A continuous production process for carbon dioxide-based biodegradable polymers
By combining continuous dissolution and precipitation processes with a batch separator, the problems of cumbersome operation and high energy consumption in the production of carbon dioxide-based biodegradable polymers have been solved, achieving efficient, low-energy industrial production with high product purity.
Patent Information
- Application Number
- CN202310367966.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-12-13
- Filing Date
- 2023-04-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-04-08
AI Technical Summary
In the existing technology, the continuous production process of carbon dioxide-based biodegradable polymers lacks simple, efficient and thorough separation methods, resulting in a cumbersome production process and high energy consumption.
A continuous dissolution and precipitation process is adopted, using a dissolver and a precipitator to dissolve the adhesive and precipitate the polymer, combined with a batch separator to achieve liquid-solid separation. By adjusting the type and amount of adhesive solvent and polymer precipitant, continuous feeding and separation are achieved, reducing energy consumption.
It has enabled the efficient and continuous production of carbon dioxide-based biodegradable polymers, reducing energy consumption, improving production efficiency, and achieving a product purity of over 99.5%, making it suitable for industrial applications.
Smart Images

Figure CN116239764B_ABST
Abstract
Description
Technical Field
[0001] The invention discloses a continuous production process of a carbon dioxide-based biodegradable polymer, belonging to the technical field of degradable plastics. Background Art
[0002] Traditional plastic polymers have poor biodegradability, and as their usage increases, they have caused serious white pollution problems. As people's environmental awareness gradually increases, the use of polymer materials with poor degradation performance has been greatly restricted. Researchers have found that the use of carbon dioxide polymerization to produce polymer materials can not only alleviate the global warming problem caused by carbon dioxide, but also improve the biodegradability of polymer materials.
[0003] Polymethylethylene carbonate (PPC) can be obtained by copolymerization of carbon dioxide and alkylene oxide. It is a transparent, fully degradable and environmentally friendly plastic with excellent biocompatibility, high barrier properties and impact toughness, but has a low glass transition temperature (Tg=30-40°C), which limits its large-scale application. In order to improve the performance of PPC, a third element is usually introduced into the main chain of PPC for modification. For example, by introducing phthalic anhydride into the main chain of PPC, the obtained degradable polymer has high light transmittance, high glass transition temperature and good foaming properties. Its preparation method and post-processing process have been reported in patents. However, there are no relevant patents or literature reports on the industrial continuous production process from reaction to post-processing until a qualified finished product is obtained.
[0004] For example, patent CN 111378101A discloses a method of preparing a catalyst based on PA, propylene oxide and CO. 2 A method for synthesizing a carbon dioxide-based polyester-polycarbonate terpolymer as a raw material, a certain mass of phthalic anhydride, propylene oxide, and a catalyst are added to a high-pressure reactor, and 1.0 MPa of CO is charged 2 , react at 80°C for 12h, quench the reaction after the reaction is completed, and obtain the product by dissolving, precipitating and drying. The patent only briefly describes the purification method of the glue obtained by the reaction, and does not mention the specific operation of implementing the method.
[0005] Patent CN 114539515A discloses a biodegradable carbon dioxide-based terpolymer and its preparation method. A certain mass of propylene oxide, lactide, and catalyst are added to a reactor, and 1.0 MPa of CO is charged. 2 , react at 25°C for 36 hours, after the reaction is completed, dissolve the polymer with acetone, then wash three times with methanol solution, and dry the washed product at 35°C in vacuum for 24 hours. This method uses methanol solution to wash three times to remove the solvent and catalyst, which is cumbersome and does not mention the specific operation method. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a continuous production process for carbon dioxide-based biodegradable polymers which is simple in operation, high in efficiency and thorough in separation.
[0007] The technical solution adopted by the present invention to solve the technical problem is: the continuous production process of the carbon dioxide-based biodegradable polymer is characterized by comprising the following steps:
[0008] 1) Carbon dioxide and comonomers complete carbon dioxide-based multi-polymerization in the reactor under the action of a catalyst to obtain a polymer glue solution. The polymer glue solution obtained after each reaction is transferred to a buffer tank for temporary storage;
[0009] 2) Continuously conveying the polymer glue liquid from the buffer tank to the dissolver, and simultaneously conveying the glue liquid dissolving agent to the dissolver, so that the glue liquid is dissolved in the glue liquid dissolving agent to obtain a mixed liquid; the dissolver is continuously fed and continuously extracted;
[0010] 3) The mixed liquid continuously extracted from the dissolver is continuously transported to the precipitator, and the polymer precipitating agent is simultaneously transported to the precipitator, so that the carbon dioxide-based biodegradable polymer is precipitated from the mixed liquid to obtain a liquid to be precipitated; the precipitator is continuously fed and continuously extracted;
[0011] 4) The sedimentation liquid continuously extracted from the precipitator enters the stratifier for stratification. The upper layer of the stratifier continuously overflows from the upper part of the stratifier and enters the recovery system. The bottom material is continuously discharged from the bottom of the stratifier and enters the devolatilizer to remove the volatile matter. The volatile matter is condensed and sent to the recovery system. The output of the devolatilizer is the finished product.
[0012] The present invention continuously dissolves the glue solution after the reaction in a dissolver, and then continuously precipitates in a precipitator after the dissolution. The dissolution and precipitation are continuously performed, thereby avoiding the quality difference between batches when discharging in batches in the reactor, and improving the production efficiency. The liquid and the precipitated sediment are also continuously separated in the stratifier, and the liquid overflows from the upper part of the stratifier by itself; the precipitated sediment is continuously discharged by itself from the bottom of the stratifier, achieving the purpose of continuous feeding and continuous separation without external power, and reducing production energy consumption compared with other separation methods.
[0013] In a preferred continuous production process of the carbon dioxide-based biodegradable polymer, the comonomer is one or a combination of epoxy compounds, anhydride compounds and ester compounds.
[0014] Preferably, the epoxy compound is an alkylene oxide. The alkylene oxide is selected from one or a combination of ethylene oxide, propylene oxide, butylene oxide, cyclohexene oxide, epichlorohydrin, pentyl oxide, and hexene oxide. The anhydride compound is terephthalic acid, phthalic anhydride, or 1,8-naphthalene anhydride. More preferably, the alkylene oxide is selected from one or a combination of two of ethylene oxide, propylene oxide, and cyclohexene oxide. The anhydride compound is phthalic anhydride.
[0015] This production process can be applied to the production of most carbon dioxide-based biodegradable polymers by adjusting the types and amounts of the glue dissolving agent and the polymer precipitating agent.
[0016] The present invention is aimed at the production of different carbon dioxide-based biodegradable polymers, and it is necessary to adjust the type and amount of the glue dissolving agent; specifically, in the above-mentioned continuous production process of carbon dioxide-based biodegradable polymers: the glue dissolving agent is one or a combination of dichloromethane, 1,2-dichloroethane, 1,2-dichloropropane, acetone, ethyl acetate, carbon tetrachloride, styrene, trichloroethylene; in step 2), the mass ratio of the polymer glue and the glue dissolving agent fed into the dissolver per unit time is 1: (0.1~3). The type and amount of the above-mentioned glue dissolving agent can meet the continuous production process of various types of carbon dioxide-based biodegradable polymers. Different choices affect the dissolution time and dissolution rate, and no examples are given here.
[0017] Preferably, the glue dissolving agent is a mixed solvent of 1,2-dichloroethane and 1,2-dichloropropane; in step 2), the mass ratio of the polymer glue and the glue dissolving agent fed into the dissolver per unit time is 1:(0.1~1). The preferred glue dissolving agent is particularly suitable for carbon dioxide-based biodegradable polymers copolymerized with carbon dioxide and epoxy compound monomers, and has a faster dissolution efficiency for such polymers, and can use less glue dissolving agent and complete the dissolution faster. The requirements for the dissolver are low, and the time required in the dissolver is shorter, which is conducive to improving the production efficiency of the entire production process.
[0018] More preferably, the mass ratio of 1,2-dichloroethane and 1,2-dichloropropane in the mixed solvent is 3-7:1; the mass ratio of the polymer glue and the glue dissolving agent delivered into the dissolver per unit time in step 2) is 1:(0.1-0.3). The more preferred glue dissolving agent is particularly suitable for the copolymerization of carbon dioxide, alkylene oxide and phthalic anhydride, has a faster dissolving efficiency for the polymer, and can use less glue dissolving agent and complete the dissolution faster. The requirements for the residence time and mixing capacity in the dissolver are low, which is conducive to improving the production efficiency of the production process.
[0019] The present invention is aimed at the production of different carbon dioxide-based biodegradable polymers, and it is necessary to adjust the type and amount of the polymer precipitating agent; specifically, in the above-mentioned continuous production process of carbon dioxide-based biodegradable polymers: the polymer precipitating agent is one or a combination of alcohols, ethers, and alkanes; in step 3), the mass ratio of the mixed liquid and the polymer precipitating agent transported into the precipitator per unit time is 1: (0.2~1.5). The type and amount of the above-mentioned polymer precipitating agent can meet the continuous production process of various types of carbon dioxide-based biodegradable polymers. Different choices affect the polymer precipitation time and precipitation rate, and no examples are given here.
[0020] Preferably, the polymer precipitating agent is a mixed precipitating agent of anhydrous ethanol and n-butyl ether in a mass ratio of 2 to 10:1; in step 3), the mass ratio of the mixed liquid and the polymer precipitating agent transported into the precipitator per unit time is 1:(0.2 to 0.4). The preferred polymer precipitating agent is particularly suitable for the copolymerization of carbon dioxide, alkylene oxide and phthalic anhydride, and has a faster precipitation efficiency for the polymer, and can use less polymer precipitating agent to complete polymer precipitation faster. The requirements for the residence time and mixing capacity in the precipitator are low, and the combination with the above-mentioned more preferred glue dissolving agent is more conducive to improving the production efficiency of the polymer production process.
[0021] Specifically, the dissolver and the precipitator are both devices with two feed ports and a liquid mixing function. The two feed ports of the dissolver respectively feed the polymer glue solution and the glue solution dissolving agent, and the two feed ports of the precipitator respectively feed the mixed solution and the polymer precipitating agent; the liquid mixing function ensures that the polymer glue solution and the glue solution dissolving agent or the mixed solution and the polymer precipitating agent are in full contact.
[0022] Specifically, the dissolver is a pipeline mixer, a kettle agitator, a twin-screw extruder, a single-screw extruder, a mixing pump, a screw pump, or a combination thereof; the precipitator is a pipeline mixer, a kettle agitator, a twin-screw extruder, a single-screw extruder, a mixing pump, a screw pump, or a combination thereof. When the kettle agitator is used as a dissolver or a precipitator, it can be used in combination with the pipeline mixer to achieve the requirements of continuous dissolution and precipitation of the present invention.
[0023] Specifically, the stratifier is a kettle type, and the aspect ratio of the stratifier is 2 to 15: 1. The stratifier of the present invention does not require stirring and rotating power, and after the sedimentation liquid enters the stratifier, it settles automatically under the action of gravity to achieve the purpose of solid-liquid separation.
[0024] The working temperature of the dissolver and the precipitator is 1°C to 100°C, and the working temperature of the devolatilizer in step 4) is 30°C to 200°C. The devolatilizer is heated and extruded, and the heating process is conducive to the volatilization and separation of the glue dissolving agent and the polymer precipitating agent, which can be recovered after condensation. At the same time, after the volatilization and separation of the glue dissolving agent and the polymer precipitating agent, the purity of the product is improved.
[0025] The invention is applied to the continuous production process of carbon dioxide-based biodegradable binary and higher copolymers.
[0026] Compared with the prior art, the continuous production process of a carbon dioxide-based biodegradable polymer of the present invention has the following beneficial effects:
[0027] The present invention aims at the deficiencies existing in the preparation and purification process of existing carbon dioxide-based biodegradable plastics, and provides a continuous production process of carbon dioxide-based biodegradable plastics. One of the innovative points of the present invention is to remove the catalyst in the glue solution after the reaction by using a solvent dissolution and a precipitating agent precipitation method, and to remove unreacted monomers, solvent molecules, precipitating agent molecules, by-products and other impurities by using a twin-screw devolatilizer. After the bulk polymerization reaction is completed, catalysts and a large amount of unreacted monomers will remain, which will cause great difficulties for the next devolatilization and refining process. The residual catalyst will also cause the product to deteriorate and denature if it exists for a long time. This process scheme not only washes away the catalyst, but also washes away a large amount of unreacted monomers, making devolatilization easier. The second innovative point is the continuous feeding and discharging of dissolution and precipitation, which is achieved continuously while ensuring the dissolution and precipitation effects, and a suitable stirring device is selected. The third innovative point is the separation of the liquid phase and the solid phase after precipitation. The present invention adopts a kettle-type stratifier with a certain aspect ratio, and realizes stratification by using the density difference between the liquid phase and the solid phase.
[0028] In summary, the continuous production process of a carbon dioxide-based biodegradable polymer provided by the present invention has the advantages of continuity, low operating temperature, good refining effect and low energy consumption. The impurity content in the obtained biodegradable plastic product is below 0.5%, which is suitable for industrialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The present invention is a schematic flow diagram of a continuous production process of a carbon dioxide-based biodegradable polymer.
[0030] Among them, 1. Reactor 2. Buffer tank 3. Dissolver 4. Separator 5. Stratifier 6. Devolatilizer 7. Condenser 8. Solvent receiving tank 9. Solvent pipeline 10. Product output end. DETAILED DESCRIPTION
[0031] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0032] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application may be combined with each other.
[0033] The present invention is further described below in conjunction with specific embodiments, wherein Embodiment 1 is the best implementation.
[0034] Example 1
[0035] 1) After the reaction in reactor 1 is completed, the polymer glue is transported to buffer tank 2 at a flow rate of 2m³ / h. After the transportation is completed, reactor 1 can carry out the next batch of reaction feeding.
[0036] The polymer glue in the buffer tank 2 is continuously transported at a flow rate of 200 kg / h to the dissolver 3 which is served by a three-way flow pump at the suction port. At the same time, a mixed solvent of 1,2-dichloroethane and 1,2-dichloropropane in a mass ratio of 5:1 is continuously transported into the dissolver 3 at a flow rate of 20 kg / h. The rotation speed is 60 r / min and the temperature is controlled at 30°C.
[0037] The mixed liquid output from the dissolver 3 is continuously transported at a flow rate of 220 kg / h to the precipitator 4, which is served by a three-way mixing pump at the suction port. At the same time, a mixed precipitating agent prepared by mixing anhydrous ethanol and n-butyl ether in a mass ratio of 6:1 is continuously transported into the precipitator 4 at a flow rate of 44 kg / h. The rotation speed is 90 r / min and the temperature is controlled at 20°C.
[0038] The liquid to be precipitated outputted from the precipitator 4 is continuously conveyed to the stratifier 5 at a flow rate of 264 kg / h. The length-to-diameter ratio of the stratifier 5 is 8:1. The upper layer liquid continuously overflows from the upper part of the stratifier 5 and enters the solvent receiving tank 8 through the solvent pipeline 9. The material at the bottom is continuously discharged from the bottom of the stratifier and enters the devolatilizer 6 to remove the volatile matter. The material entering the devolatilizer 6 is devolatilized at 150° C. and a vacuum degree of 0.1 MPa. The finished product is obtained by discharging the material at the product output end 10 of the devolatilizer 6.
[0039] The polymer glue is a carbon dioxide-based multipolymer, which is a propylene oxide-phthalic anhydride-carbon dioxide terpolymer with a number average molecular weight of 9.36×10 6 g / mol, solid content is 57.65%, and viscosity at 25°C is 150880mPa.S.
[0040] The purity of the solid sample after devolatilization was 99.74%, and the yield was 99.89%. Yield calculation method: weigh the mass of the solid sample m1; yield = m (glue) × glue solid content / m1 × 100%.
[0041] Example 2
[0042] 1) After the reaction in reactor 1 is completed, the polymer glue is transported to buffer tank 2 at a flow rate of 2m³ / h. After the transportation is completed, reactor 1 can carry out the next batch of reaction feeding.
[0043] The polymer glue in the buffer tank 2 is continuously transported at a flow rate of 200 kg / h to the dissolver 3 which is served by a three-way mixing pump at the suction port. At the same time, a mixed solvent of 1,2-dichloroethane and 1,2-dichloropropane in a mass ratio of 3:1 is continuously transported into the dissolver 3 at a flow rate of 40 kg / h. The rotation speed is 60 r / min and the temperature is controlled at 30°C.
[0044] The mixed liquid output from the dissolver 3 is continuously transported at a flow rate of 240 kg / h to the precipitator 4, which is served by a three-way mixing pump at the suction port. At the same time, a mixed precipitating agent prepared by mixing anhydrous ethanol and n-butyl ether in a mass ratio of 2:1 is continuously transported into the precipitator 4 at a flow rate of 72 kg / h. The rotation speed is 80 r / min and the temperature is controlled at 20°C.
[0045] The liquid to be precipitated outputted from the precipitator 4 is continuously conveyed to the stratifier 5 at a flow rate of 312 kg / h. The length-diameter ratio of the stratifier 5 is 5:1. The upper layer liquid continuously overflows from the upper part of the stratifier 5 and enters the solvent receiving tank 8 through the solvent pipeline 9. The material at the bottom is continuously discharged from the bottom of the stratifier and enters the devolatilizer 6 to remove the volatile matter. The material entering the devolatilizer 6 is devolatilized at 150° C. and a vacuum degree of 0.1 MPa. The product is discharged from the product output end 10 of the devolatilizer 6 to obtain the finished product.
[0046] The polymer glue is a carbon dioxide-based multipolymer, which is a propylene oxide-ethylene oxide-phthalic anhydride-carbon dioxide quaternary copolymer with a number average molecular weight of 9.36×10 6 g / mol, solid content is 54.365%, and viscosity at 25°C is 132891mPa.S.
[0047] The purity of the solid sample after devolatilization was 99.71%, and the yield was 99.89%. Yield calculation method: weigh the mass of the solid sample m1; yield = m (glue) × glue solid content / m1 × 100%.
[0048] Example 3
[0049] 1) After the reaction in reactor 1 is completed, the polymer glue is transported to buffer tank 2 at a flow rate of 2m³ / h. After the transportation is completed, reactor 1 can carry out the next batch of reaction feeding.
[0050] The polymer glue in the buffer tank 2 is continuously transported at a flow rate of 200 kg / h to the dissolver 3 which is served by a three-way mixing pump at the suction port. At the same time, a mixed solvent of 1,2-dichloroethane and 1,2-dichloropropane in a mass ratio of 7:1 is continuously transported into the dissolver 3 at a flow rate of 60 kg / h. The rotation speed is 60 r / min and the temperature is controlled at 30°C.
[0051] The mixed liquid output from the dissolver 3 is continuously transported at a flow rate of 260 kg / h to the precipitator 4, which is served by a three-way mixing pump at the suction port. At the same time, a mixed precipitating agent prepared by mixing anhydrous ethanol and n-butyl ether in a mass ratio of 10:1 is continuously transported into the precipitator 4 at a flow rate of 104 kg / h. The rotation speed is 100 r / min and the temperature is controlled at 20°C.
[0052] The liquid to be precipitated outputted from the precipitator 4 is continuously conveyed to the stratifier 5 at a flow rate of 364 kg / h. The length-to-diameter ratio of the stratifier 5 is 12:1. The upper layer liquid continuously overflows from the upper part of the stratifier 5 and enters the solvent receiving tank 8 through the solvent pipeline 9. The material at the bottom is continuously discharged from the bottom of the stratifier and enters the devolatilizer 6 to remove the volatile matter. The material entering the devolatilizer 6 is devolatilized at 150° C. and a vacuum degree of 0.1 MPa. The finished product is obtained by discharging the material at the product output end 10 of the devolatilizer 6.
[0053] The polymer glue is a carbon dioxide-based multipolymer, which is a terpolymer of propylene oxide-cyclohexene oxide-phthalic anhydride-carbon dioxide, with a number average molecular weight of 7.64×10 6 g / mol, solid content is 58.12%, and viscosity at 25°C is 161200mPa.S.
[0054] The purity of the solid sample after devolatilization was 99.70%, and the yield was 99.90%. Yield calculation method: weigh the mass of the solid sample m1; yield = m (glue) × glue solid content / m1 × 100%.
[0055] Example 4
[0056] 1) After the reaction in reactor 1 is completed, the polymer glue is transported to buffer tank 2 at a flow rate of 2m³ / h. After the transportation is completed, reactor 1 can carry out the next batch of reaction feeding.
[0057] The polymer glue in the buffer tank 2 is continuously transported at a flow rate of 200 kg / h to the dissolver 3 which is served by a three-way mixing pump at the suction port. At the same time, a mixed solvent of 1,2-dichloroethane and 1,2-dichloropropane in a mass ratio of 1:1 is continuously transported into the dissolver 3 at a flow rate of 120 kg / h. The rotation speed is 60 r / min and the temperature is controlled at 25°C.
[0058] The mixed liquid output from the dissolver 3 is continuously transported at a flow rate of 320 kg / h to the precipitator 4 which is served by a three-way mixing pump at the suction port. At the same time, a mixed precipitating agent prepared by mixing anhydrous ethanol and n-butyl ether in a mass ratio of 0.1:1 is continuously transported into the precipitator 4 at a flow rate of 256 kg / h. The rotation speed is 90 r / min and the temperature is controlled at 25°C.
[0059] The liquid to be precipitated outputted from the precipitator 4 is continuously conveyed to the stratifier 5 at a flow rate of 576 kg / h. The length-to-diameter ratio of the stratifier 5 is 2:1. The upper layer liquid continuously overflows from the upper part of the stratifier 5 and enters the solvent receiving tank 8 through the solvent pipeline 9. The material at the bottom is continuously discharged from the bottom of the stratifier and enters the devolatilizer 6 to remove the volatile matter. The material entering the devolatilizer 6 is devolatilized at 150° C. and a vacuum degree of 0.1 MPa. The product is discharged from the product output end 10 of the devolatilizer 6 to obtain the finished product.
[0060] The polymer glue is a carbon dioxide-based multi-polymer, and the carbon dioxide-based multi-polymer is a propylene oxide-carbon dioxide binary copolymer with a number average molecular weight of 15.67×10 6 g / mol, solid content is 56.57%, and viscosity at 25°C is 153429mPa.S.
[0061] The purity of the solid sample after devolatilization was 99.65%, and the yield was 99.82%. Yield calculation method: weigh the mass of the solid sample m1; yield = m (glue) × glue solid content / m1 × 100%.
[0062] Example 5
[0063] 1) After the reaction in reactor 1 is completed, the polymer glue is transported to buffer tank 2 at a flow rate of 2m³ / h. After the transportation is completed, reactor 1 can carry out the next batch of reaction feeding.
[0064] The polymer glue in the buffer tank 2 is continuously transported at a flow rate of 200 kg / h to the dissolver 3 which is served by a three-way screw pump at the suction port. At the same time, a mixed solvent of 1,2-dichloroethane and 1,2-dichloropropane in a mass ratio of 10:1 is continuously transported into the dissolver 3 at a flow rate of 200 kg / h, the rotation speed is 60 r / min, and the temperature is controlled at 45°C.
[0065] The mixed liquid output from the dissolver 3 is continuously transported at a flow rate of 400 kg / h to the precipitator 4 which is served by a three-way screw pump at the suction port. At the same time, a mixed precipitating agent prepared by mixing anhydrous ethanol and n-butyl ether in a mass ratio of 20:1 is continuously transported into the precipitator 4 at a flow rate of 400 kg / h. The rotation speed is 100 r / min and the temperature is controlled at 30°C.
[0066] The liquid to be precipitated outputted from the precipitator 4 is continuously transported to the stratifier 5 at a flow rate of 800 kg / h. The length-diameter ratio of the stratifier 5 is 15:1. The upper layer liquid continuously overflows from the upper part of the stratifier 5 and enters the solvent receiving tank 8 through the solvent pipeline 9. The material at the bottom is continuously discharged from the bottom of the stratifier and enters the devolatilizer 6 to remove the volatile matter. The material entering the devolatilizer 6 is devolatilized at 150° C. and a vacuum degree of 0.1 MPa. The product is discharged from the product output end 10 of the devolatilizer 6 to obtain the finished product.
[0067] The polymer glue is the same as in Example 1.
[0068] The purity of the solid sample after devolatilization was 99.62%, and the yield was 99.85%. Yield calculation method: weigh the mass of the solid sample m1; yield = m (glue) × glue solid content / m1 × 100%.
[0069] Example 6
[0070] 1) After the reaction in reactor 1 is completed, the polymer glue is transported to buffer tank 2 at a flow rate of 2m³ / h. After the transportation is completed, reactor 1 can carry out the next batch of reaction feeding.
[0071] The polymer glue in the buffer tank 2 is continuously transported at a flow rate of 200 kg / h to the dissolver 3, which is served by a three-way mixing pump at the suction port. At the same time, 1,2-dichloroethane is continuously transported into the dissolver 3 at a flow rate of 440 kg / h, the rotation speed is 60 r / min, and the temperature is controlled at 30°C.
[0072] The mixed liquid output from the dissolver 3 is continuously transported at a flow rate of 640 kg / h to the precipitator 4, which is served by a three-way mixing pump at the suction port. At the same time, ether is continuously transported into the precipitator 4 at a flow rate of 832 kg / h, the rotation speed is 80~100 r / min, and the temperature is controlled at 20°C.
[0073] The liquid to be precipitated outputted from the precipitator 4 is continuously conveyed to the stratifier 5 at a flow rate of 1472 kg / h. The length-diameter ratio of the stratifier 5 is 8:1. The upper layer liquid continuously overflows from the upper part of the stratifier 5 and enters the solvent receiving tank 8 through the solvent pipeline 9. The material at the bottom is continuously discharged from the bottom of the stratifier and enters the devolatilizer 6 to remove the volatile matter. The material entering the devolatilizer 6 is devolatilized at 150° C. and a vacuum degree of 0.1 MPa. The finished product is obtained by discharging the material at the product output end 10 of the devolatilizer 6.
[0074] The polymer glue is the same as in Example 1.
[0075] The purity of the solid sample after devolatilization was 98.77%, and the yield was 99.14%. Yield calculation method: weigh the mass of the solid sample m1; yield = m (glue) × glue solid content / m1 × 100%.
[0076] Example 7
[0077] 1) After the reaction in reactor 1 is completed, the polymer glue is transported to buffer tank 2 at a flow rate of 2m³ / h. After the transportation is completed, reactor 1 can carry out the next batch of reaction feeding.
[0078] The polymer glue in the buffer tank 2 is continuously transported at a flow rate of 200 kg / h to the dissolver 3 which is provided with a three-way mixing pump at the suction port. At the same time, a mixed solvent of 1,2-dichloroethane and 1,2-dichloropropane in a mass ratio of 5:1 is continuously transported into the dissolver 3 at a flow rate of 200 kg / h. The rotation speed is 60 r / min and the temperature is controlled at 30°C.
[0079] The mixed liquid output from the dissolver 3 is continuously transported at a flow rate of 400 kg / h to the precipitator 4, which is served by a three-way mixing pump at the suction port. At the same time, a mixed precipitating agent prepared by mixing anhydrous ethanol and n-butyl ether in a mass ratio of 6:1 is continuously transported into the precipitator 4 at a flow rate of 320 kg / h. The rotation speed is 100 r / min and the temperature is controlled at 20°C.
[0080] The liquid to be precipitated outputted from the precipitator 4 is continuously conveyed to the stratifier 5 at a flow rate of 720 kg / h. The length-diameter ratio of the stratifier 5 is 8:1. The upper layer liquid continuously overflows from the upper part of the stratifier 5 and enters the solvent receiving tank 8 through the solvent pipeline 9. The material at the bottom is continuously discharged from the bottom of the stratifier and enters the devolatilizer 6 to remove the volatile matter. The material entering the devolatilizer 6 is devolatilized at 150° C. and a vacuum degree of 0.1 MPa. The finished product is obtained by discharging the material at the product output end 10 of the devolatilizer 6.
[0081] The polymer glue is the same as in Example 1.
[0082] The purity of the solid sample after devolatilization was 99.24%, and the yield was 98.36%. Yield calculation method: weigh the mass of the solid sample m1; yield = m (glue) × glue solid content / m1 × 100%.
[0083] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A continuous production process for carbon dioxide-based biodegradable polymers, It is characterized in that The following steps are involved: 1) Carbon dioxide and comonomers are subjected to carbon dioxide-based multi-polymerization under the action of a catalyst in a reactor (1) to obtain a polymer glue solution, and the polymer glue solution obtained after each reaction is transferred to a buffer tank (2) for temporary storage; 2) continuously conveying the polymer glue liquid from the buffer tank (2) to the dissolver (3), and simultaneously conveying the glue liquid dissolving agent to the dissolver (3), so that the glue liquid is dissolved in the glue liquid dissolving agent to obtain a mixed liquid; the dissolver (3) continuously feeds and continuously extracts; 3) The mixed liquid continuously extracted from the dissolver (3) is continuously transported into the precipitator (4), and the polymer precipitating agent is simultaneously transported into the precipitator (4), so that the carbon dioxide-based biodegradable polymer is precipitated from the mixed liquid to obtain a liquid to be precipitated; the precipitator (4) continuously extracts while continuously feeding; 4) The liquid to be precipitated is continuously extracted from the precipitator (4) and enters the stratifier (5) for stratification. The upper layer of the stratifier (5) continuously overflows from the upper part of the stratifier (5) and enters the recovery system. The material at the bottom is continuously discharged from the bottom of the stratifier (5) and enters the devolatilizer (6) to remove volatiles. The volatiles are condensed and sent to the recovery system. The output of the devolatilizer (6) is the finished product. The glue solution dissolving agent is a mixed solvent of 1,2-dichloroethane and 1,2-dichloropropane in a mass ratio of 3 to 7:1; in step 2), the mass ratio of the polymer glue solution and the glue solution dissolving agent fed into the dissolver (3) per unit time is 1:(0.1 to 0.3); the polymer precipitating agent is a mixed precipitating agent of anhydrous ethanol and n-butyl ether in a mass ratio of 2 to 10:1; in step 3), the mass ratio of the mixed solution and the polymer precipitating agent fed into the precipitator (4) per unit time is 1:(0.2 to 0.4); The dissolver (3) is one or a combination of a pipeline mixer, a kettle agitator, a twin-screw extruder, and a single-screw extruder; the precipitator (4) is one or a combination of a pipeline mixer, a kettle agitator, a twin-screw extruder, and a single-screw extruder.
2. A continuous production process for a carbon dioxide-based biodegradable polymer according to claim 1, Features: The comonomer is one or a combination of epoxy compounds, anhydride compounds and ester compounds.
3. A continuous production process for a carbon dioxide-based biodegradable polymer according to claim 1, Features: The dissolver (3) and precipitator (4) are both devices having two feed ports and a liquid mixing function.
4. The continuous production process of a carbon dioxide-based biodegradable polymer according to claim 1, Features: The classifier (5) is of a kettle type, and the length-to-diameter ratio of the classifier (5) is 2-15:1.
Citation Information
Patent Citations
Preparation method of biodegradable carbon dioxide-based polyester-polycarbonate terpolymer
CN111378101A
Biodegradable carbon dioxide-based terpolymer and preparation method thereof
CN114539515A
Aliphatic polycarbonate washing coagulation devolatilization method and specific device thereof
CN101928387A
Method for copolymerizing carbon dioxide and propylene oxide with circulation flow reactor
CN102690411A
Method for preparing aliphatic polycarbonate through continuous solution polymerization method
CN103214666A
Cited By
Energy-saving production device and production method of a bio-based plasticizer
CN123079270A