A method for preparing high-brightness blue fluorescent MOF-2 material
By applying high-pressure treatment to the MOF-2 material and releasing the pressure, the problem of fluorescence quenching in the material was solved, and high-brightness blue fluorescent MOF-2 material was successfully prepared, which improved the optical performance of the material and expanded the selection of initial materials.
Patent Information
- Application Number
- CN202310255831.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-16
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In MOF-2 materials, it is difficult to prepare high-brightness blue fluorescent materials due to fluorescence quenching caused by the vibration and rotation of organic ligands, coordination molecules and solvents.
Different pressures were applied to the initially non-emitting MOF-2 material through a diamond anvil. After the high-pressure experiment, the pressure was released to normal pressure, and a ruby ball was used to calibrate the pressure to prepare a high-brightness blue fluorescent MOF-2 material.
This method is simple, room-temperature synthesis, and highly reproducible. The obtained MOF-2 material has a basically consistent framework structure and high-brightness blue fluorescent properties, expanding the range of initial material selection for high-brightness blue fluorescent materials.
Smart Images

Figure CN116240016B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of blue fluorescent materials, and in particular relates to a method for preparing a high-brightness blue fluorescent MOF-2 material. Background Art
[0002] Fluorescent materials have important applications in lighting, display, imaging and visible light transmission, and have become one of the research hotspots in recent years. Compared with red and green light emitting materials, the design and preparation of high-energy blue fluorescent materials is one of the more challenging tasks in this research field. MOFs materials have the characteristics of designable topological structures, multiple types of emission centers, multiple types of charge / energy transfer pathways, and the combination of various fluorescence mechanisms for fluorescence emission, so they have the potential for full-spectrum tunable luminescence. However, the large internal specific surface area and ultra-high porosity give MOFs materials great spatial freedom of movement. Especially for MOFs materials with rotatable groups, the vibration and rotation of guest molecules and organic ligands will greatly damage the optical properties of MOFs materials. Due to the structural characteristics of the para-substituted organic ligands and the obvious pore structure, the vibration and rotation freedom of organic ligands, coordination molecules and solvent molecules in MOF-2 materials are large, which is a typical example of fluorescence quenching in MOFs materials. Therefore, it is necessary to reduce the non-radiative energy loss caused by the vibration and rotation of organic ligands, coordination molecules and solvent molecules in MOF-2 materials, so as to prepare MOF-2 materials with high brightness blue fluorescence. Summary of the invention
[0003] The technical problem to be solved by the present invention is: to overcome the fluorescence quenching problem existing in MOF-2 materials, to provide a method for preparing high-brightness blue fluorescent MOF-2 materials through pressure treatment engineering, and to be able to regulate the fluorescence properties of the material by controlling different pressure points.
[0004] The present invention uses non-luminescent MOF-2 as the initial material, applies different pressures to the initial raw material through a diamond anvil, and then releases the pressure of the diamond anvil to normal pressure to obtain a bright blue fluorescent MOF-2 material. The specific technical scheme is as follows:
[0005] A method for preparing a high-brightness blue fluorescent MOF-2 material comprises the following steps: using non-emitting MOF-2 as an initial material, performing the experiment in a diamond anvil, using a T301 stainless steel gasket for a high-pressure experiment, using a diamond anvil for pre-pressing, using a laser puncher to punch a microporous sample cavity with a diameter of 160 μm at the center of a pre-pressed pit, loading the initial material into the sample cavity and then placing a ruby ball therein, and using a ruby fluorescence spectrum to calibrate the pressure in the sample cavity, and in the high-pressure fluorescence experiment, without adding a pressure-transmitting medium, the diamond anvil presses the initial material to 10 to 22 GPa, and then the diamond anvil is depressurized to normal pressure to obtain a MOF-2 material with bright blue fluorescence.
[0006] Preferably, the initial material is pressurized to 16 GPa in a diamond anvil, and then the diamond anvil is depressurized to normal pressure to obtain a MOF-2 material with optimal fluorescence performance.
[0007] The synthesis of the non-emissive MOF-2 material was based on reported literature methods.
[0008] Beneficial effects:
[0009] The advantages of the method for preparing high-brightness blue fluorescent MOF-2 materials by pressure engineering of the present invention are that the method is simple in process, room temperature synthesis, high in repeatability, clean and environmentally friendly; the preparation method of the present invention is based on the initial non-emitting MOF-2 material, and the obtained MOF-2 has a basically consistent framework structure with the initial non-emitting MOF-2, and has high-brightness blue fluorescent performance. The high-brightness blue fluorescent MOF-2 material was successfully prepared, which expands the selection range of the initial material for preparing the high-brightness blue fluorescent material. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 This is a scanning electron microscope image of the non-emissive MOF-2 sample prepared in Example 1.
[0011] Figure 2 This is the in-situ synchrotron radiation XRD spectrum of the non-emitting MOF-2 sample prepared in Example 1.
[0012] Figure 3 This is the in-situ high-pressure infrared absorption spectrum of the non-emissive MOF-2 sample prepared in Example 1.
[0013] Figure 4 This is the in-situ high-pressure Raman scattering spectrum of the non-emissive MOF-2 sample prepared in Example 1.
[0014] Figure 5 This is the fluorescence spectrum of the MOF-2 sample before and after 10 GPa pressure treatment in Example 3.
[0015] Figure 6This is the fluorescence spectrum of the MOF-2 sample before and after 14 GPa pressure treatment in Example 3.
[0016] Figure 7 This is the fluorescence spectrum of the MOF-2 sample before and after 16 GPa pressure treatment in Example 3.
[0017] Figure 8 This is the fluorescence spectrum of the MOF-2 sample of Example 3 before and after 18 GPa pressure treatment.
[0018] Fig. 9 This is the fluorescence spectrum of the MOF-2 sample of Example 3 before and after 22 GPa pressure treatment.
[0019] Fig.10 This is the in-situ synchrotron radiation XRD spectrum of the MOF-2 sample after 16 GPa pressure treatment in Example 3.
[0020] Fig.11 This is the in-situ high-pressure infrared absorption spectrum of the MOF-2 sample after 16 GPa pressure treatment in Example 3.
[0021] Fig.12 This is the in-situ high-pressure Raman scattering spectrum of the MOF-2 sample after 16 GPa pressure treatment in Example 3. DETAILED DESCRIPTION
[0022] The present invention is now described in more detail with reference to the following examples. Unless otherwise specified, all reagents used are commercially available products and are not further purified.
[0023] Example 1: Preparation and characterization of non-emissive MOF-2 samples
[0024] The synthesis of MOF-2 material refers to the reported literature method. The experiment was carried out in a Teflon hydrothermal reactor under heating in an oven. The specific synthesis process is as follows: Zn(NO3)26H2O (0.2977g, 1.0mmol) and 1,4-benzenedicarboxylic acid (H2BDC, 0.166g, 1.0mol) were dissolved in N, N-dimethylformamide (DMF, 10mL) and stirred at room temperature for 10 minutes to obtain a colorless transparent liquid. The colorless transparent solution was transferred to a polytetrafluoroethylene liner and encapsulated in a Teflon hydrothermal reactor. The reactor was placed in a 95℃ oven for reaction for 24 hours and then taken out. The obtained crystals were soaked in 1-2mL of mother liquor and diffused through distilled water at 45℃ for 12 hours. The finally obtained MOF-2 crystals were washed with DMF and H2O.
[0025] Example 2: Morphology and structural characterization of non-emissive MOF-2 samples
[0026] The non-emissive MOF-2 samples were characterized by scanning electron microscopy, in situ synchrotron radiation XRD, in situ high-pressure infrared absorption spectroscopy and in situ high-pressure Raman reflection spectroscopy.
[0027] Figure 1 This is a scanning electron microscope photo of a non-emissive MOF-2 material. The image shows that MOF-2 crystals have a layered stacking structure. Figure 2 This is the in-situ synchrotron radiation XRD spectrum of the prepared non-emitting MOF-2 sample. Figure 3 This is the in-situ high-pressure infrared absorption spectrum of the prepared non-emissive MOF-2 sample. Figure 4 This is the in-situ high-pressure Raman scattering spectrum of the prepared non-emitting MOF-2 sample. The structural characterization results are consistent with the standard spectrum reported in the literature, indicating that the MOF-2 sample was successfully prepared.
[0028] Example 3: High-pressure preparation of high-brightness blue fluorescent MOF-2 materials
[0029] The pressure treatment was carried out in a diamond anvil apparatus with an anvil face diameter of 400μm. A T301 stainless steel gasket was pre-pressed with a pit with a thickness of 40μm, and a microporous sample cavity with a diameter of about 160μm was obtained in the center of the pit using a laser puncher. After the sample was loaded into the sample cavity, it was loaded into a ruby ball to determine the actual pressure in the sample cavity. The pressure calibration was carried out using the standard ruby fluorescence method. The in-situ high-pressure fluorescence experiment was carried out using a 10mW 355nm laser excitation line. In the high-pressure experiment, no pressure-transmitting medium was added. The diamond anvil pressurized the sample to 10GPa, 14GPa, 16GPa, 18GPa and 22GPa respectively, and then the diamond anvil was depressurized to normal pressure to obtain a high-brightness blue fluorescent MOF-2 material.
[0030] Under the same test conditions, the fluorescence spectra of MOF-2 samples before and after pressure treatment at 10 GPa, 14 GPa, 16 GPa, 18 GPa and 22 GPa were collected respectively. Figure 5 This is the fluorescence spectrum of the MOF-2 sample before and after 10GPa pressure treatment. Figure 6 This is the fluorescence spectrum of the MOF-2 sample before and after 14GPa pressure treatment. Figure 7 This is the fluorescence spectrum of the MOF-2 sample before and after 16GPa pressure treatment. Figure 8 This is the fluorescence spectrum of the MOF-2 sample before and after 18GPa pressure treatment. Fig. 9 This is the fluorescence spectrum of the MOF-2 sample before and after 22GPa pressure treatment. The sample did not emit any light before pressure treatment, and the fluorescence emission was the strongest after 16GPa pressure treatment. Therefore, 16GPa is the optimal pressure point for MOF-2 material to obtain the best fluorescence performance.
[0031] Example 4: Structural Characterization of MOF-2 Samples with Best Fluorescence Performance
[0032] The MOF-2 sample with the best fluorescence performance was obtained after being treated at 16 GPa. In-situ synchrotron XRD, in-situ high-pressure infrared absorption spectroscopy and in-situ high-pressure Raman reflection spectroscopy were performed on the MOF-2 sample treated at 16 GPa.
[0033] Fig.10 This is the synchrotron radiation XRD spectrum of the MOF-2 sample after 16 GPa pressure treatment. Fig.11 This is the in-situ high-pressure infrared absorption spectrum of the MOF-2 sample after 16GPa pressure treatment. Fig.12 This is the in-situ high-pressure Raman scattering spectrum of the MOF-2 sample after 16 GPa pressure treatment. Structural characterization shows that MOF-2 has a basically consistent framework structure before and after 16 GPa pressure treatment.
Claims
1. A method for preparing a high-brightness blue fluorescent MOF-2 material, using non-emitting MOF-2 as the initial material, and conducting the experiment in a diamond anvil. A T301 stainless steel gasket is used for the high-pressure experiment. After pre-pressing the diamond anvil, a microporous sample cavity with a diameter of 160 μm is punched at the center of the pre-pressed pit using a laser puncher. After the initial material is loaded into the sample cavity, a ruby ball is placed, and the pressure in the sample cavity is calibrated using a ruby fluorescence spectrum. In the high-pressure fluorescence experiment, no pressure-transmitting medium is added. The diamond anvil presses the initial material to 10-22 GPa, and then the diamond anvil is depressurized to normal pressure to obtain a bright blue fluorescent MOF-2 material. The preparation method of the non-emissive MOF-2 is as follows: Zn(NO3)26H2O and 1,4-phthalic acid are dissolved in N,N-dimethylformamide, and a colorless transparent liquid is obtained after stirring at room temperature for 10 minutes. The colorless transparent solution is transferred to a polytetrafluoroethylene liner and encapsulated in a Teflon hydrothermal reactor. The reactor is placed in a 95°C oven for reaction for 24 hours and then taken out. The obtained crystals are immersed in 1-2 mL of mother liquor and diffused through distilled water at 45°C for 12 hours. Finally, the obtained MOF-2 crystals are washed with DMF and H2O.
2. A method for preparing a high-brightness blue fluorescent MOF-2 material according to claim 1, characterized in that: The initial material was pressurized to 16 GPa in a diamond anvil, and then the diamond anvil was depressurized to normal pressure to obtain the MOF-2 material with the best fluorescence performance.