recovery material comprising 1 wt% to 99 wt% of sodium ferrite and 1 wt% to 99 wt% of a porous material, and the average particle size of the carbon dioxide solid recovery material is 1 mm to 10 mm, and the specific surface area is 5 m 2 / g~1500m 2 / g, and the axial ratio of the average major axis diameter to the average minor axis diameter of the primary particles of the sodium ferrite is 1 to 2.

[0016] According to the carbon dioxide solid recovery material of the present invention, a molded body containing high concentration of sodium ferrite can be formed by using a porous material. Therefore, the carbon dioxide solid recovery material of the present invention containing sodium ferrite and a porous material has the excellent property of being able to fix carbon dioxide in the gas and seal it in a solid, and recover carbon dioxide by heating. In addition, if the average particle size is 1 to 10 mm, when filled in an adsorption tower, etc., it is possible to ensure the flow path of exhaust gas, etc. without reducing the pressure loss caused by the dense fine powder. As a result, carbon dioxide can be effectively fixed. In addition, the axis ratio of the average major axis diameter of the primary particles to the average minor axis diameter is as small as 1 to 2, and the shape is close to a sphere, so the dispersibility is high, and the primary particles are not easy to agglomerate, thereby improving the formability and processability. These characteristics are combined with each other, and according to the carbon dioxide solid recovery material of the present invention, carbon dioxide can be fixed in a temperature range of room temperature to 200°C, and carbon dioxide can be recovered by heating at 50 to 200°C, and the fixed recovery performance is excellent.

[0017] Preferably, the carbon dioxide solid recovery material of the present invention contains 1 wt% to 70 wt% of the sodium ferrite, 30 wt% to 99 wt% of the porous material, and has a specific surface area of ​​100 m 2 / g~1500m 2 / g.

[0018] Thus, by carrying a large amount of sodium ferrite on the surface of the porous material as a carrier, a molded body containing high-density sodium ferrite can be formed. Therefore, the carbon dioxide solid recovery material of the present invention containing sodium ferrite and a porous material has the excellent properties of being able to fix carbon dioxide in the gas and seal it into a solid, and recover carbon dioxide by heating. In addition, in the case where 1 wt% to 70 wt% of sodium ferrite is carried on 30 wt% to 99 wt% of a porous material, if the specific surface area is less than 100 m 2 / g, it is difficult to contact with the carbon dioxide contained in the gas, and the fixation and recovery performance of carbon dioxide is reduced. If the specific surface area is greater than 1500m 2 / g, it is difficult to carry out industrial production.

[0019] At this time, preferably, the hardness is 5kgf / mm 2 ~35kgf / mm 2 , the bulk density is 0.3g / mL~0.8g / mL.

[0020] Thus, when the adsorption tower is filled, it is less likely to be damaged by gravity or friction caused by the flow of exhaust gas, etc., and the flow of exhaust gas, etc., is facilitated.

[0021] Preferably, the carbon dioxide solid recovery material of the present invention contains more than 70% by weight and less than or equal to 99% by weight of the sodium ferrite, contains more than or equal to 1% by weight and less than 30% by weight of the porous material, and has a specific surface area of ​​5m 2 / g~500m 2 / g.

[0022] Thus, the porous material can promote the aggregation of sodium ferrite particles to form a molded body containing a high concentration of sodium ferrite. Therefore, the carbon dioxide solid recovery material of the present invention containing sodium ferrite and a porous material has the excellent properties of being able to adsorb carbon dioxide in the gas, seal the carbon dioxide in the solid, and release the carbon dioxide by heating. In addition, when a porous material greater than or equal to 1% by weight and less than 30% by weight is used to granulate more than 70% by weight and less than or equal to 99% by weight of sodium ferrite, if the specific surface area is less than 5m 2 / g, it is difficult to contact with the carbon dioxide contained in the gas, and the fixation and recovery performance of carbon dioxide is reduced. If the specific surface area is greater than 500m 2 / g, it is difficult to carry out industrial production.

[0023] At this time, preferably, the hardness is 3kgf / mm 2 ~30kgf / mm 2 , the sphericity is 1 to 2.

[0024] Thus, when the adsorption tower is filled, it is less likely to be damaged by gravity or friction caused by the flow of exhaust gas, etc., and the flow of exhaust gas, etc., is facilitated.

[0025] Preferably, in the carbon dioxide solid recovery material of the present invention, the pH value of the powder is 8-14.

[0026] Therefore, since the carbon dioxide solid recovery material according to the present invention is alkaline, it is easy to capture weakly acidic carbon dioxide.

[0027] Preferably, in the carbon dioxide solid recovery material of the present invention, the Na / Fe molar ratio of the sodium ferrite is 0.7 to 1.3.

[0028] Since the Na / Fe molar ratio is 0.7 to 1.3, a large amount of sodium ferrite crystal phase can be contained, thereby having good carbon dioxide fixation and recovery performance.

[0029] Preferably, in the carbon dioxide solid recovery material of the present invention, the porous material is a porous material selected from activated carbon, aluminosilicate, hydrotalcite, porous clay minerals, porous silica, and activated alumina.

[0030] By using the porous material, a molded body containing a high concentration of sodium ferrite can be formed, thereby improving the ability to fix and recover carbon dioxide.

[0031] The method for producing the carbon dioxide solid recovery material of the present invention is characterized in that it includes a step of solid phase reaction of a material containing iron oxide with an alkaline compound containing sodium.

[0032] In the manufacturing method of the carbon dioxide solid recovery material of the present invention, by mixing solids with solids, the elements are moved to react without using a solvent. Since the solvent as the reaction mother liquid is not used, waste such as the solvent used in the liquid phase reaction can be reduced. In particular, in the case of a low-temperature solid phase reaction, a very high concentration reaction can be carried out, so the energy cost can be reduced. Therefore, according to the manufacturing method of the carbon dioxide solid recovery material of the present invention, carbon dioxide can be fixed in a temperature range of room temperature to 200°C, and the fixed carbon dioxide can be efficiently recovered by heating at 50 to 200°C, so that a carbon dioxide recovery material with excellent fixing and recovery performance can be manufactured.

[0033] -Effects of the Invention-

[0034] The carbon dioxide solid recovery material according to the present invention can fix carbon dioxide in a temperature range from room temperature to 200° C., and can efficiently recover carbon dioxide by heating at 50 to 200° C., thereby having excellent carbon dioxide fixation and recovery performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is the result of thermogravimetric analysis after the carbon dioxide solid recovery material obtained in Example 1 absorbed carbon dioxide.

[0036] Figure 2 This is the result of thermogravimetric analysis after the carbon dioxide solid recovery material obtained in Example 9 absorbed carbon dioxide. DETAILED DESCRIPTION

[0037] The following description of the preferred embodiments is merely illustrative in nature and is not intended to limit the present invention, the applicable methods of the present invention, or the uses of the present invention.

[0038] (First Embodiment)

[0039] First, the carbon dioxide solid recovery material according to the first embodiment of the present invention will be described.

[0040] The carbon dioxide solid recovery material involved in this embodiment includes: 1 wt% to 70 wt% of sodium ferrite and 30 wt% to 99 wt% of porous material. If it is within the above weight % range, the sodium ferrite can be stably supported on the porous material while maintaining the original carbon dioxide fixation and recovery performance of the sodium ferrite.

[0041] The carbon dioxide solid recovery material according to the present embodiment has an average particle size of 1 mm to 10 mm and a specific surface area of ​​100 m 2 / g~1500m 2 / g. If the average particle size is less than 1mm, when the carbon dioxide solid recovery material involved in this embodiment is filled into an adsorption tower, the gap between the powders is reduced, which increases the pressure loss in the adsorption tower. Therefore, clogging may occur in the adsorption tower. If the average particle size is greater than 10mm, the contact rate between sodium ferrite and carbon dioxide decreases, and the fixed recovery performance of carbon dioxide decreases. The average particle size of the carbon dioxide solid recovery material is preferably 2mm to 8mm. In addition, if the specific surface area is less than 100m 2 / g, it is difficult to contact with carbon dioxide contained in the gas, and the fixation and recovery performance of carbon dioxide is reduced. If the specific surface area is greater than 1500m 2 / g, it is difficult to carry out industrial production. The specific surface area of ​​the solid carbon dioxide recovery material is preferably 300m 2 / g~1000m 2 / g.

[0042] In the carbon dioxide solid recovery material involved in the present embodiment, the axial ratio of the average major axis diameter of the primary particles of sodium ferrite to the average minor axis diameter (average major axis diameter / average minor axis diameter) is 1 to 2. If the axial ratio is greater than 2, the primary particles are easily agglomerated with each other, and it is difficult for sodium ferrite to maintain a highly dispersed state. In addition, the axial ratio cannot be less than 1. The axial ratio of the primary particles of the carbon dioxide solid recovery material is preferably 1.1 to 1.9.

[0043] The shape of the solid recovery material is not particularly limited, but is preferably a spherical shape, a spindle shape, a rectangular parallelepiped shape, a dice shape, a cylindrical shape, or the like.

[0044] Preferably, the hardness of the carbon dioxide solid recovery material involved in this embodiment is 5kgf / mm 2 ~35kg / mm 2 , the bulk density is 0.3g / mL to 0.8g / mL. If the hardness and bulk density are within the above range, it is not easy to be damaged by gravity or friction caused by the flow of exhaust gas when filled in an adsorption tower, etc., and it is convenient for the flow of exhaust gas and other gases. The more preferred hardness is 6kgf / mm 2 ~33kgf / mm 2, the bulk density is 0.35g / mL~0.70g / mL.

[0045] The powder pH value of the carbon dioxide solid recovery material according to the present embodiment is preferably 8 to 14. If the powder pH value is 8 to 14, the carbon dioxide solid recovery material according to the present embodiment is alkaline and thus easily captures weakly acidic carbon dioxide. A more preferred powder pH value is 9 to 14.

[0046] In the carbon dioxide solid recovery material according to the present embodiment, the Na / Fe molar ratio of the sodium ferrite is preferably 0.7 to 1.3. Within the above molar ratio range, a large amount of sodium ferrite crystal phase can be contained, thereby having good carbon dioxide fixation and recovery performance.

[0047] The porous material involved in the present embodiment is a porous material selected from porous clay minerals such as activated carbon, zeolite, porous silica and activated alumina. In addition to zeolite, porous clay minerals can also use smectite, sepiolite, imogolite, palygorskite, kaolin, montmorillonite, bentonite, attapulgite, acid clay, cordierite, limonite, etc. Because the above-mentioned porous material has excellent adsorption, it can carry a large amount of sodium ferrite, so that the fixed recovery capacity of carbon dioxide can be improved. In particular, because the micropore diameter of activated carbon is small, it has a strong adsorption force. Therefore, activated carbon can carry a large amount of sodium ferrite, improve the fixed recovery capacity of carbon dioxide, which is more preferred.

[0048] As the porous material, it is preferred that the porosity is greater than 50% and less than or equal to 70%. If the porosity is less than 50%, the specific surface area of ​​the carbon dioxide solid recovery material, that is, the contact area with carbon dioxide, is reduced, and the absorption rate of carbon dioxide is likely to decrease. If the porosity is greater than 70%, the volume ratio of sodium ferrite is reduced, and the fixed recovery performance of carbon dioxide is reduced.

[0049] The carbon dioxide solid recovery material involved in this embodiment can selectively adsorb and fix carbon dioxide from a gas containing carbon dioxide. The above-mentioned adsorption temperature is about 10°C to 200°C between room temperature and the exhaust gas outlet temperature. Since no additional heating from the outside is required, the energy cost consumed by adsorption can be reduced (the above is the carbon dioxide fixation process).

[0050] Preferably, the carbon dioxide solid recovery material involved in this embodiment desorbs the carbon dioxide captured in the above-mentioned carbon dioxide fixation process in a gas atmosphere without carbon dioxide at a temperature of 50 to 200° C. to recover carbon dioxide. Since the desorption temperature is as low as below 200° C., the energy cost consumed by desorption can be reduced (the above is the carbon dioxide recovery process).

[0051] Next, the method for producing the carbon dioxide solid recovery material according to the first embodiment of the present invention will be described.

[0052] The carbon dioxide solid recovery material according to the present embodiment can be obtained by reacting a material containing iron oxide with a basic compound containing sodium in the presence of a porous material (support).

[0053] When the material containing iron oxide is reacted with the alkaline compound containing sodium in the presence of a porous material (support), there is a tendency to carry a large amount of sodium ferrite on the surface of the support. Therefore, the fixed recovery performance of carbon dioxide is improved, and it is preferably used as a carbon dioxide solid recovery material. In addition, as a feature of solid phase reaction, the crystal growth of sodium ferrite tends to be isotropic, so there is a tendency to suppress the axial ratio of primary particles.

[0054] As a specific manufacturing method, iron oxide is mixed with a sodium source powder, and then mixed with a porous material, so that the mixture of iron oxide and sodium source powder is attached to the surface of the porous material, and the carbon dioxide solid recovery material involved in this embodiment can be obtained by firing. Granulation can be performed as needed. In addition, in addition to conventional firing, steam heating, microwave heating, ultrasonic heating, etc. can also be performed.

[0055] As other manufacturing examples, the following methods i) to iv) can also be used. i) The sodium source aqueous solution is adsorbed on the porous material, directly dried, and iron oxide is added for solid phase synthesis. ii) The iron oxide aqueous slurry is adsorbed on the porous material, directly dried, and sodium source powder is added for solid phase synthesis. iii) The iron oxide and the sodium source powder are reacted in a solid phase, and the reactant is attached to the porous material. iv) The iron oxide and the sodium source are reacted by a wet method, and then attached to the porous material by a wet method, and then dried.

[0056] As a support, for example, a porous material selected from porous clay minerals such as activated carbon and zeolite, porous silica and activated alumina can be used. In addition to zeolite, porous clay minerals can also use smectite, sepiolite, imogolite, palygorskite, kaolin, montmorillonite, bentonite, attapulgite, acid clay, cordierite, limonite, etc. The content of the porous material is preferably 30% to 99% by weight. This is because, as mentioned above, by carrying a large amount of sodium ferrite, the fixation and recovery capacity of carbon dioxide is improved.

[0057] The material containing iron oxide is not particularly limited, and for example, ferrous chloride tetrahydrate, iron (III) chloride hexahydrate, and iron (II) sulfate heptahydrate can be used.

[0058] The sodium-containing compound is not particularly limited, and for example, sodium nitrite, sodium sulfate, sodium carbonate, sodium bicarbonate, and sodium hydroxide can be used. However, in consideration of industrial use, sodium nitrite and sodium sulfate, which may generate toxic nitrous acid gas and sulfurous acid gas during production, should be avoided.

[0059] Usually, solid phase reaction is to mix solid with solid, and to make the synthetic method of element moving and reacting when not using solvent.Owing to not using solvent as reaction mother solution, therefore can reduce wastes such as solvent used in liquid phase reaction.In addition, in the case of low temperature solid phase reaction as feature of the present invention, can carry out extremely high concentration reaction, therefore can also reduce energy cost.In addition, owing to not needing above-mentioned high reaction concentration and washing, therefore can expect high yield of product.

[0060] (Second Embodiment)

[0061] Next, a carbon dioxide solid recovery material according to a second embodiment of the present invention will be described.

[0062] The carbon dioxide solid recovery material involved in this embodiment contains more than 70 weight % and less than or equal to 99 weight % of sodium ferrite and more than or equal to 1 weight % and less than 30 weight % of porous material. If it is within the above weight % range, the carbon dioxide solid recovery material involved in this embodiment can form a molded body containing high concentration of sodium ferrite while maintaining the original carbon dioxide fixation and recovery performance of sodium ferrite.

[0063] The carbon dioxide solid recovery material according to the present embodiment has an average particle size of 1 mm to 10 mm and a specific surface area of ​​5 m 2 / g~500m 2 / g. If the average particle size is less than 1mm, when the carbon dioxide solid recovery material involved in this embodiment is filled into an adsorption tower, the gap between the powders is reduced, which increases the pressure loss in the adsorption tower. Therefore, clogging may occur in the adsorption tower. If the average particle size is greater than 10mm, the contact rate between sodium ferrite and carbon dioxide decreases, and the fixed recovery performance of carbon dioxide decreases. The average particle size of the carbon dioxide solid recovery material is preferably 2mm to 8mm. In addition, if the specific surface area is less than 5m 2 / g, it is difficult to contact with carbon dioxide contained in the gas, and the fixation and recovery performance of carbon dioxide is reduced. If the specific surface area is greater than 500m 2 / g, it is difficult to carry out industrial production. The specific surface area of ​​the carbon dioxide solid recovery material is preferably 30m 2 / g~300m 2 / g.

[0064] In the carbon dioxide solid recovery material involved in the present embodiment, the axial ratio of the average major axis diameter of the primary particles of sodium ferrite to the average minor axis diameter (average major axis diameter / average minor axis diameter) is 1 to 2. If the axial ratio is greater than 2, the primary particles are easily agglomerated with each other, and it is difficult for sodium ferrite to maintain a highly dispersed state. In addition, the axial ratio cannot be less than 1. The axial ratio of the primary particles of the carbon dioxide solid recovery material is preferably 1.1 to 1.9.

[0065] In the carbon dioxide solid recovery material involved in this embodiment, the average primary particle size of the primary particles of sodium ferrite is preferably 0.05 μm to 1.0 μm. If it is less than 0.05 μm, it is difficult to carry out industrial production. In addition, if it is greater than 1.0 μm, the absorption performance of carbon dioxide is reduced. It is more preferably 0.1 μm to 0.7 μm.

[0066] Preferably, the hardness of the carbon dioxide solid recovery material involved in this embodiment is 3kgf / mm 2 ~30kgf / mm 2 , and the sphericity is 1 to 2. If the hardness and sphericity are within the above ranges, when the carbon dioxide recovery material involved in this embodiment is filled in an adsorption tower, etc., it is not easily damaged by gravity or friction caused by the circulation of exhaust gas, etc., and the circulation of exhaust gas, etc. is convenient.

[0067] The shape of the carbon dioxide solid recovery material is not particularly limited, and is preferably a spherical shape, a spindle shape, a rectangular parallelepiped shape, a dice shape, a cylindrical shape, or the like.

[0068] The powder pH of the carbon dioxide solid recovery material according to the present embodiment is preferably 8 to 14. When the powder pH is 8 to 14, the carbon dioxide solid recovery material according to the present embodiment becomes alkaline, and thus it is easy to capture weakly acidic carbon dioxide.

[0069] In the carbon dioxide solid recovery material according to the present embodiment, the Na / Fe molar ratio of sodium ferrite is preferably 0.7 to 1.3. Within the above molar ratio range, a large amount of sodium ferrite crystal phase can be contained, thereby having good carbon dioxide fixation and recovery performance.

[0070] The porous material involved in the present embodiment is preferably a porous material selected from activated carbon, aluminosilicate, hydrotalcite, porous clay mineral, porous silica and activated alumina. Porous clay minerals can use zeolite, smectite, sepiolite, imogolite, palygorskite, kaolin, montmorillonite, bentonite, attapulgite, acid clay, cordierite, limonite, etc. Since the above-mentioned porous material has excellent adsorption, it can form a molded body containing high concentration of sodium ferrite, thereby improving the fixation and recovery capacity of carbon dioxide.

[0071] As the porous material, it is preferred that the porosity is greater than 50% and less than or equal to 70%. If the porosity is less than 50%, the specific surface area of ​​the carbon dioxide solid recovery material, that is, the contact area with carbon dioxide, is reduced, and the absorption rate of carbon dioxide is likely to decrease. If the porosity is greater than 70%, the volume ratio of sodium ferrite is reduced, and the fixed recovery performance of carbon dioxide is reduced.

[0072] The carbon dioxide solid recovery material involved in this embodiment can selectively adsorb and fix carbon dioxide from a gas containing carbon dioxide. The above-mentioned adsorption temperature is about 10°C to 200°C between room temperature and the exhaust gas outlet temperature. Since no additional heating from the outside is required, the energy cost consumed by adsorption can be reduced (the above is the carbon dioxide fixation process).

[0073] Preferably, the carbon dioxide solid recovery material involved in this embodiment desorbs the carbon dioxide captured in the above-mentioned carbon dioxide fixation process in a gas atmosphere without carbon dioxide at a temperature of 50 to 200° C. to recover carbon dioxide. Since the desorption temperature is as low as below 200° C., the energy cost consumed by desorption can be reduced (the above is the carbon dioxide recovery process).

[0074] Next, a method for producing a carbon dioxide solid recovery material according to a second embodiment of the present invention will be described.

[0075] The carbon dioxide solid recovery material according to the present embodiment can be obtained by reacting a material containing iron oxide with a basic compound containing sodium in the presence of a porous material (support).

[0076] When the material containing iron oxide is reacted with the alkaline compound containing sodium in the presence of a porous material (support), there is a tendency to form a nearly spherical body containing high-concentration sodium ferrite. Therefore, the fixed recovery performance of carbon dioxide is improved, and it is preferably used as a carbon dioxide solid recovery material. In addition, as a feature of solid phase reaction, the crystal growth of sodium ferrite tends to be isotropic, so there is a tendency to suppress the axial ratio of primary particles.

[0077] As a specific manufacturing method, first, iron oxide and sodium source powder are mixed and crushed, and sodium ferrite particle powder is obtained by calcining, and then the obtained sodium ferrite particle powder is mixed with a porous material, and granulated using a granulator such as a rotary granulator. Then, a carbon dioxide solid recovery material can be obtained by calcining. In addition to conventional calcining, calcining can also be performed by steam heating, microwave heating, ultrasonic heating, etc.

[0078] As a support, for example, a porous material selected from porous clay minerals such as activated carbon, aluminosilicate, hydrotalcite, zeolite, porous silica and activated alumina can be used. In addition to zeolite, porous clay minerals can also use smectite, sepiolite, imogolite, palygorskite, kaolin, montmorillonite, bentonite, attapulgite, acid clay, cordierite, limonite, etc. The content of porous material is preferably greater than or equal to 1% by weight and less than 30% by weight. This is because as mentioned above, by forming a shaped body containing high concentration sodium ferrite, the fixed recovery capacity of carbon dioxide is improved.

[0079] The material containing iron oxide is not particularly limited, and for example, hematite, magnetite, maghemite, goethite, etc. can be used.

[0080] The sodium-containing compound is not particularly limited, and for example, sodium nitrite, sodium hydroxide, sodium oxide, sodium carbonate, etc. can be used. However, in consideration of industrial use, sodium nitrite, sodium sulfate, etc., which may generate toxic nitrous acid gas, sulfurous acid gas, etc. during production, should be avoided.

[0081] Usually, solid phase reaction is to mix solid with solid, and to make the synthetic method of element moving and reacting when not using solvent.Owing to not using solvent as reaction mother solution, therefore can reduce wastes such as solvent used in liquid phase reaction.In addition, in the case of low temperature solid phase reaction as feature of the present invention, can carry out extremely high concentration reaction, therefore can also reduce energy cost.In addition, owing to not needing above-mentioned high reaction concentration and washing, therefore can expect high yield of product.

[0082] [Example]

[0083] Representative embodiments of the present invention are shown below.

[0084] The composition of the carbon dioxide solid recovery material described in the present invention is identified in the following manner: the carbon dioxide solid recovery material is crushed and granulated with a mortar, and then identified using a fully automatic multifunctional X-ray diffraction device D8 ADVANCE manufactured by Bruker Corporation. The result shows that the material is sodium α-ferrate and a porous material.

[0085] The content of sodium ferrite and porous material contained in the carbon dioxide solid recovery material described in the present invention is quantified in the following manner: after the carbon dioxide solid recovery material is crushed and granulated with a mortar, elemental analysis (but excluding oxygen) is performed using a scanning fluorescent X-ray analyzer ZSX PrimusII manufactured by Rigaku Corporation, and quantification is performed.

[0086] The average particle size of the carbon dioxide solid recovery material of the present invention is determined by measuring the major axis and the minor axis of 80 particles using a caliper and taking the average value as the average particle size.

[0087] The BET specific surface area of ​​the carbon dioxide solid recovery material of the present invention is measured by the following method: using Multisorb-16 manufactured by QUANTA CHROME, the surface area is measured by the BET method using nitrogen.

[0088] The hardness of the carbon dioxide solid recovery material of the present invention is determined as follows: the average value of the crushing hardness of 80 particles is taken as the hardness using a digital dynamometer ZP-500N manufactured by IMADA CO., LTD.

[0089] The bulk density of the carbon dioxide solid recovery material of the present invention is measured according to Japanese Industrial Standard JIS Z2504.

[0090] The bulk density of the carbon dioxide solid recovery material according to the present invention is evaluated in the following four stages.

[0091] ◎: Carbon dioxide solid recovery material with bulk density of 0.3 to less than 0.5 g / mL

[0092] ○: Carbon dioxide solid recovery material with bulk density of 0.5-0.8 g / mL

[0093] △: Carbon dioxide solid recovery material with bulk density greater than 0.8 to less than 2g / mL

[0094] ×: Carbon dioxide solid recovery materials with a bulk density of less than 0.3 g / mL and greater than or equal to 2 g / mL

[0095] The sphericity of the carbon dioxide solid recovery material according to the present invention is evaluated in the following two stages by calculating the major axis / minor axis ratio.

[0096] ○: Carbon dioxide solid recovery material with a sphericity greater than or equal to 1 and less than 2

[0097] ×: Carbon dioxide solid recovery material with a sphericity of 2 or more

[0098] The pH value of the carbon dioxide solid recovery material described in the present invention is determined in the following manner: 5 g of the sample is weighed and placed in a 300 ml conical flask, 100 ml of boiling pure water is added, and the flask is heated and kept boiling for about 5 minutes, then the flask is plugged and cooled to room temperature, water corresponding to the weight loss is added, the flask is plugged again and shaken for 1 minute, and the pH value of the supernatant obtained is measured according to Japanese Industrial Standard JIS Z8802-7 after standing for 5 minutes, and the obtained value is used as the pH value.

[0099] The Na / Fe molar ratio of sodium ferrite contained in the carbon dioxide solid recovery material described in the present invention is obtained by the following method: after the carbon dioxide solid recovery material is crushed and granulated with a mortar, elemental analysis (but excluding oxygen) is performed using a scanning fluorescent X-ray analyzer ZSX PrimusII manufactured by Rigaku Corporation, and quantification is performed.

[0100] The axial ratio of the sodium ferrite contained in the carbon dioxide recovery material described in the present invention is calculated in the following manner: the average major axis diameter and the average minor axis diameter of the particle sizes of 350 primary particles shown in the microscope photograph of the scanning electron microscope S-4800 manufactured by Hitachi High-Tech Corporation are measured respectively, and expressed as the ratio of the above-mentioned average major axis diameter to the average minor axis diameter (average major axis diameter / average minor axis diameter).

[0101] The average primary particle size of the sodium ferrite particle powder contained in the carbon dioxide recovery material according to the present invention is represented by the average value of the above-mentioned average major axis diameter and average minor axis diameter.

[0102] In order to study the carbon dioxide fixation and recovery capacity of the carbon dioxide recovery material described in the present invention, 1.00 weight parts of the sample were placed on a combustion boat and put into an acrylic tube with inlet and outlet pipes. A mixed gas (carbon dioxide + nitrogen) with a humidity adjusted to a range of 20-100% and a carbon dioxide concentration adjusted to a range of 1-100 vol% was introduced from the inlet at a flow rate of 500 mL / min. The carbon dioxide adsorption amount after 2 hours was determined by using a differential thermal-thermogravimetric simultaneous measurement device STA7000 manufactured by Hitachi High-Tech Corporation. The temperature was raised from room temperature to 200°C, and the fixed carbon dioxide recovery amount was calculated based on its thermal weight loss.

[0103] <Method for producing solid carbon dioxide recovery material>

[0104] [Experimental Example 1]

[0105] Example 1

[0106] 9.0 parts by weight of ferrous chloride tetrahydrate are dissolved in 900 parts by weight of pure water, and 10.0 parts by weight of granular activated carbon (KURARAY CO., LTD. KURARAY COAL 4GG, 4×6 mesh) is added thereto as a porous support and immersed for 1 hour. 27 parts by weight of urea dissolved in 100 parts by weight of pure water are added thereto, the temperature is raised to 90°C, stirred for 3 hours, then cooled and stirred for 10 hours. Then, the solid matter remaining on the sieve is dried at 80°C for 12 hours through a 1mm mesh sieve to obtain activated carbon loaded with iron oxide. The obtained activated carbon loaded with iron oxide and 1.80 parts by weight of sodium hydroxide are mixed in solid form, the mixture is placed in a crucible, and a solid phase reaction is carried out at 400°C in a nitrogen flow for 16 hours. Then, it is cooled to room temperature and used as a solid recovery material for carbon dioxide. The obtained solid recovery material for carbon dioxide is crushed and characterized by X-ray diffraction, and the result is sodium ferrite and amorphous carbon. In addition, the content of sodium ferrite was 33% as determined by fluorescent X-ray. The content of porous material was 67%. The BET specific surface area of ​​the carbon dioxide solid recovery material was 678 m 2 / g. The short axis is 4mm, the long axis is 8mm, and the average particle size is 6mm. The pH value of the powder is 13.

[0107] The hardness of the obtained carbon dioxide solid recovery material is 20kgf / mm 2 , and the bulk density is 0.48 g / mL. These results show that when the carbon dioxide recovery material involved in Example 1 is filled into a carbon dioxide adsorption tower, etc., it is not easily damaged by gravity or friction caused by the circulation of exhaust gas, etc., and is convenient for the circulation of exhaust gas, etc. It should be noted that the hardness of the obtained carbon dioxide recovery material is evaluated according to the following three stages.

[0108] ○: crush hardness is 10kgf / mm 2 Carbon dioxide recovery materials

[0109] △: Crushing hardness is 5 to less than 10 kgf / mm 2 Carbon dioxide recovery materials

[0110] ×: Crushing hardness is less than 5kgf / mm 2 Carbon dioxide recovery materials

[0111] The Na / Fe molar ratio of sodium ferrite contained in the obtained carbon dioxide solid recovery material was 1.0, which was approximately the same as the feed ratio of the raw material.

[0112] In order to study the carbon dioxide fixation and recovery performance of the obtained carbon dioxide solid recovery material, 1.00 weight parts of the sample was placed on a No. 2 combustion boat (12×60×9mm), and 500mL / min of model combustion exhaust gas was introduced for 2 hours. Usually, the exhaust gas when burning fuel in the atmosphere is composed of a maximum of 80vol% nitrogen and 20vol% carbon dioxide with a relative humidity of RH80-100%. Therefore, at room temperature 25°C, 400mL / min of nitrogen and 100mL / min of carbon dioxide were mixed, and the mixed gas was introduced into water to prepare a model exhaust gas with 20vol% carbon dioxide and a relative humidity of RH80%.

[0113] Weigh 10 mg of the ventilated sample, use a thermogravimetric device (TG) to pass dry air at 300 mL / min and raise the temperature to 200°C at 10°C / min to measure the desorption temperature and desorption amount of carbon dioxide adsorbed on the sample. The horizontal axis is the sample temperature measurement diagram as shown in Figure 1 As shown. The TG curve is the weight % of the remaining sample at each temperature when the initial weight is 100%, and the sample loss is attributed to the release of carbon dioxide. The DTG curve is a differential curve of the TG curve, and the temperature at the maximum value of the DTG curve is regarded as the desorption temperature of carbon dioxide. The DTA curve appears as a downward convex curve, and it can be seen that the endothermic reaction occurs near 114°C. It is quantified by considering it as the thermal decomposition of NaHCO3, and the result shows that the desorption temperature of carbon dioxide is 114°C, and the desorption amount of carbon dioxide is 10 weight % relative to the solid content of the sample, which shows that it has excellent carbon dioxide fixation and recovery performance.

[0114] Furthermore, a new sample was prepared after ventilation, and the weight was measured, which was 1.15 parts by weight, confirming a 15% increase in mass. X-ray diffraction analysis of the sample surface confirmed that 85% by weight of Na 1-x FeO2 and 15 wt% NaHCO3, it can be seen that carbon dioxide is fixed on the sodium ferrite component. Furthermore, the sample was heated at 120°C in an electric furnace for 1 hour, and the weight was measured. The result was 1.05 parts by weight. It can be seen that 0.10 parts by weight (10 wt% relative to the solid recovery material of carbon dioxide) of carbon dioxide can be adsorbed / desorbed in this cycle. The X-ray diffraction of the surface of the sample was measured, and the result confirmed 90 wt% NaFeO2 and 10 wt% Na2CO3. Furthermore, as described above, when carbon dioxide was contacted with the sample, the amount was increased to 1.15 parts by weight, and the amount was reduced to 1.05 parts by weight when heated, and 0.10 parts by weight (10 wt% relative to the solid recovery material of carbon dioxide) of carbon dioxide can be adsorbed / desorbed. This operation was repeated 10 times, and it was confirmed that the increase or decrease in mass did not change. This shows that the solid recovery material of carbon dioxide involved in Example 1 has excellent carbon dioxide fixation and recovery performance, especially excellent repeatability.

[0115] Embodiments 2 to 8

[0116] Solid recovered materials according to Examples 2 to 8 were obtained in the same manner as in Example 1 except that the types and amounts of the iron raw material and the support were variously changed.

[0117] The production conditions of these examples are recorded in Table 1, the various properties of the obtained carbon dioxide solid recovery materials are recorded in Table 2, and the effects are recorded in Table 3.

[0118] Comparative Example 1

[0119] 9.0 parts by weight of ferrous chloride tetrahydrate was dissolved in 900 parts by weight of pure water and stirred for 1 hour. 27 parts by weight of urea dissolved in 100 parts by weight of pure water was added thereto, the temperature was raised to 90°C, stirred for 3 hours, then cooled and stirred for 10 hours, filtered and washed with water, and dried at 80°C for 12 hours to obtain iron oxide particles. The obtained iron oxide particles and 1.80 parts by weight of sodium hydroxide were mixed in solid form, the mixture was placed in a crucible, and a solid phase reaction was carried out at 400°C in a nitrogen stream for 16 hours. The obtained powder was crushed and determined to be sodium ferrite by X-ray diffraction. In addition, the content of sodium ferrite was 90% by weight by fluorescent X-ray. The remaining 10% by weight was hematite. The obtained powder was suspended in 100 parts by weight of pure water, 10 parts by weight of activated carbon was added thereto as a porous support, and after stirring for 16 hours, the water was removed by distillation while rotating using an evaporator to obtain a carbon dioxide solid recovery material. The solid recovered material was crushed and characterized by X-ray diffraction, and the results showed that it contained hematite, sodium ferrite and amorphous carbon. In addition, fluorescent X-rays showed that the content of hematite and sodium ferrite was 33%. The content of porous material was 67%. The BET specific surface area of ​​the carbon dioxide solid recovered material was 700 m 2 / g. The minor axis is 4 mm, the major axis is 8 mm, and the average particle size is 6 mm. In addition, the carbon dioxide fixation and recovery performance was examined in the same manner as in the examples. As a result, no desorption of carbon dioxide was observed even when the temperature was raised to 200°C.

[0120] The production conditions of this comparative example are shown in Table 1, various properties of the obtained carbon dioxide solid recovery material are shown in Table 2, and the effects are shown in Table 3.

[0121]

[0122]

[0123] [Table 3]

[0124]

[0125] [Experimental Example 2]

[0126] Example 9

[0127] Iron oxide particles 1 (100ED manufactured by TODA KOGYO CORP., hematite, specific surface area 11 m 2 / g) 100 parts by weight, weigh the sodium raw material sodium nitrite particle powder so that Na / Fe=1.0 (molar ratio), and mix and grind it with a sample mill. The mixed and ground material is placed in a crucible and sintered at 400°C for 16 hours. Then, it is cooled to room temperature and ground with a sample mill to obtain sodium ferrite particle powder. The BET specific surface area of ​​the obtained sodium ferrite particle powder is 4.0 m 2 / g. The primary particles were quantified by scanning electron microscopy, with an average major axis diameter of 0.7μm, an average minor axis diameter of 0.4μm, an average primary particle diameter of 0.57μm, and an axial ratio of 1.6. The pH value of the powder is as high as 13.8. 5 parts by weight of powdered activated carbon were mixed with 100 parts by weight of the obtained sodium ferrite particle powder as a porous material, and a rotary granulator was used to rotate the granulator at 40rpm to obtain spherical granules with a particle size of 5mm. It was placed in a crucible and sintered at 400°C for 16 hours in a nitrogen flow. Then, it was cooled to room temperature to obtain a carbon dioxide solid recovery material. The obtained carbon dioxide solid recovery material was crushed and characterized by X-ray diffraction, which showed sodium ferrite and amorphous carbon. In addition, it was found by fluorescent X-ray that the sodium ferrite content was 95%. The porous material was 5%. The BET specific surface area of ​​the carbon dioxide solid recovery material is 54m 2 / g. The short axis is 5mm, the long axis is 5mm, and the average particle size is 5mm. The pH value of the powder is 13.

[0128] The hardness of the obtained carbon dioxide solid recovery material is 10kgf / mm 2 , and the sphericity is 1.0. These results show that when the carbon dioxide recovery material involved in Example 9 is filled into a carbon dioxide adsorption tower, etc., it is not easily damaged by gravity or friction caused by the circulation of exhaust gas, etc., and it is convenient for the circulation of exhaust gas, etc. It should be noted that the hardness of the obtained carbon dioxide recovery material is evaluated according to the following three stages.

[0129] ○: crush hardness is 10kgf / mm 2 Carbon dioxide recovery materials

[0130] △: crush hardness greater than or equal to 3kgf / mm 2 And less than 10kgf / mm 2 Carbon dioxide recovery materials

[0131] ×: Crushing hardness is less than 3kgf / mm 2 Carbon dioxide recovery materials

[0132] The Na / Fe molar ratio of sodium ferrite contained in the obtained carbon dioxide solid recovery material was 1.0, which was approximately the same as the feed ratio of the raw material.

[0133] In order to study the carbon dioxide fixation and recovery performance of the obtained carbon dioxide solid recovery material, 1.00 weight parts of the sample was placed on a No. 2 combustion boat (12×60×9mm), and 500mL / min of model combustion exhaust gas was introduced for 2 hours. Usually, the exhaust gas when burning fuel in the atmosphere is composed of a maximum of 80vol% nitrogen and 20vol% carbon dioxide with a relative humidity of RH80-100%. Therefore, at room temperature 25°C, 400mL / min of nitrogen and 100mL / min of carbon dioxide were mixed, and the mixed gas was introduced into water to prepare a model exhaust gas with 20vol% carbon dioxide and a relative humidity of RH80%.

[0134] Weigh 10 mg of the ventilated sample, use a thermogravimetric device (TG) to pass dry air at 300 mL / min and raise the temperature to 200°C at 10°C / min to measure the desorption temperature and desorption amount of carbon dioxide adsorbed on the sample. The horizontal axis is the sample temperature measurement diagram as shown in Figure 2 As shown. The TG curve is the weight % of the remaining sample at each temperature when the initial weight is 100%, and the sample loss is attributed to the release of carbon dioxide. The DTG curve is a differential curve of the TG curve, and the temperature at the maximum value of the DTG curve is regarded as the desorption temperature of carbon dioxide. The DTA curve appears as a downward convex curve, and it can be seen that the endothermic reaction occurs near 114°C. It is quantified by considering it as the thermal decomposition of NaHCO3, and the result shows that the desorption temperature of carbon dioxide is 114°C, and the desorption amount of carbon dioxide is 17 weight % relative to the solid content of the sample, which shows that it has excellent carbon dioxide fixation and recovery performance.

[0135] Furthermore, a new sample was prepared after ventilation, and the weight was measured, which was 1.27 parts by weight, confirming a 27% increase in mass. X-ray diffraction analysis of the sample surface confirmed that 79% by weight of Na 1-x FeO2 and 21 wt% NaHCO3, it can be seen that carbon dioxide is fixed on the sodium ferrite component. Furthermore, the sample was heated at 120°C in an electric furnace for 1 hour and the weight was measured. The result was 1.10 parts by weight. It can be seen that 0.17 parts by weight (17 wt% relative to the solid carbon dioxide recovery material) of carbon dioxide can be adsorbed / desorbed in this cycle. X-ray diffraction of the sample surface was measured, and the result confirmed that 90 wt% of Na 1-xFeO2 and 10 wt% Na2CO3. Furthermore, as described above, when carbon dioxide is contacted with the sample, the amount is increased to 1.27 parts by weight, and when heated, the amount is reduced to 1.10 parts by weight, and 0.17 parts by weight (17 wt% relative to the carbon dioxide solid recovery material) of carbon dioxide can be adsorbed / desorbed. This operation was repeated 10 times, and it was confirmed that there was no change in the increase or decrease in mass. This shows that the carbon dioxide solid recovery material involved in Example 9 has excellent carbon dioxide fixation and recovery performance, especially excellent repeatability.

[0136] Embodiments 10 to 16

[0137] Solid recovered materials according to Examples 10 to 16 were obtained in the same manner as in Example 9 except that the types and amounts of the iron raw material and the support were variously changed.

[0138] The manufacturing conditions of these embodiments are recorded in Table 4, the characteristic properties of the obtained carbon dioxide solid recovery materials are recorded in Table 5, and the effects are recorded in Table 6.

[0139] Comparative Example 2

[0140] 100 parts by weight of the sodium ferrite particle powder obtained in Example 9 was granulated with a rotary granulator at 40 rpm while adding a small amount of 1% carboxymethyl cellulose aqueous solution, placed in a crucible, and subjected to solid phase reaction at 400°C in a nitrogen stream for 16 hours. Then, it was cooled to room temperature to obtain a carbon dioxide solid recovery material. The obtained carbon dioxide solid recovery material was crushed and characterized by X-ray diffraction, and the result was sodium ferrite. In addition, fluorescent X-rays showed that the content of sodium ferrite was 100%. The BET specific surface area of ​​the carbon dioxide solid recovery material was 4m 2 / g. The short axis is 4mm, the long axis is 9mm, and the average particle size is 6.5mm. The pH value of the powder is 10.

[0141] The hardness of the obtained carbon dioxide solid recovery material is 1kgf / mm 2 , judged as ×. In addition, the sphericity is 2.3, judged as ×. These results show that when the carbon dioxide recovery material is filled into the carbon dioxide adsorption tower, etc., it is easy to be damaged by gravity or friction caused by the circulation of exhaust gas, etc., and the shape is irregular, making it difficult to fill.

[0142] The production conditions of this comparative example are recorded in Table 4, the various properties of the obtained carbon dioxide solid recovery material are recorded in Table 5, and the effects are recorded in Table 6.

[0143]

[0144]

[0145] [Table 6]

[0146]

[0147] As described above, it can be seen that the carbon dioxide solid recovery material of the present invention has excellent carbon dioxide adsorption and recovery performance. In addition, the solid recovery material has high hardness, high sphericity or low bulk density, so it can be directly filled into the carbon dioxide adsorption tower.

Claims

1. A carbon dioxide solid recovery material, wherein: The carbon dioxide solid recovery material is a carbon dioxide solid recovery material containing 1 wt% to 99 wt% of sodium ferrite and 1 wt% to 99 wt% of a porous material, with an average particle size of 1 mm to 10 mm and a specific surface area of ​​5 m 2 / g~1500m 2 / g, The axial ratio of the average major axis diameter to the average minor axis diameter of the primary particles of the sodium ferrite is 1 to 2.

2. The carbon dioxide solid recovery material according to claim 1, wherein: The carbon dioxide solid recovery material contains 1 wt% to 70 wt% of the sodium ferrite and 30 wt% to 99 wt% of the porous material, with a specific surface area of ​​100 m 2 / g~1500m 2 / g.

3. The carbon dioxide solid recovery material according to claim 2, wherein: The hardness of the carbon dioxide solid recovery material is 5kgf / mm 2 ~35kgf / mm 2 , the bulk density is 0.3g / mL~0.8g / mL.

4. The carbon dioxide solid recovery material according to claim 1, wherein: The carbon dioxide solid recovery material contains more than 70% by weight and less than or equal to 99% by weight of the sodium ferrite, contains more than or equal to 1% by weight and less than 30% by weight of the porous material, and has a specific surface area of ​​5m 2 / g~500m 2 / g.

5. The carbon dioxide solid recovery material according to claim 4, wherein: The hardness of the carbon dioxide solid recovery material is 3kgf / mm 2 ~30kgf / mm 2 , the sphericity is 1 to 2.

6. The carbon dioxide solid recovery material according to any one of claims 1 to 5, wherein: The powder pH value of the carbon dioxide solid recovery material is 8-14.

7. The carbon dioxide solid recovery material according to any one of claims 1 to 5, wherein: The Na / Fe molar ratio of the sodium ferrite is 0.7 to 1.

3.

8. The carbon dioxide solid recovery material according to any one of claims 1 to 5, wherein: The porous material is a porous material selected from activated carbon, aluminosilicate, hydrotalcite, porous clay minerals, porous silica and activated alumina.

9. The method for producing a carbon dioxide solid recovery material according to any one of claims 1 to 8, wherein: The method for producing a carbon dioxide solid recovery material comprises the step of subjecting a material containing iron oxide to a solid phase reaction with an alkaline compound containing sodium.