Self-assembled monolayer modified tin diselenide sensing material and its preparation method and application

By using self-assembled single-layer film technology on the surface of tin diselenide to enhance its adsorption capacity for nitrogen dioxide, it solves the problem of low responsiveness and sensitivity of existing tin diselenide gas-sensitive materials and achieves high-efficiency nitrogen dioxide at room temperature. Nitrogen oxide detection.

CN116237020BActive Publication Date: 2024-10-22CHONGQING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310065679.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-13
Publication Date
2024-10-22
Estimated Expiration
2043-01-13

AI Technical Summary

Technical Problem

The existing tin diselenide gas-sensing materials have complex preparation methods and low responsivity and sensitivity, making it difficult to efficiently detect nitrogen dioxide at room temperature.

Method used

Using self-assembled monolayer film technology, 3-aminopropyltriethoxysilane is combined with the surface of tin diselenide to form an organic monolayer film, which enhances its adsorption capacity and responsiveness to nitrogen dioxide.

Benefits of technology

The sensitivity and specificity of the sensing material are significantly improved at room temperature and are suitable for the detection and adsorption of nitrogen dioxide. The resistance change can be used to determine the concentration of nitrogen dioxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116237020B_ABST
    Figure CN116237020B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of gas sensing materials technology, specifically relating to a self-assembled monolayer modified tin diselenide sensing material, its preparation method, and its application. The sensing material modifies the tin diselenide surface with an organic monolayer film formed by the self-assembly of 3-aminopropyltriethoxysilane. The 3-aminopropyltriethoxysilane significantly enhances the sensing material's adsorption capacity for nitrogen dioxide, giving it high sensitivity, specificity, and stability at room temperature, making it highly suitable for the detection and adsorption of nitrogen dioxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of gas sensing materials, and more specifically, relates to a self-assembled monolayer film modified tin diselenide sensing material and a preparation method and application thereof. Background Art

[0002] With the rapid growth of the number of motor vehicles in my country, a large amount of exhaust gas is discharged into the atmosphere. Since nitrogen dioxide in exhaust gas is highly irritating, long-term inhalation by humans can cause throat discomfort, dry cough, and even delayed pulmonary edema and other injuries. Therefore, designing and developing a gas-sensitive sensing material with high specificity, high responsiveness, and high sensitivity for nitrogen dioxide detection is of great value to protecting the green environment and human health.

[0003] Layered metal disulfide is a new type of two-dimensional material. It is often used for room temperature gas detection due to its advantages such as large specific surface area, high carrier concentration, and abundant gas adsorption sites. As a representative of them, tin diselenide has a large adsorption energy for nitrogen dioxide according to first-principles calculations, indicating that it has specific recognition ability for nitrogen dioxide. The responsiveness of gas sensors based on tin diselenide is usually low, and some methods and strategies need to be adopted to improve its gas-sensitive response ability. For example, Chinese patent application CN109521063A discloses a petal-shaped SnSe 2 A nitrogen dioxide gas sensor is provided, which includes a gas-sensitive material and a heating substrate. Petal-shaped tin diselenide nano-gas-sensitive material is coated on the surface of the heating substrate. Although the sensitivity of tin diselenide is improved to a certain extent, the petal-shaped tin diselenide requires a special and complicated preparation process, and the detection needs to be carried out at a high temperature of 90 to 150°C, which consumes a lot of energy and is inconvenient to use.

[0004] Therefore, there is an urgent need to provide a tin diselenide gas-sensitive sensing material with high nitrogen dioxide response, good sensitivity and easy use. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the existing tin diselenide gas-sensitive material, such as the complex preparation method, low material responsiveness and sensitivity, and to provide a self-assembled monolayer film modified tin diselenide sensing material with high nitrogen dioxide responsiveness, good sensitivity and easy use.

[0006] The purpose of the invention is to provide a method for preparing the self-assembled monolayer film modified tin diselenide sensing material.

[0007] Another object of the present invention is to provide application of the self-assembled monolayer film modified tin diselenide sensing material.

[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0009] Self-assembled monolayer technology is an ordered molecular film that is spontaneously formed on a specific substrate material by chemical adsorption and self-organization of long-chain organic molecules. This technology has the characteristics of simple operation and high film stability. And according to the difference in the tail functional groups of the assembled organic molecules, the adsorption capacity of different gas molecules can be changed, thereby enhancing the selectivity and responsiveness of the substrate gas sensor.

[0010] Therefore, the present invention provides a self-assembled monolayer film modified tin diselenide sensing material. On the surface of tin diselenide, 3-aminopropyltriethoxysilane is used to self-assemble to form an organic monolayer film to modify the tin diselenide.

[0011] The tin diselenide is a semiconductor material. The tin diselenide is modified by self-assembling an organic monolayer film formed by 3-aminopropyltriethoxysilane on the surface of the tin diselenide. The resistance of the self-assembled monolayer modified tin diselenide sensing material is stable at more than 53,000Ω in the air. When it comes into contact with nitrogen dioxide molecules, nitrogen dioxide will capture the free electrons in the self-assembled monolayer modified tin diselenide sensing material. Since tin diselenide exhibits N-type semiconductor properties, the loss of electrons will cause the conductivity of the gas-sensitive sensing material to decrease and the resistance to increase. By measuring the relationship between the resistance change and the nitrogen dioxide concentration, the concentration of nitrogen dioxide in the environment can be obtained.

[0012] In addition, the present invention also provides a method for preparing the self-assembled monolayer modified tin diselenide sensing material, which specifically comprises the following steps:

[0013] The tin diselenide is evenly dispersed in an ethanol solution, 3-aminopropyltriethoxysilane is added, the mixture is fully contacted and reacted completely, and then post-processed to obtain the product.

[0014] Furthermore, the uniform dispersion method is ultrasound. Preferably, the power of the ultrasound is 100 to 200 W, and the ultrasound time is 20 to 40 minutes.

[0015] Furthermore, the mass volume ratio of the tin diselenide to 3-aminopropyltriethoxysilane is (50-200) mg / mL.

[0016] Furthermore, the ethanol volume fraction of the ethanol solution is 80-95%.

[0017] Furthermore, after the tin diselenide is placed in an ethanol solution, the mass concentration of the tin diselenide is (1-5) mg / mL.

[0018] Furthermore, the sufficient contact is carried out by stirring, which can be magnetic stirring, and the stirring rate is (300-500) rpm.

[0019] Furthermore, the time required for the sufficient contact reaction to be complete is 1 to 12 hours.

[0020] Furthermore, the preparation method of tin diselenide comprises the following steps:

[0021] Dissolve tin salt and selenium salt in water, add hydrazine hydrate, mix thoroughly to complete the reaction, complete the hydrothermal reaction at 160-180°C, and perform post-treatment to obtain the product. This method utilizes the reducing property of hydrazine hydrate to reduce tin salt and selenium salt to simple substances, and the two simple substances combine under hydrothermal conditions to generate tin diselenide.

[0022] Furthermore, the tin salt is selected from one or more of stannous chloride, stannous sulfate, and tin methane sulfonate.

[0023] Furthermore, the selenium salt is selected from one or more of selenium dioxide, selenium powder and selenium chloride.

[0024] Furthermore, the mass volume ratio of the tin salt, selenium salt and water is (0.4-0.5):(0.4-0.5):(20-40) g / mL.

[0025] Furthermore, the volume mass ratio of the hydrazine hydrate to the tin salt is 1:(200-300) mL / mg.

[0026] Furthermore, the fully mixed reaction is carried out in combination with magnetic stirring, with a stirring rate of (300-500) rpm and a time of 20-40 minutes.

[0027] Furthermore, the hydrothermal reaction time is 20 to 24 hours.

[0028] Furthermore, the post-treatment is specifically as follows: after washing three times with water and anhydrous ethanol alternately, the reactant is dried at 60 to 80° C. for 10 to 14 hours.

[0029] The 3-aminopropyltriethoxysilane in the present invention can adjust the energy band structure of the gas sensing material and regulate the active site of tin diselenide. In addition, the amino group at the tail end of the 3-aminopropyltriethoxysilane has a unique adsorption characteristic for nitrogen dioxide, which greatly improves the adsorption capacity of the sensing material for nitrogen dioxide. It has high sensitivity, specificity and stability at room temperature and is very suitable for application in the detection and adsorption of nitrogen dioxide.

[0030] Therefore, the present invention also claims to protect the application of the self-assembled monolayer modified tin diselenide sensing material in the detection of nitrogen dioxide.

[0031] The application of the self-assembled monolayer modified tin diselenide sensing material in nitrogen dioxide adsorption is further protected.

[0032] The present invention has the following beneficial effects:

[0033] The present invention provides a self-assembled monolayer film modified tin diselenide sensing material, wherein 3-aminopropyltriethoxysilane is used to self-assemble on the surface of tin diselenide to form an organic monolayer film to modify the tin diselenide. The 3-aminopropyltriethoxysilane can greatly improve the adsorption capacity of the sensing material for nitrogen dioxide, so that the sensing material has high sensitivity, specificity and stability at room temperature, and is very suitable for the detection and adsorption of nitrogen dioxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a scanning electron microscope (STEM-EDS) image of the tin diselenide gas sensitive sensor material modified with 3-aminopropyltriethoxysilane in Example 1 of the present invention.

[0035] Figure 2 This is a TEM high-resolution contrast fringe image of the tin diselenide gas-sensitive sensor material modified with 3-aminopropyltriethoxysilane in Example 1 of the present invention.

[0036] Figure 3 This is an X-ray photoelectron spectroscopy analysis (XPS) graph of the tin diselenide gas sensitive sensor material modified with 3-aminopropyltriethoxysilane on Sn 3d, Se 3d, N 1s and Si 2p in Example 1 of the present invention.

[0037] Figure 4 This is a dynamic response recovery curve of the tin diselenide gas-sensitive sensor material modified with 3-aminopropyltriethoxysilane in Example 1 of the present invention to 500 ppb nitrogen dioxide.

[0038] Figure 5 The dynamic response recovery curve, linear relationship and long-term stability result statistical diagram of the 3-aminopropyltriethoxysilane modified tin diselenide gas sensitive sensor material to different concentrations of nitrogen dioxide gas in Example 1 of the present invention.

[0039] Figure 6 This is a statistical diagram of the sensitivity data of the tin diselenide gas-sensitive sensor material modified with 3-aminopropyltriethoxysilane in Example 1 of the present invention to different gases at 5 ppm.

[0040] Figure 7 This is a statistical chart of the resistance value measurement results of the tin diselenide gas sensitive sensor material modified with 3-aminopropyltriethoxysilane in Example 1 of the present invention. DETAILED DESCRIPTION

[0041] The present invention is further described below in conjunction with the accompanying drawings and specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0042] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0043] Example 1 Preparation of a self-assembled monolayer modified tin diselenide gas-sensitive sensor material

[0044] 1. The preparation of the self-assembled monolayer modified tin diselenide gas-sensitive sensor material specifically comprises the following steps:

[0045] S1. Preparation of tin diselenide nanosheets: 451 mg of stannous chloride dihydrate and 443 mg of selenium dioxide were dissolved in 30 mL of deionized water, 2 mL of hydrazine hydrate was added dropwise to the solution, and magnetic stirring was performed at 400 rpm for 30 minutes to complete the reaction; the obtained reaction solution was transferred into a stainless steel autoclave with a polytetrafluoroethylene liner, and hydrothermally reacted at 180° C. for 24 hours; the reactant was washed several times and dried at 60° C. for 12 hours to obtain tin diselenide nanosheets;

[0046] S2. The tin diselenide nanosheets obtained in step S1 are ultrasonically treated at 150 W for 30 minutes in 20 mL of ethanol / water (volume ratio 95:5) solution to obtain a uniform dispersion; 0.5 mL of 3-aminopropyltriethoxysilane is added to the dispersion and magnetically stirred at 400 rpm for 3 hours to complete the reaction; after multiple washings, the reactant is dried at 60° C. for 12 hours to obtain a tin diselenide gas-sensitive sensing material modified with 3-aminopropyltriethoxysilane.

[0047] 2. Determination of physical and chemical properties

[0048] (1) The STEM-EDS image of the 3-aminopropyltriethoxysilane-modified tin diselenide gas-sensitive sensor material obtained in this example was measured. The results are shown in Figure 1 As can be seen from the figure, the tin diselenide gas-sensitive sensing material modified by 3-aminopropyltriethoxysilane presents an obvious two-dimensional layer structure, and Sn, Se, O, and Si are evenly distributed in the material.

[0049] (2) The TEM high-resolution contrast fringe pattern of the 3-aminopropyltriethoxysilane-modified tin diselenide gas-sensitive sensor material obtained in this example was measured. The results are shown in Figure 2 The measurements can determine the material's interplanar spacing, further proving the existence of tin diselenide.

[0050] (3) The XPS graphs of Sn3d, Se 3d, N 1s and Si 2p of the 3-aminopropyltriethoxysilane modified tin diselenide gas sensitive sensor material obtained in this example were measured. The results are shown in Figure 3 As can be seen from the figure, tin diselenide exists and 3-aminopropyltriethoxysilane molecules are assembled on the surface.

[0051] (4) The dynamic response recovery curve of the 3-aminopropyltriethoxysilane-modified tin diselenide gas-sensitive sensor material obtained in this example to nitrogen dioxide gas with a concentration of 500 ppb at 25° C. was measured by the dynamic gas distribution method. The results are shown in Figure 4 As can be seen from the figure, the material has a good response characteristic to nitrogen dioxide, and the nitrogen dioxide resistance response rate, that is, the sensitivity, reaches 318%.

[0052] (5) The dynamic response recovery curve and linear relationship of the 3-aminopropyltriethoxysilane modified tin diselenide gas sensitive sensor material obtained in this example to different concentrations of nitrogen dioxide gas (100 ppb, 200 ppb, 300 ppb, 400 ppb, 500 ppb) at 25°C were measured by dynamic gas distribution method. The results are shown in Figure 5 As can be seen from the figure, the material shows a step-wise response to different concentrations of nitrogen dioxide. As the concentration of nitrogen dioxide increases, the sensitivity of the response change increases accordingly. The linear fitting R 2 =0.997; The response of the 3-aminopropyltriethoxysilane-modified tin diselenide gas-sensitive sensor material to 100, 300, and 500 ppb nitrogen dioxide was measured every five days for a total of 30 days to observe the stability of the material. The results are shown in Figure 5 ,It can be seen from the figure that the sensing material exhibits ,stable response values ​​to various concentrations of gases within 30 days.

[0053] (6) The sensitivity of the 3-aminopropyltriethoxysilane-modified tin diselenide gas-sensitive sensor material obtained in this example to different gases was measured (the resistance values ​​Rg and Ra of the sensor device in the target gas and air were tested respectively, and the sensitivity was calculated by the following formula S = (Rg-Ra) / Ra). The results are shown in Figure 6 As can be seen from the figure, the tin diselenide gas-sensitive sensing material modified with 3-aminopropyltriethoxysilane has a high selectivity for nitrogen dioxide.

[0054] (7) The resistance value of the 3-aminopropyltriethoxysilane-modified tin diselenide gas-sensitive sensor material obtained in this example was measured. The results are shown in Figure 7 As can be seen from the figure, the 3-aminopropyltriethoxysilane-modified tin diselenide gas-sensitive sensor material obtained in this example has a resistance value of more than 53000Ω in the air.

[0055] The morphological features of the following embodiments are similar to those of Embodiment 1 and are not repeated here.

[0056] Example 2 Preparation of a self-assembled monolayer modified tin diselenide gas sensitive sensor material

[0057] The preparation of the self-assembled monolayer modified tin diselenide gas-sensitive sensing material specifically comprises the following steps:

[0058] S1. Preparation of tin diselenide nanosheets: 451 mg of stannous chloride dihydrate and 443 mg of selenium dioxide were dissolved in 30 mL of deionized water, 2 mL of hydrazine hydrate was added dropwise to the solution, and magnetic stirring was performed at 400 rpm for 30 minutes to complete the reaction; the obtained reaction solution was transferred into a stainless steel autoclave with a polytetrafluoroethylene liner, and hydrothermally reacted at 180° C. for 24 hours; the reactant was washed several times and dried at 60° C. for 12 hours to obtain tin diselenide nanosheets;

[0059] S2. Preparation of gas-sensitive sensing material: The tin diselenide nanosheets obtained in step S1 were ultrasonically treated at 150 W for 30 minutes in 20 mL of ethanol / water (volume ratio 95:5) solution to obtain a uniform dispersion; 0.5 mL of 3-aminopropyltriethoxysilane was added to the dispersion and magnetically stirred at 400 rpm for 1 hour to complete the reaction; after multiple washings, the reactants were dried at 60° C. for 12 hours to obtain 3-aminopropyltriethoxysilane-modified tin diselenide gas-sensitive sensing material.

[0060] It was determined that the 3-aminopropyltriethoxysilane modified tin diselenide gas-sensitive sensor material obtained in this example had good response characteristics to nitrogen dioxide gas with a concentration of 500 ppb at 25° C., and the nitrogen dioxide resistance response rate, that is, the sensitivity, was 253%.

[0061] Example 3 Preparation of a self-assembled monolayer modified tin diselenide gas sensitive sensor material

[0062] The preparation of the self-assembled monolayer modified tin diselenide gas-sensitive sensing material specifically comprises the following steps:

[0063] S1. Preparation of tin diselenide nanosheets: 451 mg of stannous chloride dihydrate and 443 mg of selenium dioxide were dissolved in 30 mL of deionized water, 2 mL of hydrazine hydrate was added dropwise to the solution, and magnetic stirring was performed at 400 rpm for 30 minutes to complete the reaction; the obtained reaction solution was transferred into a stainless steel autoclave with a polytetrafluoroethylene liner, and hydrothermally reacted at 180° C. for 24 hours; the reactant was washed several times and dried at 60° C. for 12 hours to obtain tin diselenide nanosheets;

[0064] S2. Preparation of gas-sensitive sensing material: The tin diselenide nanosheets obtained in step S1 were ultrasonically treated at 150 W for 30 minutes in 20 mL of ethanol / water (volume ratio 95:5) solution to obtain a uniform dispersion; 0.5 mL of 3-aminopropyltriethoxysilane was added to the dispersion and magnetically stirred at 400 rpm for 6 hours to complete the reaction; after multiple washings, the reactants were dried at 60° C. for 12 hours to obtain 3-aminopropyltriethoxysilane-modified tin diselenide gas-sensitive sensing material.

[0065] It was determined that the 3-aminopropyltriethoxysilane-modified tin diselenide gas-sensitive sensor material obtained in this example had good response characteristics to nitrogen dioxide gas with a concentration of 500 ppb at 25° C., and the nitrogen dioxide resistance response rate, that is, the sensitivity, was 228%.

[0066] Example 4 Preparation of a self-assembled monolayer modified tin diselenide gas-sensitive sensor material

[0067] The preparation of the self-assembled monolayer modified tin diselenide gas-sensitive sensing material specifically comprises the following steps:

[0068] S1. Preparation of tin diselenide nanosheets: 451 mg of stannous chloride dihydrate and 443 mg of selenium dioxide were dissolved in 30 mL of deionized water, 2 mL of hydrazine hydrate was added dropwise to the solution, and magnetic stirring was performed at 400 rpm for 30 minutes to complete the reaction; the obtained reaction solution was transferred into a stainless steel autoclave with a polytetrafluoroethylene liner, and hydrothermally reacted at 180° C. for 24 hours; the reactant was washed several times and dried at 60° C. for 12 hours to obtain tin diselenide nanosheets;

[0069] S2. Preparation of gas-sensitive sensing material: The tin diselenide nanosheets obtained in step S1 were ultrasonically treated at 150 W for 30 minutes in 20 mL of ethanol / water (volume ratio 95:5) solution to obtain a uniform dispersion; 0.5 mL of 3-aminopropyltriethoxysilane was added to the dispersion and magnetically stirred at 400 rpm for 12 hours to complete the reaction; after multiple washings, the reactant was dried at 60° C. for 12 hours to obtain 3-aminopropyltriethoxysilane-modified tin diselenide gas-sensitive sensing material.

[0070] It was determined that the 3-aminopropyltriethoxysilane-modified tin diselenide gas-sensitive sensor material obtained in this example had good response characteristics to nitrogen dioxide gas with a concentration of 500 ppb at 25° C., and the nitrogen dioxide resistance response rate, that is, the sensitivity, was 186%.

[0071] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A self-assembled monolayer modified tin diselenide sensing material, characterized in that: On the surface of tin diselenide, 3-aminopropyltriethoxysilane was used to self-assemble to form an organic monolayer film to modify tin diselenide; The preparation method of the self-assembled monolayer modified tin diselenide sensing material specifically comprises the following steps: The tin diselenide is uniformly dispersed in an ethanol solution, 3-aminopropyltriethoxysilane is added, the reaction is fully contacted and completed, and post-treatment is performed to obtain the product; The mass volume ratio of the tin diselenide to 3-aminopropyltriethoxysilane is 50-200 mg / mL.

2. The self-assembled monolayer modified tin diselenide sensing material according to claim 1, characterized in that: The uniform dispersion method is ultrasound.

3. The self-assembled monolayer modified tin diselenide sensing material according to claim 2, characterized in that: The ethanol volume fraction of the ethanol solution is 80-95%.

4. The self-assembled monolayer modified tin diselenide sensing material according to claim 1, characterized in that: The preparation method of tin diselenide comprises the following steps: Dissolve the tin salt and selenium source in water, add hydrazine hydrate, mix thoroughly to complete the reaction, perform hydrothermal reaction at 160-200°C to complete the reaction, and perform post-treatment to obtain the product.

5. The self-assembled monolayer modified tin diselenide sensing material according to claim 4, characterized in that: The tin salt is selected from one or more of stannous chloride, stannous sulfate and tin methane sulfonate.

6. The self-assembled monolayer modified tin diselenide sensing material according to claim 4, characterized in that: The selenium source is selected from one or more of selenium dioxide, selenium powder and selenium chloride.

7. Use of the self-assembled monolayer modified tin diselenide sensing material according to claim 1 in the detection of nitrogen dioxide.

8. Use of the self-assembled monolayer modified tin diselenide sensing material according to claim 1 in nitrogen dioxide adsorption.