A non-quenched and tempered steel for high-sulfur controlled phosphorus crankshaft and a low-cost production method thereof

By using pyrite to regulate sulfur and blowing nitrogen to stir and deploy nitrogen in crankshaft production, the problem of high cost and sulfide inclusions in traditional non-quenched and tempered steel materials has been solved, and the low cost of non-quenched and tempered steel for high-sulfur and phosphorus-controlled crankshafts has been achieved. Cost-effective production and excellent cutting performance.

CN116240450BActive Publication Date: 2024-10-01JIANGYIN XINGCHENG SPECIAL STEEL WORKS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211536068.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-02
Publication Date
2024-10-01
Estimated Expiration
2042-12-02

AI Technical Summary

Technical Problem

In the production process of traditional non-quenched and tempered steel materials for crankshafts, the deployment cost of sulfur and nitrogen elements is high, and the presence of sulfide inclusions seriously deteriorates the quality of molten steel, affecting the cutting performance and production cost of the material.

Method used

By using pyrite to regulate sulfur in steel during the electric furnace smelting and refining process, and blowing nitrogen to stir and prepare nitrogen during the VD vacuum degassing process, the S and P content in the molten steel is controlled to ensure the stability of sulfur recovery and nitrogen Element distribution, using the production process of electric furnace smelting, electric furnace tapping, refining, VD vacuum degassing, continuous casting, heating, rolling and cooling, to prepare non-quenched and tempered steel for high-sulfur and phosphorus-controlled crankshafts.

Benefits of technology

It significantly reduces the material manufacturing cost, improves the easy-cutting performance of the crankshaft, reduces the generation of sulfide inclusions, and improves the cutting performance of steel and the surface quality of the workpiece.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003977714150000011
    Figure HDA0003977714150000011
  • Figure HDA0003977714150000021
    Figure HDA0003977714150000021
  • Figure HDA0003977714150000022
    Figure HDA0003977714150000022
Patent Text Reader

Abstract

The present invention relates to a non-quenched and tempered steel for a high-sulfur controlled phosphorus crankshaft and a low-cost production method thereof. The chemical composition mass percentage of the steel is C: 0.34-0.41%, Si: 0.15-0.80%, Mn: 1.20-1.65%, P: 0.020-0.035%, S: 0.060-0.090%, Cr: 0.10-0.30%, Al: 0.020-0.040%, Ti: ≤0.005%, V: 0.10-0.15%, N: 0.010-0.015%, and the balance is Fe and inevitable impurity elements. The S is added and regulated during molten steel smelting with pyrite as the source. Process: (1) electric furnace smelting→(2) refining→(3) VD vacuum degassing→(4) continuous casting→(5) heating→(6) rolling→(7) cooling. By controlling the S and P content in molten steel, the cutting performance of crankshaft products is improved and the manufacturing cost is greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alloy materials, and in particular relates to non-quenched and tempered steel for crankshafts and a production method thereof. Background Art

[0002] The crankshaft is one of the five core components of an internal combustion engine, and its production cost has a great impact on the overall production cost of the internal combustion engine. The production cost of the crankshaft involves raw materials, forging and machining, of which machining costs account for nearly 70%. At the same time, with the development of the machining industry towards high-speed, automated and unmanned operation and the increasing production volume, non-quenched and tempered steel for crankshafts with better machinability has become a product in market demand.

[0003] The sulfur content of traditional non-quenched and tempered steel materials for crankshafts is between 0.015% and 0.060%, and the chip breaking and chip removal capabilities are insufficient during the machining process of the crankshaft. Crankshaft steels with a phosphorus content greater than 0.060% and controlled phosphorus content are rarely seen on the market.

[0004] In addition, in the current production process of non-quenched and tempered steel materials for sulfur-containing crankshafts, the mixing of sulfur and nitrogen elements is usually regulated by adding high-cost materials such as sulfur-iron alloys, sulfur-containing pig iron, sulfur (sulfur) wire, vanadium-nitrogen alloys and nitrogen-manganese wire, etc., which results in high material costs.

[0005] The Chinese patent with the authorization announcement number CN 101613782 B and the announcement date of February 9, 2011, entitled "A method for producing non-quenched and tempered steel containing nitrogen and sulfur", discloses a method for producing non-quenched and tempered steel containing nitrogen and sulfur. No VD vacuum treatment is performed during the production process of the steel. The sulfur content in the final steel is 0.050-0.010%, and the S content is all controlled by adding the sulfur (sulfur) line at the end of refining, which not only has high production costs, but also seriously deteriorates the quality of the molten steel and produces more sulfide inclusions. The nitrogen content is 0.010-0.020%, and the nitrogen element is controlled by blowing nitrogen during the refining process. Considering the instability of recovery, one or more precious alloys of manganese nitride, vanadium nitride or chromium nitride are added for final matching, which has high production costs.

[0006] The Chinese patent with the authorization announcement number CN 110714161 B and the announcement date of September 22, 2020, entitled "A high-sulfur free-cutting steel for automobiles and its production process", discloses a high-sulfur free-cutting steel and its production process. The chemical composition of the steel is as follows: C0.15-0.19%, Si 0.20-0.30%, Mn 1.20-1.30%, P≤0.035%, S0.080-0.12%, Ni 0.12-0.18%, Ti 0.010-0.025%, and the balance is Fe and unavoidable impurities. The sulfur element in the steel is added to the high-sulfur pig iron during the electric furnace smelting process, and the material cost is high.

[0007] The Chinese patent document with application publication number CN 110016613 A, publication date 2019.07.06, and titled “A sulfur-containing automobile crankshaft steel and preparation method thereof” discloses a sulfur-containing automobile crankshaft steel, the chemical composition of which is as follows by mass percentage: C 0.40-0.44%, Si 0.15-0.35%, Mn 0.60-0.80%, P≤0.020%, S0.015-0.030%, Cr 1.05-1.25%, Mo 0.15-0.25%, Al≤0.060%, Ni≤0.30%, Cu≤0.30%, Pb≤0.020%, Sn≤0.030%, and the rest are Fe and unavoidable impurities. The sulfur element is prepared by using ferrosulfur alloy or sulfur (sulfur) wire, and is added after the VD vacuum treatment to adjust the S content in the molten steel. Not only is the material cost high, but adding a large amount at the end of the steelmaking process will seriously deteriorate the purity of the molten steel. Summary of the invention

[0008] The present invention provides a non-quenched and tempered steel for a high-sulfur and controlled-phosphorus crankshaft and a low-cost production method thereof, which improves the easy-cutting processing performance of the crankshaft product by controlling the contents of S and P in molten steel and greatly reduces the manufacturing cost.

[0009] The technical solution adopted by the present invention to solve the above problems is: a non-quenched and tempered steel for a high-sulfur controlled phosphorus crankshaft, the chemical composition of the steel is C: 0.34-0.41%, Si: 0.15-0.80%, Mn: 1.20-1.65%, P: 0.020-0.035%, S: 0.060-0.090%, Cr: 0.10-0.30%, Al: 0.020-0.040%, Ti: ≤0.005%, V: 0.10-0.15%, N: 0.010-0.015%, and the balance is Fe and unavoidable impurity elements, wherein the S is added and regulated during smelting of molten steel using pyrite as the source.

[0010] Preferably, the chemical composition of the steel in percentage by mass is C: 0.37-0.39%, Si: 0.65-0.72%, Mn: 1.45-1.55%, S: 0.075-0.085%, P: 0.025-0.035%, Cr: 0.18-0.25%, Al: 0.025-0.035%, V: 0.11-0.13%, N: 0.012-0.015%, and the remainder is Fe and unavoidable impurity elements.

[0011] Based on the above chemical composition design, pyrite is used to adjust the sulfur element in the steel during electric furnace smelting, electric furnace steelmaking and refining. At the same time, attention should be paid to the slag basicity of the electric furnace oxidation slag and the refining reduction slag to ensure the stability of sulfur recovery. At the same time, nitrogen is blown and stirred throughout the VD vacuum process to adjust the nitrogen element in the steel to ensure the smooth smelting of the molten steel with the above composition.

[0012] The element design of the non-quenched and tempered steel for high-sulfur controlled phosphorus crankshaft of the present invention is determined as follows:

[0013] C is the most basic and effective strengthening element in steel. It contributes the most to strength and hardness and has the most economical use cost. Considering that the crankshaft surface needs to be treated with medium-frequency induction quenching, in order to ensure that the material has sufficient strength / hardness and hardenability while taking into account a certain plasticity, C is determined to be 0.34~0.41%, and C is preferably 0.37~0.39%.

[0014] Si can be used as a deoxidizer and reducing agent in the steelmaking process, and improves the strength of the steel in the form of solid solution strengthening. It can significantly strengthen ferrite and significantly improve the yield strength. However, too high a content will reduce the cold working performance of the steel. Si is determined to be 0.15-0.80%, and Si is preferably 0.65-0.72%.

[0015] Mn is an effective element for deoxidation and desulfurization in steel. It improves the strength and hardness of steel while significantly improving the hardenability of steel and improving the hot processing performance of steel. At the same time, Mn is the element with the strongest binding force with S in steel, and the formed MnS compound helps to improve the cutting performance of steel. Mn is determined to be 1.20-1.65%, and Mn is preferably 1.45-1.55%.

[0016] P is usually a harmful impurity in steel, but it is an element that can be integrated into a solid solution (such as ferrite) and can make the matrix embrittled to facilitate cutting. P is determined to be 0.020-0.035%, preferably P: 0.025~0.035%.

[0017] S is usually also a harmful impurity in steel, but it can significantly improve the cutting performance of steel. Its effect of improving the machinability of steel is very significant. It can significantly increase the life of the tool and reduce the surface roughness of the workpiece. S is determined to be 0.060-0.090%, and S is preferably 0.075-0.085%.

[0018] Cr can effectively improve the hardenability of steel to obtain the required strength and reduce the tendency of surface decarburization during heating of steel. However, since it is a strong carbide precipitation element, it will affect the performance of the induction quenching layer. Therefore, the content cannot be too high. It is determined that: Cr: 0.10~0.30%, preferably Cr: 0.18~0.25%.

[0019] Al is an effective deoxidizer. The AlN formed can refine the grains. When the content is low, the effect is not obvious. When the content is high, it is easy to form coarse inclusions and deteriorate the performance of the steel. The Al content is determined to be 0.020-0.040%. The preferred Al content is 0.025-0.035%.

[0020] V has a high solubility in steel and is one of the most commonly used and most effective strengthening elements for non-quenched and tempered steel. It exists in steel mainly in the form of V carbonitride compounds. It affects the structure and properties of steel by forming V (C, N) compounds that precipitate at grain boundaries, thereby refining ferrite grains and improving the strength and toughness of steel. V is a precious alloy. In order to ensure that the steel has a reasonable cost-effectiveness, V is determined to be 0.10-0.15%, and V is preferably 0.11-0.13%.

[0021] N is a common element in non-quenched and tempered steels. It is mainly used to enhance the precipitation strengthening effect and refine the grains. Adding appropriate N to the steel expands the precipitation range of carbonitrides and improves the effective effect of microalloying elements. The same mechanical properties can be obtained with a smaller content of microalloying elements. N is determined to be 0.010-0.015%, and preferably N is 0.012-0.015%.

[0022] Another object of the present application is to provide a method for producing the above-mentioned non-quenched and tempered steel, the process of which is as follows: (1) electric furnace smelting → (2) refining → (3) VD vacuum degassing → (4) continuous casting → (5) heating → (6) rolling → (7) cooling. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The chemical composition of the non-quenched and tempered steel for the crankshaft of Examples 1 and 2 of the present invention;

[0024] Figure 2 This is a state diagram of sulfide inclusions in the non-quenched and tempered steel for crankshafts according to Example 1 of the present invention;

[0025] Figure 3 This is a state diagram of sulfide inclusions in non-quenched and tempered steel for crankshafts according to Example 2 of the present invention;

[0026] Figure 4 This is the chip machining effect of the crankshaft forged from steel obtained in Examples 1 and 2 of the present invention. DETAILED DESCRIPTION

[0027] The present invention is further described in detail below in conjunction with examples. The examples are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0028] Use Figure 1 Two batches of non-quenched and tempered steel for crankshafts were produced with the chemical composition shown, corresponding to Examples 1-2.

[0029] The non-quenched and tempered steel for the crankshaft with low cost and high sulfur and controlled phosphorus in the embodiment of the present invention is manufactured according to the following production process

[0030] Electric furnace smelting

[0031] Scrap steel and molten iron are used as raw materials, wherein the molten iron contains 0.025% sulfur and 0.10% phosphorus, and 250kg±20kg of pyrite containing 45% sulfur is added at a recovery rate of 45%; the binary basicity of the oxide slag CaO / SiO2 during the smelting process is controlled to be 1.7-2.2, so as to ensure that the electric furnace steelmaking target is more than 0.025% phosphorus and more than 0.050% sulfur; when the electric furnace steelmaking is conducted, 60kg±5kg of pyrite containing 45% sulfur is added with the steel flow at a recovery rate of 65%, and P brought into by other ferroalloys is considered to ensure that the refining target is 0.030% phosphorus and 0.065% sulfur (that is, P and S must be respectively greater than the specified contents when refined).

[0032] Refining

[0033] The binary basicity of CaO / SiO2 in the reducing slag during the refining process is controlled at 3.5-4.0. At the end of refining (before hanging the bag), 30kg-40kg of pyrite containing 45% sulfur is added at a recovery rate of 75% to ensure that the VD target is 0.030% phosphorus (0.025% P is the preferred lower limit. Considering the mixed flushing of steel slag during the VD treatment process, there will be a small loss of P, so the VD target P is controlled to be above 0.030%) and the sulfur is controlled at 0.075-0.085%.

[0034] The difference in the amount of pyrite added leads to the difference in the S content in the final product. The difference in the P content in the final product mainly depends on the content added in the raw materials and the content brought in from other ferroalloys. The P content is mainly affected by the addition of high-carbon ferromanganese and high-carbon ferrochrome. When using the aforementioned alloys to adjust the manganese and chromium content in the molten steel, P is introduced incidentally to increase the P content in the molten steel.

[0035] VD Vacuum Degassing

[0036] During the vacuum treatment, nitrogen is blown and stirred throughout the process to adjust the nitrogen element in the steel. The nitrogen pressure is controlled at 0.4MPa and the flow rate is controlled at 400NL / min. During soft blowing, argon stirring is switched. The final N content in the steel is mainly determined by the length of soft blowing time.

[0037] Continuous Casting

[0038] A 300mm×300mm square continuous casting machine was used for casting, and the casting superheat was controlled at 20-35℃. The secondary cooling weak cooling water volume was 0.16L / kg. Electromagnetic stirring (2Hz / 150A) of the crystallizer and electromagnetic stirring (20Hz / 200A) of the end were used to improve the surface and internal quality of the ingot.

[0039] Heating before rolling

[0040] Use a walking beam heating furnace to heat the ingot, with the temperature of the preheating section controlled at 650-800℃, the temperature of the heating section controlled at 950-1050℃, the temperature of the soaking section controlled at 1120-1180℃, and the total heating time of 260-330min, of which the preheating section time must be ≥120min to ensure that the ingot heats up slowly and is heated sufficiently and evenly.

[0041] Rolling

[0042] After the ingot leaves the heating furnace, it is descaled with high-pressure water, the starting rolling temperature is 1000-1020℃, and then it is rolled using 6 primary rolling mills + 6 intermediate rolling mills + 6 finishing rolling mills, with the final rolling temperature controlled at 920-950℃; the maximum rolling specification of round steel is φ100mm.

[0043] cool down

[0044] After rolling, place the stepping cooling bed on the cooling bed and control the stepping speed to achieve a round steel cooling rate of 0.6-1.0℃ / s to ensure that the temperature of the lower cooling bed is ≤520℃.

[0045] Combination Figure 2 , 3 In the two embodiments, the final sulfide inclusions in the steel are basically spindle-shaped, discontinuous and evenly distributed, and the aspect ratio of the sulfide is ≤8.

[0046] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.

Claims

1. A non-quenched and tempered steel for a high-sulfur and controlled-phosphorus crankshaft, characterized in that: The chemical composition of the steel is C: 0.34-0.41%, Si: 0.15-0.80%, Mn: 1.20-1.65%, P: 0.020-0.035%, S: 0.060-0.090%, Cr: 0.10-0.30%, Al: 0.020-0.040%, Ti: ≤0.005%, V: 0.10-0.15%, N: 0.010-0.015%, and the balance is Fe and unavoidable impurity elements, wherein the S is added and regulated during molten steel smelting with pyrite as the source; the production method of the steel comprises: Step 1: Electric furnace smelting Use scrap steel and molten iron as raw materials, wherein the molten iron contains more than 0.025% sulfur and more than 0.10% phosphorus, and add 250kg± (0-20kg) of pyrite containing 45% sulfur at a recovery rate of 45%; control the binary basicity of CaO / SiO2 of the oxide slag during the smelting process at 1.7-2.2 to ensure that the target of electric furnace steel tapping is more than 0.025% phosphorus and more than 0.050% sulfur; when the electric furnace is tapping, add 60kg± (0-5kg) of pyrite containing 45% sulfur with the steel flow at a recovery rate of 65%, considering the P brought into other ferroalloys, to ensure that the refining target is more than 0.030% phosphorus and more than 0.065% sulfur; Step 2: Refining The CaO / SiO2 binary basicity of the reducing slag in the refining process is controlled at 3.5-4.

0. At the end of refining, 30kg-40kg of pyrite containing 45% sulfur is added at a recovery rate of 75%, ensuring that the VD target is above 0.030% phosphorus and 0.075-0.085% sulfur; Step 3: VD vacuum degassing During the whole process of vacuum degassing, nitrogen is blown to stir the molten steel to increase nitrogen in the molten steel, and argon is switched to stir during soft blowing; Step 4: Continuous Casting The continuous casting process is used to cast square continuous casting billets of more than 300mm×300mm, and the casting superheat is controlled at 20-35℃. The continuous casting secondary cooling zone is weakly cooled. The continuous casting process uses electromagnetic stirring of the crystallizer and electromagnetic stirring at the end to improve the surface and internal quality of the billet. Step 5: Heating For heating of the ingot, the temperature of the preheating section is controlled at 650-800°C, the temperature of the heating section is controlled at 950-1050°C, the temperature of the soaking section is controlled at 1120-1180°C, and the total heating time is 260-330 minutes, of which the preheating time is ≥120 minutes; Step 6: Rolling After the ingot leaves the heating furnace, it is descaled with high-pressure water, and the rolling temperature is set at 1000-1020°C. Six primary rolling mills, six intermediate rolling mills, and six finishing rolling mills are used for rolling, and the final rolling temperature is 920-950°C. The ingot is rolled into round steel with specifications of φ80-100mm. Step 7: Cooling After rolling, the round steel is placed on the cooling bed, and the step speed is controlled to meet the cooling rate of 0.6-1.0℃ / s to ensure that the temperature of the lower cooling bed is ≤520℃.

2. The high-sulfur and phosphorus-controlled non-quenched and tempered steel for crankshaft according to claim 1, characterized in that: The chemical composition of steel in mass percentage is C: 0.37~0.39%, Si: 0.65~0.72%, Mn: 1.45~1.55%, S: 0.075~0.085%, P: 0.025-0.035%, Cr: 0.18~0.25%, Al: 0.025~0.035%, V: 0.11~0.13%, N: 0.012~0.015%, and the balance is Fe and unavoidable impurity elements.

3. The non-quenched and tempered steel for high-sulfur and controlled-phosphorus crankshaft according to claim 1, characterized in that: The sulfide inclusions in the steel are spindle-shaped, discontinuous and evenly distributed, and the aspect ratio of the sulfide is ≤8.

4. The high-sulfur and phosphorus-controlled non-quenched and tempered steel for crankshaft according to claim 1, characterized in that: In step 4, the weak cooling water volume of the second cooling zone is 0.16 L / kg, the frequency / current of the electromagnetic stirring of the crystallizer is 2 Hz / 150 A, and the frequency / current of the terminal electromagnetic stirring is 20 Hz / 200 A.