A method for fixing flash welding and joint heat treatment of 75kg / m hypereutectoid rails for heavy-duty railways

By using GAAS80/580 fixed flash welding machine and dual-frequency normalizing heating treatment technology in eutectoid rails used in heavy-haul railways, the problem of poor welding performance is solved, a typical pearlite structure is formed, and the tensile strength of the joint is improved. and impact performance, ensuring the smoothness and safety of the line.

CN116237624BActive Publication Date: 2024-10-29BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310090822.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-09
Publication Date
2024-10-29
Estimated Expiration
2043-02-09

AI Technical Summary

Technical Problem

The welding performance of hypereutectoid rails used in heavy-haul railways is poor, resulting in overheated zone defects, abnormal microstructure and increased brittleness in the joints, affecting the smoothness and safety of the line.

Method used

GAAS80/580 fixed flash welding machine is used for welding to control the weld seam amount, camber amount and preheating current, combined with dual-frequency normalizing heating treatment and air jet cooling technology to ensure uniform cooling of the joint temperature and avoid carbon and alloy burning Damage, forming a typical pearlite structure.

Benefits of technology

The tensile strength, impact performance and toughness of the joint are improved to match the performance of the base material and meet the service requirements of heavy-haul railways and line operation safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116237624B_ABST
    Figure CN116237624B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for fixing flash welding and heat treatment of joints of 75kg / m hypereutectoid rails for heavy-duty railways, including a joint fixing flash welding process and a joint heat treatment process. After using the flash welding joint process and the joint heat treatment process of the present invention, it can be ensured that the hypereutectoid rail fixing flash welding joints are all normal pearlite structures, and there are no abnormal structures such as bainite, martensite and secondary cementite; the present invention solves the problems of low hardness of high-strength and high-hardness hypereutectoid rail joints, poor joint drop hammer performance and low joint collapse, and can effectively improve the performance matching between the rail joint and the parent material, improve the comprehensive mechanical properties and contact fatigue performance of the joint, thereby effectively improving the service performance of the joint.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rail welding, and in particular to a method for fixing flash welding and heat treatment of joints of a 75kg / m hypereutectoid rail for heavy-duty railways. Background Art

[0002] Flash welding is one of the important ways to connect rails and is widely used in the production of 500-meter-long rails. The welding performance of steel is mainly affected by the chemical composition of steel. The research and development of pearlite rails in my country are all "high carbon, low silicon, and medium manganese". As the main elements, and according to the different strength and hardness requirements, alloy strengthening elements such as chromium and vanadium are added. Due to the high strength and high hardness of the hypereutectoid pearlite rails used in heavy-duty railways, the carbon content of the rails can reach about 1%, and its alloy content is also high, making its welding performance very poor, mainly manifested as: ① There are many defects in the welding overheating zone. There is segregation of carbon and manganese components along the austenite grain boundary in the overheating zone of flash welding, resulting in abnormal microstructures such as bainite or martensite in the joint under the supercooled state, and secondary cementite is prone to appear near the heat-affected zone, resulting in increased brittleness of the joint. ② Due to the cyclic heating of the welding heat-affected zone, the grain size increases significantly, and the non-equilibrium process of rapid heating and cooling of the joint leads to a decrease in the toughness of the flash welded joint. The impact of the joint is only about 50% of the parent material, and there is a risk of rail breakage at the joint when the rail line is in service. ③ Due to the burning of carbon and alloys during the welding process, the mechanical properties of the joint are significantly reduced, especially the hardness of the joint is significantly reduced, and the performance of the joint and the parent material are poorly matched. During the service of the line, saddle wear and peeling of the joint will occur, which seriously affects the smoothness of the seamless line. The poor welding performance of hypereutectoid rails seriously restricts the large-scale application of rails in seamless and heavy-load lines.

[0003] Rail flash welding process and joint heat treatment process directly affect the joint microstructure performance and service status. Improper flash welding process will cause defects such as overburning, unwelded, excessive gray spots, and liquefaction cracks in the joint. The metallographic grain size of the welded joint is relatively coarse, only about 1-2 levels, and the joint performance is very poor. The welded joint is subjected to normalizing heat treatment, and the weld microstructure is significantly refined, and the grain size is increased from level 1 to more than level 8, which greatly improves the toughness of the flash welded joint. However, improper weld heat treatment process, such as high or low heating temperature, fast or slow heating speed, long or short high temperature residence time, uneven temperature distribution, and continuous cooling under air cooling conditions, is prone to coarse organization in the joint, especially in the heat-affected zone, and even easy to form harmful organizations such as martensite, causing hardening and embrittlement at the joint. During the service of the line, under the action of wheel-rail stress, the joint is very likely to break, becoming a weak link in line operation.

[0004] The flash welding and joint heat treatment method for fixing 75kg / m hypereutectoid rails for heavy-duty railways provided by the present invention can ensure that the joints are all normal pearlite structures, and there are no abnormal structures such as bainite, martensite and secondary cementite. The problems of low hardness, poor drop hammer performance and low collapse of high-strength and high-hardness hypereutectoid rail joints containing Ni, Nb and RE are solved, and an excellent joint matching the performance of the parent material is obtained, so that the joint performance meets the inspection requirements for joint mechanical properties and drop hammer in "TB / T 1632.2-2014 Rail Welding Part 2: Flash Welding".

[0005] The patent with publication number CN201810708275.9 discloses a heat treatment method for rail flash welded joints. The method is for dissimilar rail welded joints of hypereutectoid rails and eutectoid rails. After welding, the high-temperature welded joints are directly cooled in three stages. The temperature is reduced from 1000-1400°C to 650-720°C in the first cooling stage, the temperature is reduced to 350-410°C in the second cooling stage, and the temperature is reduced to 10-30°C in the third cooling stage. This patent is an invention for rail mobile flash welder welding, and the cooling medium can be a water mist mixture. According to the requirements of TB / T 1632.2 standard, the mobile flash welded joint drop hammer is required to be continuous for 15 times, and the joint cooling treatment can only use compressed air, which does not meet the standard requirements for joint heat treatment process, and the invention does not meet the requirement of 25 times continuous for fixed flash welded joints.

[0006] The patent with publication number CN202010886023.2 discloses a post-weld heat treatment method for 1300MPa low-alloy heat-treated rails. This method cools the rail welded joints with a residual temperature of 900-1100°C formed by the welded joints in three stages: natural cooling to 650-720°C in the first stage, controlled cooling to 480-550°C in the second stage, and controlled cooling to 10-30°C in the second stage. This patent is an invention for the welding of mobile flash welders for rails. The cooling medium can be a water mist mixture, and the joint hardness is tested by Vickers hardness, which does not meet the heat treatment process and performance inspection requirements of the TB / T 1632.2 standard for fixed flash welded joints. In addition, a certain proportion of abnormal point-like martensitic structures appear in the joints of this invention, which not only fails to meet the standard requirements but also seriously affects the safety of the joint line operation.

[0007] The patent with the publication number CN201510319185.7 discloses a method for post-weld heat treatment of hypereutectoid rail welded joints, which is to use a medium frequency or oxyacetylene flame to quickly heat the weld area to 900-920°C for the hypereutectoid rail flash welded joint or gas pressure welded joint, cool the joint to 430-450°C at a cooling rate of 2.2-2.8°C / s, and then cool it to room temperature in air. The full-section weld impact energy Aku of the patent is ≥9J, which meets the standard requirement of ≥6.5J, but is lower than the parent material impact performance index; the joint hardness after heat treatment reaches 105% of the parent material. The hypereutectoid rail welded joint has too high hardness, which will inevitably lead to abnormal structure in the joint, high hardness and low toughness in the joint, which seriously affects the service performance of the joint and the safety of line operation. Summary of the invention

[0008] The purpose of the present invention is to provide a method for fixing flash welding and heat treatment of 75kg / m hypereutectoid rails for heavy-duty railways. After using the flash welding joint process and the joint heat treatment process of the present invention, it can be ensured that the flash welding joints for fixing hypereutectoid rails are all normal pearlite structures, and there are no abnormal structures such as bainite, martensite and secondary cementite. The present invention solves the problems of low hardness, poor drop hammer performance and low collapse of high-strength and high-hardness hypereutectoid rail joints, and can effectively improve the performance matching between the rail joint and the parent material, improve the comprehensive mechanical properties and contact fatigue performance of the joint, thereby effectively improving the service performance of the joint.

[0009] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0010] The present invention discloses a method for fixing flash welding and heat treatment of joints of a 75kg / m hypereutectoid rail for heavy-duty railway, comprising:

[0011] 1) Grind and remove rust from the end face of the 75kg / m cross-section hypereutectoid rail produced by rolling, and remove rust and grind from the electrode clamping end;

[0012] 2) Use flash welding machine for rail welding; the welding machine oil temperature is controlled at 28-42℃, the water temperature is controlled at 18-22℃, and the grid voltage is between 416~425V;

[0013] 3) Joint fixed flash welding process: The seam of the rail weld is controlled between 10 and 12 mm, the arching is controlled between 0.35 and 0.55 mm, the flash welding preheating times are between 10 and 12 times, the secondary preheating current is controlled between 61 and 67 KA, the flash welding upsetting amount is controlled between 10 and 13 mm, the upsetting force is controlled between 580 and 690 KN, the welding time is controlled between 130 and 140 s, and the final melting speed is controlled between 2.40 and 2.60 mm / s;

[0014] 4) Air cool the high-temperature welded joint to below 200°C to ensure that each position of the joint undergoes a complete phase change. When the joint temperature is less than 300°C, the cooling can be accelerated appropriately;

[0015] 5) Joint heat treatment process: Use the joint dual-frequency normalizing machine for induction heating treatment. First, perform low-frequency induction heating of the joint: use 57-65kW low-frequency power for heating for 80-92s, and heat the joint from 0-200℃ to 830-850℃;

[0016] 6) After the joint reaches the target temperature, the joint is immediately subjected to high-frequency induction heating: the normalizing machine is adjusted to 67-75kW high-frequency power for heating for 88-100s, and the joint is heated from 810-840℃ to 890-910℃;

[0017] 7) After the joint reaches the target temperature of 890-910℃, stop heating and immediately perform air jet accelerated cooling on the joint, rail waist and rail bottom. The air jet cooling nozzle is 20-30mm away from the top of the rail, 40-50mm away from the side of the rail head, 50-60mm away from the rail waist, and 50-60mm away from the rail bottom. The air jet pressure is 0.34-0.45MPa, and the air jet time is 110-130s; the joint air jet final cooling temperature should be controlled between 450-500℃, then stop air jet cooling, and the joint is naturally cooled to room temperature.

[0018] Furthermore, the flash welder is a GAAS80 / 580 fixed flash welder.

[0019] Furthermore, in 6), high-frequency heating ensures that the temperature within the range of 0-15 mm below the tread of the rail head can be heated to the target temperature, and the total joint heating time is controlled between 160 and 190 seconds.

[0020] Furthermore, the tensile strength of the joint Rm ≥ 1175MPa, the elongation of the joint A ≥ 10.2%, the impact of the joint KU2 ≥ 19.7J, and the fatigue load cycle of the joint 2×10 6 The average hardness of the joint is H J Average hardness of base material H P The ratio satisfies: H J / H P ≥0.91, average hardness of joint soft spot H J1 Average hardness of base material H P Ratio: H J1 / H P ≥0.84, softening area W≤20mm.

[0021] Furthermore, the joint did not break after 25 hammer drops, and the weld and heat-affected zone were typical pearlite structures without the presence of harmful structures such as martensite, bainite or secondary cementite.

[0022] Compared with the prior art, the beneficial technical effects of the present invention are:

[0023] Based on the above invention, the tensile strength of the joint is Rm≥1175MPa, the elongation of the joint is A≥10.2%, the impact of the joint is KU2≥19.7J, and the fatigue load cycle of the joint is 2×10 6 The average hardness of the joint is H J Average hardness of base material H P The ratio satisfies: H J / H P ≥0.91, average hardness of joint soft spot H J1 Average hardness of base material H P Ratio: H J1 / H P ≥0.84, softening area W≤20mm, the joint was not broken after 25 hammer drops, the weld and heat affected zone are typical pearlite structures, there is no martensite, bainite or secondary cementite harmful structure, all performances meet the standard requirements.

[0024] The present invention can effectively improve the mechanical properties of the flash welded joints of 75kg / m hypereutectoid rails for heavy-duty railways, improve the strength, hardness and toughness of the hypereutectoid rail joints, and make them match the performance of the parent material. The welded joints of the present invention can meet the requirement that the joints are not broken after 25 hammer drops, and improve the risk of fracture caused by "saddle-shaped" wear or abnormal microstructure of the joints caused by excessive hardness difference between the parent material and the joint in the welding area during the service of the line. The characteristics of the flash welded joints with high strength, high hardness and high toughness of the hypereutectoid rails are fully utilized by adding Ni, Nb and RE elements, ensuring that the hypereutectoid rails and joints meet the service requirements of heavy-duty railways and the safety of line operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The test results of the longitudinal section of the joint (test line 1) of Example 1 are as follows;

[0026] Figure 2 The test results of the longitudinal section of the joint (test line 1) of Example 2;

[0027] Figure 3 The test results of the longitudinal section of the joint (test line 1) of Example 3. DETAILED DESCRIPTION

[0028] The 75kg / m hypereutectoid steel rail flash welded by the present invention has C, Si, Mn, Cr, Nb, Ni and RE as main alloy elements, and the weight percentage of the chemical composition of the steel rail is C: 0.93-1.10%, Si: 0.50-0.80%, Mn: 0.80-1.20%, Cr: 0.10-0.45%, Ni: 0.10-0.50%, Nb: 0.01-0.03%, RE: 0.0005-0.0020%, P≤0.010%, S≤0.005%, Al:≤0.004%, and the rest is Fe. The steel rail is produced by smelting, continuous casting, slow cooling of steel billets, rolling, heat treatment and the like. The size of the continuous casting billet of the rail is 280mm×380mm, the rolling section is 75kg / m, the rolling compression ratio of the rail is greater than or equal to 11:1, the final rolling temperature of the rail should not be higher than 980℃, and the final cooling temperature of the online heat treatment of the rail should not be higher than 540℃, so as to ensure the grain size, pearlite sheet spacing, tensile strength and hardness of the rail.

[0029] A method for fixing flash welding and heat treatment of joints of 75kg / m hypereutectoid rails for heavy-duty railways, comprising:

[0030] 1) Use GAAS80 / 580 fixed flash welder for rail welding. The oil temperature of the welder is controlled at about 40℃, the water temperature is controlled at about 20℃, and the grid voltage is between 416 and 425V.

[0031] 2) Select two 75kg / m cross-section rails of the same material, grind and remove rust from the end faces and the electrode clamping end. The weld seam of the rails should be controlled between 10 and 12 mm, and the arching should be controlled between 0.35 and 0.55 mm.

[0032] 3) The flash welding preheating times are between 10 and 12 times, the secondary preheating current is controlled between 61 and 67KA, the flash welding upsetting amount is controlled between 10 and 13mm, the upsetting force is controlled between 580 and 690KN, the welding time is controlled between 130 and 140s, and the final melting speed is controlled between 2.40 and 2.60mm / s.

[0033] 4) The time from flash welding top forging to embossing should be controlled within 15 seconds. The maximum embossing allowance allowed for the rail head is 2.0mm, the maximum embossing allowance allowed for the rail head jaw and rail waist is 2.0mm, and the maximum embossing allowance allowed for the rail bottom is 1.5mm.

[0034] 5) Air cool the high-temperature welded joint to below 200℃ to ensure that each position of the joint is completely phase-changed. When the joint temperature is less than 300℃, the cooling can be accelerated appropriately. After the joint is cooled, grind the joint weld bar flat, that is, grind the convex allowances at the rail head and rail bottom flat.

[0035] 6) Use a dual-frequency normalizing machine to normalize the welded joints. First, use low-frequency induction heating: use 57-65kW low-frequency power for heating for 80-92s, and heat the joints from 0-200℃ to 830-850℃.

[0036] 7) After the low-frequency induction heating of the joint reaches the target temperature, turn off the low-frequency heating and immediately perform high-frequency induction heating on the joint. The normalizing machine is adjusted to 67-75kW high-frequency power for 88-100s, and the joint is heated from 810-840℃ to 890-910℃. The total time of the joint normalizing heat treatment is controlled between 160-190s.

[0037] 8) When the joint of normalizing heat treatment reaches the target temperature of 890-910℃, stop heating and immediately perform air jet accelerated cooling treatment on the joint, rail waist and rail bottom. The air jet cooling nozzle is 20-30mm away from the top surface of the rail, 40-50mm away from the side of the rail head, 50-60mm away from the rail waist, and 50-60mm away from the rail bottom. The air jet pressure is 0.34-0.45MPa, and the air jet time is 110-130s. The final air jet cooling temperature of the joint should be controlled between 450-500℃, and then the air jet cooling is stopped, and the joint is naturally cooled to room temperature.

[0038] Process comparison during implementation:

[0039] The carbon content of 75kg / m hypereutectoid rail for heavy-duty railway can reach about 1.0%, and the alloy content of the rail is also relatively high. The fusion line and overheating zone in the fixed flash welding process are prone to segregation of elements such as C and Mn, microstructural defects and secondary cementite. Therefore, the invention is made for the welding process and joint heat treatment process parameters of the hypereutectoid rail. By repeatedly adjusting the key parameters such as preheating current, preheating times, top end amount, tail burning rate, joint normalizing heating method, normalizing temperature, and final cooling temperature, combined with comparative analysis of joint mechanical properties and drop hammer results, the flash welding process and joint heat treatment process of 75kg / m hypereutectoid rail are determined.

[0040] The main adjustment parameters of the welding process during the implementation and the corresponding joint hardness and drop hammer test results are shown in Table 1.

[0041] Table 1 Comparison results of different welding processes and performance during implementation

[0042]

[0043] As can be seen from Table 1, the performance test of the joints under different welding processes was carried out at a hammer drop height of 6.4 meters: Example 1 Rail Flash Welding Process, the number of broken rails by the hammer drop was 9, and obvious gray spots and liquefaction cracks were found in most fractures, and the number of gray spots was large, and the gray spot area of ​​some fractures exceeded the standard requirements; Example 2 Rail Flash Welding Process, the number of broken rails by the hammer drop was 4, and obvious gray spots were also found in the hammer drop fractures, and no single gray spot area and total gray spot area were found to exceed the standard; Example 3 Rail Flash Welding Process, no fracture occurred during the hammer drop, and the joint hardness also met the requirements. Increasing the number of preheating times and increasing the amount of top forging can squeeze out the oxidation products produced during weld welding, and minimize or eliminate gray spots as much as possible, but too many preheating times will lead to increased heat input during flash welding, causing serious carbon and alloy burnout in the fusion zone of the joint, further reducing the strength and hardness of the joint in the welded state.

[0044] The grain size of the fixed flash welded joint of 75kg / m hypereutectoid rail is relatively coarse in the welded state, only about 1-2 levels, and the mechanical properties of the joint are very poor. Normalizing heat treatment of the welded joint can refine the weld microstructure and effectively improve the comprehensive mechanical properties of the flash welded joint. The comparison of different joint heat treatment processes during the implementation process is shown in Table 2.

[0045] Table 2 Comparison of different heat treatment processes during implementation

[0046]

[0047]

[0048] The flash welded joints after normalizing in Example 1 to Example 3 were subjected to comparative analysis of Rockwell hardness performance of the longitudinal section of the rail head according to "TB / T 1632.2-2014 Rail Welding Part 2: Flash Welding". The comparative analysis results are shown in Table 3 to Table 5. Figure 1-Figure 3 .

[0049] Table 3 Test results of joint longitudinal section (test line 1) of Example 1

[0050]

[0051] Table 4 Test results of joint longitudinal section (test line 1) of Example 2

[0052]

[0053]

[0054] Table 5 Test results of joint longitudinal section (test line 1) of Example 3

[0055]

[0056] From Table 3-Table 5 and Figure 1-Figure 3 It can be seen that the average hardness ratio of the welded joints in Example 1 and Example 2 to the average hardness of the base material H J / H P The values ​​of the hardness of the hypereutectoid rail joints are both less than 0.90, and the width of the softening zone W is both greater than 20 mm, which does not meet the standard requirements for heat-treated joints in "TB / T1632.2-2014 Rail Welding Part 2: Flash Welding". The hardness of the hypereutectoid rail joints is too low and the width of the softening zone is too wide. During the service of the line, the welds will experience low collapse, poor wear resistance, and horseshoe saddle joints, which will affect the smoothness of the joints and the safety of train operation. The joint hardness and softening zone width of Example 3 meet the standard requirements, and the joint and the parent material achieve excellent hardness matching.

[0057] According to the sampling method of "TB / T 1632.2-2014 Rail Welding Part 1: General Technical Conditions", the flash welded joints of Example 3 were tested for joint tensile and joint impact properties. The specific results are shown in Tables 5 and 6.

[0058] Table 5 Tensile properties of flash welded joint in Example 3

[0059]

[0060] Table 6 Impact properties of flash welded joints in Example 3

[0061]

[0062] It can be seen from Tables 5 and 6 that the tensile properties and impact properties of the flash welded joint of Example 3 meet the standard requirements, and the joint has a large performance margin.

[0063] From the process comparison during the implementation process, it can be seen that the tensile strength Rm of the joint in Example 3 is ≥1175MPa, the joint extension A is ≥10.2%, the joint impact KU2 is ≥19.7J, and the average hardness H of the joint is J Average hardness of base material H P The ratio satisfies: H J / H P ≥0.91, average hardness of joint soft spot H J1 Average hardness of base material H P Ratio: H J1 / H P≥0.84, softening area W≤20mm, joint dropped hammer 25 times without breaking, all performances meet the standard requirements. The strength, hardness and toughness of the 75kg / m hypereutectoid rail fixed flash welded joint for heavy-duty railway obtained in Example 3 match the performance of the rail parent material, can meet the requirements of heavy-duty railway for the smoothness of rail joints, improve the risk of fracture caused by "saddle-shaped" wear or abnormal microstructure of the joint caused by excessive difference in hardness of the parent material in the welding area and the joint during the service of the hypereutectoid rail in the line, give full play to the characteristics of high strength, high hardness and high toughness of the flash welded joint by adding Ni, Nb and RE elements to the hypereutectoid rail, and ensure that the hypereutectoid rail and the joint meet the service requirements of heavy-duty railway and the safety of line operation.

[0064] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for fixing flash welding and heat treatment of joints of 75kg / m hypereutectoid rails for heavy-duty railways, characterized in that: include: 1) Grind and remove rust from the end face of the 75kg / m cross-section hypereutectoid rail produced by rolling, and remove rust and grind from the electrode clamping end; 2) Use flash welding machine for rail welding; the welding machine oil temperature is controlled at 28-42℃, the water temperature is controlled at 18-22℃, and the grid voltage is between 416~425V; 3) Joint fixed flash welding process: The seam of the rail weld is controlled between 10 and 12 mm, the arch is controlled between 0.35 and 0.55 mm, the flash welding preheating times are between 10 and 12 times, the secondary preheating current is controlled between 61 and 67 KA, the flash welding upsetting amount is controlled between 10 and 13 mm, the upsetting force is controlled between 580 and 690 KN, the welding time is controlled between 130 and 140 s, and the final melting speed is controlled between 2.40 and 2.60 mm / s; 4) Air cool the high-temperature welded joint to below 200°C to ensure that each position of the joint undergoes a complete phase change. When the joint temperature is less than 300°C, the cooling can be accelerated appropriately; 5) Joint heat treatment process: Use the joint dual-frequency normalizing machine for induction heating treatment. First, perform low-frequency induction heating of the joint: use 57-65kW low-frequency power for heating for 80-92s, and heat the joint from 0-200℃ to 830-850℃; 6) After the joint reaches the target temperature, the joint is immediately subjected to high-frequency induction heating: the normalizing machine is adjusted to 67-75kW high-frequency power for heating for 88-100s, and the joint is heated from 810-840℃ to 890-910℃; high-frequency heating ensures that the temperature within the range of 0-15mm below the tread of the rail head can be heated to the target temperature, and the total joint heating time is controlled between 160-190s; 7) After the joint reaches the target temperature of 890-910℃, stop heating and immediately perform air jet accelerated cooling on the joint, rail waist and rail bottom. The air jet cooling nozzle is 20-30mm away from the top surface of the rail, 40-50mm away from the side of the rail head, 50-60mm away from the rail waist and 50-60mm away from the rail bottom; the air jet pressure is 0.34-0.45MPa, and the air jet time is 110-130s; the joint air jet final cooling temperature should be controlled between 450-500℃, then stop air jet cooling, and let the joint cool naturally to room temperature; The flash welded 75kg / m hypereutectoid rail has C, Si, Mn, Cr, Nb, Ni and RE as main alloying elements. The weight percentage of the chemical composition of the rail is C: 0.93~1.10%, Si: 0.50~0.80%, Mn: 0.80~1.20%, Cr: 0.10~0.45%, Ni: 0.10~0.50%, Nb: 0.01~0.03%, RE: 0.0005~0.0020%, P≤0.010%, S≤0.005%, Al: ≤0.004%, and the rest is Fe; the size of the continuous casting billet of the rail is 280mm×380mm, the rolling section is 75kg / m, the rolling compression ratio of the rail is greater than or equal to 11:1, the final rolling temperature of the rail should not be higher than 980℃, and the final cooling temperature of the online heat treatment of the rail should not be higher than 540℃.

2. The method for fixing flash welding and heat treatment of joints of 75kg / m hypereutectoid rails for heavy-duty railways according to claim 1, characterized in that: The flash welder is a GAAS80 / 580 fixed flash welder.

3. The method for fixing flash welding and joint heat treatment of 75kg / m hypereutectoid rail for heavy-duty railway according to claim 1, characterized in that: The tensile strength of the joint is Rm ≥ 1175MPa, the elongation of the joint is A ≥ 10.2%, the impact of the joint is KU2 ≥ 19.7J, and the fatigue load cycle of the joint is 2×10 6 The average hardness of the joint is H J Average hardness of base material H P The ratio satisfies: H J / H P ≥0.91, average hardness of joint soft spot H J1 Average hardness of base material H P Ratio: H J1 / H P ≥0.84, softening area W≤20mm.

4. The method for fixing flash welding and heat treatment of joints of 75kg / m hypereutectoid rails for heavy-duty railways according to claim 1, characterized in that: The joint was not broken after 25 hammer drops, and the weld and heat-affected zone were typical pearlite structures without any harmful structures such as martensite, bainite or secondary cementite.

Citation Information

Patent Citations

  • Post-weld heat treatment method for hypereutectoid rail welded joints

    CN104862466B

  • Heat treatment method for flash welded joints of rails

    CN108504848B

  • Post-welding heat treatment method for 1,300MPa-grade low-alloy heat treatment steel rail

    CN112063826A

  • Method for eliminating 75 kg / m hypereutectoid steel rail moving flash welding joint overburning defects

    CN113414480A

  • Heat treatment process for high-strength and high-toughness bainite steel rail welded joint for heavy haul railway

    CN114507772A