A spiro compound and an organic electroluminescent device

By designing spirocyclic compounds, the luminescence efficiency and life of OLED are improved, the problem of low OLED light extraction efficiency is solved, the higher optical coupling ratio and material stability are achieved, and the overall performance of the device is improved.

CN116239478BActive Publication Date: 2024-11-12NANJING TOPTO MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310095913.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-10
Publication Date
2024-11-12
Estimated Expiration
2043-02-10

AI Technical Summary

Technical Problem

The existing organic electroluminescent devices (OLEDs) have a large gap between the external quantum efficiency and the internal quantum efficiency, resulting in low light extraction efficiency, which seriously restricts its development and application, especially the interface between ITO film and glass substrate and glass substrate. The total reflection effect caused by the interface with the air is severe, limiting the proportion of light coupled to the external space.

Method used

A class of spirocyclic compounds were designed to form fluorene compounds by introducing cycloalkane groups and bridging them with fluorenyl groups, and connecting them with biphenylamine compounds. The amine compounds were synthesized through Buchwald-Hartwig Cross Coupling Reaction to improve the space of the material Sector resistance and torque block the reverse transmission of energy, improve luminescence efficiency and life, while reducing the glass transition temperature of the material, improving the molecular arrangement and cleaning difficulty during the evaporation process.

Benefits of technology

It improves the luminous efficiency and life of OLED, reduces lateral leakage and crosstalk problems, enhances the solvent properties and production efficiency of the material, and significantly improves the performance and application prospects of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116239478B_ABST
    Figure CN116239478B_ABST
Patent Text Reader

Abstract

The invention discloses a spiro compound and an organic electroluminescent device, and relates to the technical field of organic electroluminescence. The compounds in the compounds in the present application all have cycloalkane groups such as a three-membered ring or a four-membered ring or a five-membered ring or a six-membered ring, and the cycloalkane is bridged with a fluorenyl to form a fluorene compound, and the fluorene compound is connected with a biphenylamine compound to form an amino compound, and the amino compound and the phenyl of 9,9-diphenylfluorene are synthesized by Buchwald-Hartwig Cross Coupling Reaction. The introduction of specific groups such as a three-membered ring, a four-membered ring, a five-membered ring, and a six-membered ring effectively increases the steric hindrance and torque of the material, thereby improving the triplet energy level of the material, effectively blocking the reverse transfer of energy from the light-emitting layer to the transmission layer, thereby improving the luminous efficiency and life of the device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic electroluminescence, and in particular to a spiro compound and an organic electroluminescent device. Background Art

[0002] Organic light-emitting devices (OLED) have the advantages of being thin and light, actively emitting light, having a wide viewing angle, fast response, low energy consumption, excellent low temperature and shock resistance, and potential flexible design. OLED is a fully solid-state device, without a vacuum cavity or liquid components, so it is not afraid of vibration and is easy to use. With its high resolution, wide viewing angle, and wide operating temperature range, it will be widely used in the fields of weapons and equipment and harsh environments. In addition, OLED can also be used as a flat backlight source and lighting source in the display field. Therefore, OLED has a good development prospect.

[0003] OLED does not require the backlight system used in LCD. When LCD is working, it selectively blocks certain backlight areas to allow the image to appear, while OLED relies on its own light. Because OLED does not require a backlight system, its power consumption is less than LCD (most of the power consumed by LCD is used for the backlight system). This is especially important for battery-powered devices.

[0004] OLED is a current-type organic light-emitting device. It emits light through the injection and recombination of carriers. The luminous intensity is proportional to the injected current. Under the action of the electric field, the holes generated by the anode and the electrons generated by the cathode will move, inject into the hole transport layer and the electron transport layer respectively, and migrate to the light-emitting layer. When the two meet in the light-emitting layer, energy excitons are generated, which excite the light-emitting molecules and finally produce visible light.

[0005] Since there is a huge gap between the external quantum efficiency and the internal quantum efficiency of OLED, the development of OLED is greatly restricted. Therefore, how to improve the light extraction efficiency of OLED has become a hot topic of research. Total reflection occurs at the interface between ITO film and glass substrate and at the interface between glass substrate and air. The light emitted to the front external space of OLED device accounts for about 20% of the total EL of organic material film. The remaining about 80% of the light is mainly confined in the organic material film, ITO film and glass substrate in the form of waveguide, which seriously restricts the development and application of OLED. How to reduce the total reflection effect in OLED devices and increase the proportion of light coupling to the front external space of the device, thereby improving the performance of the device, has attracted widespread attention.

[0006] In order to fully utilize the excellent characteristics of organic light-emitting devices, the materials that constitute the organic layers in the device, such as hole injection materials, hole transport materials, light-emitting materials, electron transport materials, electron injection materials, etc., must be backed by stable and effective materials, and there is a continuous demand for the development of new materials. Summary of the invention

[0007] The purpose of the present invention is to provide a spiro compound and an organic electroluminescent device in view of the above technical problems.

[0008] The purpose of the present invention can be achieved by the following measures:

[0009] A spiro compound having a structure as shown in Formula 1:

[0010]

[0011] in,

[0012] R1 and R3 are connected so that R1-C-R3 constitutes a C3-C20 cycloalkyl or a C3-C20 cycloalkenyl;

[0013] R2 is selected from the group consisting of deuterium or the following groups which may or may not be deuterated: one or more of a C1-C10 alkyl group, a C3-C10 cycloalkyl group, a C6-C20 aromatic group or a C1-C10 alkyl-substituted C6-C20 aromatic group;

[0014] n is an integer from 0 to 5.

[0015] In the present invention, R1 and R3 are alkyl or alkenyl, and the total number of carbon atoms of the two is 2-19.

[0016] Preferably, R1 and R3 are connected so that R1-C-R3 constitutes a C3-C12 cycloalkyl or a C3-C12 cycloalkenyl.

[0017] Further preferably, R1-C-R3 constitutes one of a C3-C10 cycloalkyl group, a C3-C9 cycloalkyl group, a C3-C8 cycloalkyl group, a C3-C7 cycloalkyl group or a C3-C6 cycloalkyl group.

[0018] More preferably, R1-C-R3 constitutes cyclopropane, cyclobutane, cyclopentane or cyclohexane.

[0019] Preferably, R2 is a deuterated or non-deuterated group selected from the group consisting of one or more of a C1-C4 alkyl group, a phenyl group, a biphenyl group, a naphthyl group, a phenanthryl group, an anthracenyl group, and a 9,9-dimethylfluorenyl group.

[0020] More preferably, R2 is one or more of the following groups which may be deuterated or not: methyl, ethyl, propyl, phenyl, biphenyl, naphthyl, phenanthryl, anthracenyl, 9,9-dimethylfluorenyl.

[0021] More preferably, R2 is methyl, ethyl, propyl, deuterated methyl, deuterated ethyl or deuterated propyl.

[0022] Preferably, n is an integer of 0-4, especially an integer of 0-3, such as =0, 1, 2, 3.

[0023] In a preferred embodiment, the cycloalkyl group formed by R1-C-R3 is a monocyclic alkyl group.

[0024] Further preferably, the structural formula of the compound of the present invention is shown in Formula 2-Formula 4 below:

[0025]

[0026] Furthermore, the compound of the present invention may be any one of the following compounds:

[0027]

[0028]

[0029]

[0030]

[0031]

[0032]

[0033]

[0034]

[0035]

[0036]

[0037]

[0038]

[0039]

[0040]

[0041]

[0042]

[0043]

[0044]

[0045]

[0046]

[0047]

[0048]

[0049]

[0050]

[0051]

[0052]

[0053]

[0054]

[0055]

[0056]

[0057]

[0058]

[0059] The spiro compound having the structure shown in Formula 1 of the present invention has a synthesis reaction route as follows:

[0060]

[0061] An organic electroluminescent device comprises a first electrode, a second electrode and an organic layer formed between the first electrode and the second electrode, wherein the organic layer contains the above compound.

[0062] Furthermore, the organic layer comprises a hole injection layer, a first hole transport layer, a second hole transport layer, a light-emitting layer, a hole blocking layer, an electron transport layer, and an electron injection layer; and at least one of the hole injection layer, the first hole transport layer, the second hole transport layer, the light-emitting layer, the hole blocking layer, the electron transport layer, and the electron injection layer contains the above-mentioned compound.

[0063] Furthermore, the hole transport layer contains the above-mentioned compound.

[0064] An electronic display device containing the organic electroluminescent device.

[0065] An OLED lighting device containing the organic electroluminescent device.

[0066] The room temperature described in the present invention is 25±5°C.

[0067] Beneficial effects of the present invention:

[0068] The present invention designs a new type of organic electroluminescent material. This type of material has the following characteristics:

[0069] 1. The compounds in the present invention all have a cycloalkane group (such as a three-membered ring, a four-membered ring, a five-membered ring, or a six-membered ring, etc.), the cycloalkane is bridged with a fluorene group to form a fluorene compound, the fluorene compound is connected with a biphenylamine compound to form an amino compound, and the amino compound and the phenyl group of 9,9-diphenylfluorene are synthesized by Buchwald-Hartwig Cross Coupling Reaction to synthesize the compound of the present invention. The introduction of specific groups such as three-membered rings, four-membered rings, five-membered rings, and six-membered rings effectively increases the steric hindrance and torque of the material, thereby increasing the triplet energy level of the material, effectively blocking the reverse transfer of energy from the light-emitting layer to the transmission layer, thereby improving the luminous efficiency and life of the device.

[0070] 2. The introduction of cycloalkane groups (such as three-membered rings, four-membered rings, five-membered rings, six-membered rings, etc.) on the fluorene group effectively increases the steric hindrance and torque of the material. The large steric hindrance and torque improve the orientation of the molecular arrangement of the material during vapor deposition, thereby making the film layer formed by vapor deposition have a certain anisotropy. This property effectively solves the lateral leakage and crosstalk problems of the device.

[0071] 3. The fluorene group containing a cycloalkane group (such as a three-membered ring, a four-membered ring, a five-membered ring, or a six-membered ring, etc.) is connected to the phenyl group of 9,9-diphenylfluorene through nitrogen, which greatly improves the torque and spatial rotational freedom of the material, reduces the rigidity of the material, and then reduces the glass transition temperature of the material, thereby avoiding the problem of pore blocking during the evaporation process of the material. At the same time, the large torque and spatial rotational freedom greatly improve the solubility of the material in the solvent, thereby significantly reducing the difficulty and cost of cleaning the mask, improving the utilization efficiency of the mask, and improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0072] Figure 1 It is a schematic structural diagram of an organic electroluminescent device of the present invention;

[0073] The numbers in the figure represent: 1-anode, 2-hole injection layer, 3-first hole transport layer, 4-second hole transport layer, 5-light-emitting layer, 6-hole blocking layer, 7-electron transport layer, 8-electron injection layer, 9-cathode.

[0074] Figure 2 This is the HPLC chart of compound 4 prepared in Example 1 of the present invention.

[0075] Figure 3 is the DSC spectrum of compound 4 prepared in Example 1 of the present invention, Figure 3 It can be seen that the Tg value of compound 4 is 130.00°C.

[0076] Figure 4 is the TGA spectrum of compound 4 prepared in Example 1 of the present invention, Figure 4 It can be seen that the thermal weight loss temperature Td value is 417.73℃.

[0077] Figure 5 is a life graph of the organic electroluminescent device in Application Example 1 and Comparative Example 1 of the present invention; Figure 5 It can be seen that the T97% lifespans of the organic electroluminescent devices prepared in Application Example 1 and Comparative Example 1 of the present invention are 709 h and 461 h, respectively.

[0078] Figure 6 This is the NMR chart of compound 4 prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0079] The following further illustrates and describes embodiments of various aspects. It should be understood that the description herein is not intended to limit the claims to the specific aspects described. On the contrary, it is intended to cover substitutions, modifications and equivalents that may be included in the spirit and scope of the present disclosure defined by the appended claims.

[0080] As used herein, in "deuterated" or "undeuterated", the term "deuterated" means that at least one hydrogen in the group is re-coordinated with deuterium. The term "undeuterated" means that all hydrogens in the group are not re-coordinated with deuterium.

[0081] The "aromatic group" herein refers to a group containing one or more aromatic rings, and the aromatic rings here include but are not limited to benzene, naphthalene, phenanthrene, fluorene, acenaphthene, pyridine, pyrimidine, pyrrole, furan, thiophene, etc. C6-C30 in the aromatic group of C6-C30 means that the group contains 6-30 carbon atoms. In the aromatic group of C6-C20 substituted by C1-C10 alkyl, C1-C10 refers to the number of carbon atoms of the substituent, and C6-C20 refers to the number of carbon atoms of the aromatic group without substituents. Aromatic groups can be divided into monocyclic aromatic groups and polycyclic aromatic groups. Specific aromatic groups in the present invention include but are not limited to phenyl, biphenyl, terphenyl, anthracene, naphthyl, phenanthryl, fluorenyl, dibenzofuranyl, dibenzothiophenyl, 9,9-spirobifluorenyl, 9,9-dimethylfluorenyl or 9,9-diphenylfluorenyl, etc. Aromatic groups can be substituted and unsubstituted.

[0082] "Cycloalkyl" herein refers to a monocyclic or fused ring ("fused" ring means that each ring in the system shares a pair of adjacent carbon atoms with other rings in the system) group that is all carbon, wherein one or more rings are saturated alicyclic rings, which generally have 3-20 carbon atoms, preferably 3-12 carbon atoms, and more preferably 3-10 carbon atoms. Cycloalkyl can be divided into monocyclic alkyls having only one ring and fused cyclic alkyls having multiple rings. Examples of monocyclic alkyls include, but are not limited to, cyclopropane, cyclobutane, cyclopentane, cyclohexane, cycloheptane. Cycloalkyl can be substituted and unsubstituted.

[0083] "Cycloalkenyl" herein refers to a monocyclic or fused ring ("fused" ring means that each ring in the system shares a pair of adjacent carbon atoms with other rings in the system) group that is all carbon, wherein one or more rings do not have a completely connected π electron system and contain at least one alkenyl group, which generally has 3-20 carbon atoms, preferably 3-12 carbon atoms, more preferably 3-10 carbon atoms, and the examples of cycloalkenyl groups include but are not limited to cyclopentene, cyclohexene, cyclohexadiene, cycloheptatriene. Cycloalkenyl groups may be substituted and unsubstituted.

[0084] The "deuterated aromatic group" herein refers to a group in which one or more hydrogen atoms in an aromatic group are substituted with deuterium.

[0085] The "deuterated phenyl group" herein refers to a group in which one or more hydrogen atoms in a phenyl group are replaced by deuterium.

[0086] Herein, “n is an integer of 0-5” means n is 0, 1, 2, 3, 4, 5, and “n is an integer of 0-3” means n is 0, 1, 2, 3.

[0087] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0088] Embodiment 1:

[0089]

[0090] The synthesis method of compound 4 is as follows:

[0091]

[0092] Under nitrogen protection, in a three-necked flask, 1-a (29 g, 167 mmol, 1 eq) and 1-b (25 g, 184 mmol, 1.1 eq) were dissolved in 300 mL of toluene, and Pd(Pph3)4 (3.8 g, 3.34 mmol, 2% eq) and potassium carbonate (69 g, 0.5 mol, 3 eq) were added. 80 mL of ethanol and 80 mL of water were added, and the reaction was carried out at 90 ° C. The reaction progress was monitored by HPLC.

[0093] After 24 hours of reaction, HPLC monitoring showed that 1-b was basically reacted. The reaction was stopped, the room temperature was lowered, and the filtrate was filtered through silica gel. The filtrate was washed with water, separated, and the filtrate was concentrated until there was no droplet. Petroleum ether was added and stirred at 0°C for 1 hour. Solid precipitated and was filtered with suction, rinsed with a small amount of petroleum ether, and dried at 55°C.

[0094] Under nitrogen protection, in a three-necked flask, 1-c (25.5 g, 144 mmol, 1.2 eq) and 1-d (36 g, 120 mmol, 1 eq) were dissolved in 300 mL of toluene, and Pd(dppf)Cl2 (0.9 g, 1.2 mmol, 1% eq), S-phos (1 g, 2.4 mmol, 2% eq), sodium tert-butoxide (15 g, 156 mmol, 1.3 eq) were added. The reaction was refluxed at 110 ° C and the reaction progress was monitored by HPLC.

[0095] HPLC monitoring showed that the reaction of intermediate 1-d was complete, so the reaction was stopped, the room temperature was lowered, 300 mL of water was added, the liquids were separated, the organic phase was passed through silica gel, and it was concentrated under reduced pressure until there were no droplets. Ethanol was boiled to cool, and the solid precipitated was filtered and dried.

[0096] Under nitrogen protection, in a three-necked flask, 1-e (38 g, 95 mmol, 1.02 eq) and 1-f (38 g, 95 mmol, 1 eq) were dissolved in 300 mL of toluene, and Pd2(dba)3 (0.9 g, 1.4 mmol, 1.5% eq), sodium tert-butoxide (12 g, 120 mmol, 1.5 eq), tri-tert-butylphosphine (4 mL, 2.85 mmol, 3% eq) were added and refluxed at 110 ° C. The reaction progress was monitored by HPLC.

[0097] HPLC monitoring showed that the intermediate 1-f was completely reacted. The reaction was stopped, the room temperature was lowered, 300 mL of water was added, the liquid was separated, the organic phase was passed through silica gel, and the mixture was concentrated under reduced pressure until there was no droplet. The ethanol was boiled and cooled, and the solid was filtered and recrystallized from toluene + ethanol 11 times to obtain the target product. Finally, compound 4 (17 g, yield 25%) was obtained, HPLC purity 99.92%, ESI-MS (m / z) (M+): theoretical value 717.96, measured value 717.34, elemental analysis results (molecular formula C55H43N): theoretical value C, 92.01; H, 6.04; N, 1.95; measured value C, 92.03; H, 6.06; N, 1.91.

[0098] The following product compounds were obtained in a similar manner:

[0099] Table 1

[0100]

[0101]

[0102]

[0103]

[0104]

[0105]

[0106]

[0107]

[0108]

[0109]

[0110]

[0111]

[0112]

[0113] The synthetic identification results of the compounds prepared above are shown in Table 2 below:

[0114] Table 2

[0115]

[0116]

[0117] Embodiment 63:

[0118]

[0119] The synthesis method of compound 2 is as follows:

[0120]

[0121] Under nitrogen protection, in a three-necked flask, 63-a (14.22 g, 0.084 mol, 1.03 eq) and 63-b (24.54 g, 0.082 mol, 1 eq) were dissolved in 300 mL of toluene, and Pd2(dba)3 (1.5 g, 1.64 mmol, 2% eq), tri-tert-butylphosphine (5 mL, 2.5 mmol, 3% eq), sodium tert-butoxide (12 g, 0.13 mol, 1.6 eq) were added. The mixture was refluxed at 110°C and the reaction progress was monitored by HPLC.

[0122] HPLC monitoring showed that the reaction of intermediate 63-a was complete, so the reaction was stopped, the room temperature was lowered, 300 mL of water was added, the liquids were separated, the organic phase was passed through silica gel and anhydrous magnesium sulfate, the organic phase was concentrated under reduced pressure, and the next reaction was directly carried out without purification.

[0123] Under nitrogen protection, in a three-necked flask, 63-c (30 g, 77.2 mmol, 1 eq) and 63-d (32.5 g, 81.8 mmol, 1.06 eq) were dissolved in 300 mL of toluene, and Pd2(dba)3 (1.4 g, 1.55 mmol, 2% eq), tri-tert-butylphosphine (4.7 mL, 2.32 mmol, 3% eq) and sodium tert-butoxide (12 g, 0.12 mol, 1.5 eq) were added. The mixture was refluxed at 110°C and the reaction progress was monitored by HPLC.

[0124] HPLC monitoring showed that the intermediate 63-c was completely reacted. The reaction was stopped, the room temperature was lowered, 300 mL of water was added, the mixture was filtered, the liquid was separated, the organic phase was passed through silica gel and anhydrous magnesium sulfate, the organic phase was concentrated under reduced pressure, and the mixture was purified by chromatography column. The eluent was PE / MC, gradient elution, and the product was collected. The operation was performed three times to obtain the final target product. Compound 2 (7.45 g, yield 13.7%) was finally obtained, HPLC purity 99.92%, ESI-MS (m / z) (M+): theoretical value 703.93, measured value 703.45, elemental analysis results (molecular formula C54H41N): theoretical value C, 92.14; H, 5.87; N, 1.99; theoretical value C, 92.10; H, 5.91; N, 1.99.

[0125] The following product compounds were obtained in a similar manner:

[0126] Table 3

[0127]

[0128]

[0129]

[0130]

[0131] The synthetic identification results of the compounds prepared above are shown in Table 4 below:

[0132] Table 4

[0133]

[0134] Material property test:

[0135] Test compounds of the present invention 1, 2, 3, 4, 7, 12, 13, 19, 22, 28, 31, 40, 41, 42, 43, 49, 52, 67, 72, 79, 88, 100, 102, 106, 118, 120, 121, 139, 196, 197, 198, 202, 205, 208, 209, 210, 217, 223, 224, 226, 253, 256, 2 The thermal weight loss temperature Td and glass transition temperature Tg of 62, 264, 265, 274, 277, 283, 295, 297, 301, 305, 313, 316, 322, 393, 394, 400, 412, 418, 420, 430, 433, 439, 451, 457, 469, 478, 490, 499, 511, 519, and 529. The test results are shown in Table 5.

[0136] Note: Thermogravimetric temperature Td is the temperature at which the weight loss is 5% in a nitrogen atmosphere, and is measured on a TGA N-1000 thermogravimetric analyzer with a nitrogen flow rate of 10 mL / min. The melting point Tg is measured by differential scanning calorimetry (DSC, Shinco DSC N-650) with a heating rate of 10°C / min.

[0137] Table 5:

[0138]

[0139]

[0140]

[0141]

[0142] It can be seen from the above data that the compounds synthesized in the present invention have excellent thermal stability, which means that the compounds conforming to the general structural formula of the present invention all have excellent thermal stability and can meet the requirements for the use of organic electroluminescent materials.

[0143] Device performance test:

[0144] Application Example 1:

[0145] ITO was used as the reflective layer anode substrate material, and its surface was treated with water, acetone, and N2 plasma in sequence;

[0146] On top of the ITO anode substrate, 10 nm of HT-1 doped with 2% by mass of NDP-9 was deposited to form a hole injection layer (HIL);

[0147] 100 nm of HT-1 was evaporated on the hole injection layer (HIL) to form the first hole transport layer (HTL);

[0148] Vacuum evaporation of the compound 4 designed by the present invention on the first hole transport layer (HTL) to form a second hole transport layer (GPL) with a thickness of 30 nm;

[0149] Compounds G1 and G2 were co-evaporated at a mass ratio of 5:5 as green light host materials, and GD-1 was evaporated as a doping material (the amount of GD-1 was 8% of the total mass of G1 and G2) on the second hole transport layer (GPL) to form a light-emitting layer with a thickness of 30 nm;

[0150] HB-1 was evaporated onto the light-emitting layer to obtain a hole blocking layer (HBL) with a thickness of 20 nm;

[0151] ET-1 and LiQ were co-evaporated onto the hole blocking layer (HBL) in a mass ratio of 5:5 to obtain an electron transport layer (ETL) with a thickness of 30 nm;

[0152] Magnesium (Mg) and silver (Ag) were mixed and evaporated on the electron transport layer (ETL) in a mass ratio of 9:1 to form an electron injection layer (EIL) with a thickness of 50 nm;

[0153] Thereafter, silver (Ag) is evaporated onto the electron injection layer to form a cathode with a thickness of 100 nm, and a DNTPD with a thickness of 50 nm is deposited on the cathode sealing layer. In addition, the cathode surface is sealed with a UV curable adhesive and a sealing film (seal cap) containing a dehumidifier to protect the organic electroluminescent device from being affected by oxygen or moisture in the atmosphere. Thus, an organic electroluminescent device is prepared.

[0154]

[0155] Application Example 2-80

[0156] The compounds 1, 2, 3, 7, 12, 13, 19, 22, 28, 31, 40, 41, 42, 43, 49, 52, 67, 72, 79, 88, 100, 102, 106, 118, 120, 121, 139, 196, 197, 198, 202, 205, 208, 209, 210, 217, 223, 224, 226, 253, 256, 262, 264, 266 64, 265, 274, 277, 283, 295, 297, 301, 305, 313, 316, 322, 393, 394, 400, 412, 418, 420, 430, 433, 439, 451, 457, 469, 478, 490, 499, 511, 519, 529 are used as the second hole transport material, and the other parts are consistent with those in Application Example 1, and the organic electroluminescent device of Application Example 2-80 is manufactured based on this.

[0157] Comparative Examples 1-3:

[0158] The difference from Application Example 1 is that A-40, A-50, A-53, Compound 7 and Compound 8 in CN111635323B are used respectively instead of Compound 4 in the present application as the second hole transport material, and the rest is the same as Application Example 1.

[0159] The characteristics of the organic electroluminescent device manufactured in the above application example and the organic electroluminescent device manufactured in the control example are that at a current density of 10 mA / cm 2 The results were shown in Table 6.

[0160] Table 6:

[0161]

[0162]

[0163]

[0164] As shown in Table 6 above, when the compounds of the present invention are applied to organic electroluminescent devices, at the same current density, the luminous efficiency is greatly improved, the starting voltage of the device is reduced, the power consumption of the device is relatively reduced, and the life of the device is correspondingly improved.

[0165] The organic electroluminescent devices prepared in the control examples 1-3, application examples 1-8, and application examples 63-70 were respectively subjected to luminescence life tests to obtain luminescence life T97% data (the time when the luminescence brightness decreases to 97% of the initial brightness). The test equipment was a TEO luminescent device life test system. The results are shown in Table 7:

[0166] Table 7:

[0167]

[0168]

[0169] It can be seen from Table 7 above that when the compound of the present invention is applied to an organic electroluminescent device, the service life is greatly improved at the same current density, and the compound has broad application prospects.

Claims

1. A spiro compound, characterized in that The compound is any one of the following compounds:

2. An organic electroluminescent device, characterized in that: The invention comprises a first electrode, a second electrode and an organic layer formed between the first electrode and the second electrode, wherein the organic layer contains the compound according to claim 1.

3. The organic electroluminescent device according to claim 2, characterized in that: The organic layer comprises a hole injection layer, a first hole transport layer, a second hole transport layer, a light-emitting layer, a hole blocking layer, an electron transport layer, and an electron injection layer; at least one of the hole injection layer, the first hole transport layer, the second hole transport layer, the light-emitting layer, the hole blocking layer, the electron transport layer, and the electron injection layer contains the compound according to claim 1.

4. The organic electroluminescent device according to claim 3, characterized in that: The first hole transport layer and the second hole transport layer contain the compound according to claim 1.

5. An electronic display device, characterized in that: Contains the organic electroluminescent device as claimed in claim 2.

6. An OLED lighting device, characterized in that: Contains the organic electroluminescent device as claimed in claim 2.