A Ti-Zr-Nb-Sn alloy with high elastic-thermal effect and preparation method thereof
By optimizing the alloy composition and heat treatment process, a high elastic thermal effect Ti-Zr-Nb-Sn alloy was prepared, which solved the problems of the existing alloy's adiabatic temperature decrease and the critical stress, and achieved efficient solid-state refrigeration performance, suitable for new models Elastic thermal refrigeration material.
Patent Information
- Application Number
- CN202211106266.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-09-10
AI Technical Summary
The adiabatic temperature of the existing Ti-Zr-Nb-Sn alloys becomes smaller under uniaxial loading and unloading stresses, and the critical stress of driving phase transition is large, which cannot meet the needs of solid-state refrigeration applications.
By optimizing the alloy composition and changing the heat treatment process, the oligocrystal microstructure and strong crystallographic texture are obtained to suppress the precipitation of harmful phases during cooling. High vacuum smelting, annealing heat treatment and extremely fast cooling processes are used to prepare high elastic thermal effect Ti-Zr- Nb-Sn alloy.
The high elastic thermal effect of Ti-Zr-Nb-Sn alloy is achieved, with a larger adiabatic temperature, low critical stress, small stress hysteresis, and good elastic thermal cycle stability, meeting the needs of solid state refrigeration applications.
Smart Images

Figure CN116254430B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of elasto-caloric solid-state refrigeration, and relates to a Ti-Zr-Nb-Sn alloy with high elasto-caloric effect and a preparation method thereof.
[0002] Background
[0003] As the global demand for refrigeration gradually increases, the proportion of refrigeration energy consumption in global electricity has exceeded 20%. However, traditional vapor compression refrigeration technology cannot meet the future requirements for energy consumption and environmental protection. Therefore, the development of new refrigeration technology is urgent. In recent years, solid-state refrigeration technology based on elastocaloric effect has been considered to be the most promising non-gas-liquid compression refrigeration technology due to its advantages such as zero room temperature gas emission, simple actual operation, low application cost and good conversion efficiency. The first-order martensitic phase transformation of shape memory alloys is accompanied by huge latent heat of phase transformation. Under the action of uniaxial loading and unloading stress, reversible heat exchange with the outside world occurs to achieve refrigeration effect. It is one of the most common elastocaloric solid-state refrigeration materials.
[0004] Metastable β-type Ti-based shape memory alloys are widely used in the biomedical field due to their low elastic modulus, good biocompatibility and high corrosion resistance. Although existing Ti-Zr-Nb-Sn alloys also exhibit elasto-caloric effect under uniaxial loading and unloading stress, the adiabatic temperature change of the elasto-caloric effect is small, and the critical stress for driving the phase change is large, which cannot meet the application requirements of solid-state refrigeration and is not suitable as elasto-caloric solid-state refrigeration materials. Therefore, achieving high elasto-caloric effect and low critical stress of Ti-Zr-Nb-Sn alloys is of great significance in promoting the development and application of elasto-caloric solid-state refrigeration. In view of the above-mentioned problems, it is very necessary to study and design a new method for preparing Ti-Zr-Nb-Sn alloys with high elasto-caloric effect to solve the problems existing in the existing elasto-caloric refrigeration technology. Summary of the invention
[0005] The present invention proposes a method for preparing a Ti-Zr-Nb-Sn alloy with high elastic-caloric effect to solve the problems of poor elastic-caloric effect and high critical stress in the existing Ti-Zr-Nb-Sn alloy. The method optimizes the alloy composition and changes the heat treatment process to obtain oligocrystalline microstructure and strong crystallographic texture and inhibit the precipitation of harmful phases during the cooling process, thereby achieving high elastic-caloric effect with excellent comprehensive performance, making the Ti-Zr-Nb-Sn alloy a new type of elastic-caloric refrigeration material with excellent performance.
[0006] The present invention provides a method for preparing a Ti-Zr-Nb-Sn alloy with high elastic-thermal effect, comprising the following steps:
[0007] S1. configuring raw materials according to the atomic percentage of Ti-Zr-Nb-Sn alloy;
[0008] S2. The raw materials configured in step S1 are subjected to high vacuum melting to obtain an alloy ingot having a uniform composition;
[0009] S3. The alloy ingot prepared in step S2 is subjected to annealing heat treatment in a high vacuum or inert gas protection environment;
[0010] S4. The alloy ingot after the heat treatment in step S3 is quenched by using an extremely rapid cooling process to obtain the Ti-Zr-Nb-Sn alloy with a β single phase.
[0011] Preferably, in step S1, the general chemical formula of the Ti-Zr-Nb-Sn alloy is Ti 97-x-y Zr x Nb y Sn3, and 16≤x≤20, 10≤y≤12.
[0012] Preferably, in step S1, the general chemical formula of the Ti-Zr-Nb-Sn alloy is Ti 68 Zr 18 Nb 11 Sn3.
[0013] Preferably, in step S1, Ti, Zr, Nb, Sn metal raw materials with a purity higher than 99.9% are configured according to the atomic percentage of the Ti-Zr-Nb-Sn alloy.
[0014] Preferably, in step S2, the vacuum degree is drawn to 1×10 -2 Pa, high-purity Ar gas was introduced for gas washing and repeated several times; after the gas washing was completed, the vacuum degree was drawn to 3×10 -3 Pa, prepare to smelt the raw materials; before smelting the raw materials, melt the high-purity titanium ingot in a high-purity Ar gas environment and cool it to remove the residual oxygen in the furnace.
[0015] Preferably, in step S2, the raw material is turned over no less than 4 times during the smelting process, and magnetic stirring is applied during the smelting process to ensure the composition uniformity of the alloy ingot.
[0016] Preferably, in step S2, during the alloy smelting process, the smelting furnace is cooled by circulating water, and the circulating water temperature is 20-25°C.
[0017] Preferably, in step S3, the high-purity inert gas includes any one of helium and argon with a purity of more than 99.99%, or a combination of the two.
[0018] Preferably, in step S3, the annealing heat treatment temperature is 900-1100° C., and the annealing time is 2-6 hours.
[0019] Preferably, in step S4, the alloy ingot after heat treatment is subjected to extreme rapid quenching in ice-salt water.
[0020] The beneficial effect of the present invention is that the Ti-Zr-Nb-Sn alloy with high elastocaloric effect prepared by the present invention not only has a large adiabatic temperature change, but also has the advantages of low critical stress, small stress hysteresis and good elastocaloric cycle stability, etc., which meets the application requirements of elastocaloric solid-state refrigeration and is an elastocaloric refrigeration material with great development potential.
[0021] The invention discloses a method for preparing a Ti-Zr-Nb-Sn alloy with high elasto-caloric effect. By optimizing the alloy composition and changing the heat treatment process, the Ti-Zr-Nb-Sn alloy obtains an oligocrystalline microstructure and a strong crystallographic texture. The method also suppresses the precipitation of harmful phases during the cooling process, thereby realizing the high elasto-caloric effect of the Ti-Zr-Nb-Sn alloy. The method has important guiding significance for optimizing the elasto-caloric properties of elasto-caloric refrigeration materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Ti prepared in Example 1 of the present invention 68 Zr 18 Nb 11 SEM image of Sn3 alloy grains.
[0023] Figure 2 Ti prepared in Example 1 of the present invention 68 Zr 18 Nb 11 DSC curve of Sn3 alloy.
[0024] Figure 3 Ti prepared in Example 1 of the present invention 68 Zr 18 Nb 11 Stress-strain curve of Sn3 alloy.
[0025] Figure 4 Ti prepared in Example 1 of the present invention 68 Zr 18 Nb 11 Temperature variation diagram of Sn3 alloy under adiabatic unloading. DETAILED DESCRIPTION
[0026] The following embodiments of the present invention are described in further detail in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0027] Example 1
[0028] S1. The Ti, Zr, Nb, Sn metal raw materials with a purity higher than 99.9% are68 Zr 18 Nb 11 The atomic percentage of Sn3 alloy is configured.
[0029] S2. Place the raw materials prepared in step S1 in a high vacuum arc melting furnace for melting. First, draw the vacuum degree to 1×10 -2 Pa, and then introduce high-purity Ar gas for gas washing and repeat several times, and then draw the vacuum degree to 3×10 -3 Pa or less, prepare the raw materials for smelting. Before smelting the raw materials, melt the high-purity titanium ingots in a high-purity Ar gas protection environment and cool them to remove the residual oxygen in the furnace. In order to ensure the uniformity of the composition of the alloy ingots, the raw materials are turned over no less than 4 times during the smelting process, and magnetic stirring is applied during the smelting process. During the alloy smelting process, the smelting furnace is cooled by circulating water, and the circulating water temperature is 20°C.
[0030] S3. The alloy ingot obtained in step S2 is sealed in a high-purity Ar gas protection environment, and then placed in a box-type annealing furnace preheated to 1000° C. for annealing for 2 h;
[0031] S4. The alloy ingot that has completed the annealing treatment in step S3 is subjected to an extremely rapid quenching treatment in ice salt water.
[0032] The final Ti-Zr-Nb-Sn alloy with high elasto-caloric effect was obtained. The adiabatic temperature change was measured to be 10.7K, the critical stress driving the phase change was 50MPa, the stress hysteresis was 12MPa, and it maintained good stability during 2000 elasto-caloric cycles. Figure 1 The Ti prepared in this example 68 Zr 18 Nb 11 SEM image of grains of Sn3 alloy; Figure 2 The Ti prepared in this example 68 Zr 18 Nb 11 DSC curve of Sn3 alloy; Figure 3 The Ti prepared in this example 68 Zr 18 Nb 11 Stress-strain curve of Sn3 alloy; Figure 4 The Ti prepared in this example 68 Zr 18 Nb 11 Temperature variation diagram of Sn3 alloy under adiabatic unloading.
[0033] Example 2
[0034] The difference between this embodiment and embodiment 1 is that in step S3, the alloy ingot is placed in a box-type annealing furnace preheated to 1100° C. for annealing for 2 hours. The rest is the same as embodiment 1.
[0035] The adiabatic temperature change of the finally obtained Ti-Zr-Nb-Sn alloy with high elasto-caloric effect was measured to be 9.4K, the critical stress driving the phase transition was 100MPa, and the stress hysteresis was 20MPa.
[0036] Example 3
[0037] The difference between this embodiment and embodiment 1 is that in step S3, the alloy ingot is placed in a box-type annealing furnace preheated to 900° C. for annealing for 6 hours. The rest is the same as embodiment 1.
[0038] The adiabatic temperature change of the finally obtained Ti-Zr-Nb-Sn alloy with high elasto-caloric effect was measured to be 8.4K, the critical stress driving the phase transition was 75MPa, and the stress hysteresis was 15MPa.
[0039] Example 4
[0040] The difference between this embodiment and embodiment 1 is that step S1 is based on Ti 67 Zr 20 Nb 10 The atomic percentage of Sn3 alloy is the same as that of Example 1.
[0041] The adiabatic temperature change of the finally obtained Ti-Zr-Nb-Sn alloy with high elasto-caloric effect was measured to be 10.2K, the critical stress driving the phase transition was 80MPa, and the stress hysteresis was 19MPa.
[0042] Example 5
[0043] The difference between this embodiment and embodiment 1 is that step S1 is based on Ti 69 Zr 16 Nb 12 The atomic percentage of Sn3 alloy is the same as that of Example 1.
[0044] The adiabatic temperature change of the finally obtained Ti-Zr-Nb-Sn alloy with high elasto-caloric effect was measured to be 9.5K, the critical stress driving the phase transition was 108MPa, and the stress hysteresis was 30MPa.
[0045] Comparative Example 1
[0046] The alloy in this comparative example is the same as that in Example 1, which is Ti 68 Zr 18 Nb 11 Sn3, but this comparative example adopts the existing technology to prepare the alloy, and the preparation method specifically includes:
[0047] S1. The method of obtaining the alloy ingot is exactly the same as that of steps S1 and S2 of Example 1, and Ti is obtained. 68 Zr 18 Nb 11 Sn3 alloy ingot;
[0048] S2. The alloy ingot obtained in step S1 is cut into a rectangular ingot having a thickness of 8 mm by a wire-cut electric discharge machine, and the surface oxide layer is removed by sandpaper polishing;
[0049] S3. The rectangular ingot after grinding in step S2 is repeatedly cold-rolled at room temperature for several times, with a cumulative cold-rolling reduction of 96%, and a 0.3 mm thick plate is obtained after grinding the surface oxide layer;
[0050] S4. The cold-rolled sheet sample obtained in step S3 is sealed in an Ar environment, and then annealed at 650° C. for 10 min.
[0051] S5. The sample heat treated in S4 is water quenched at room temperature.
[0052] The adiabatic temperature change of the Ti-Zr-Nb-Sn alloy finally obtained was measured to be 2.8K, the critical stress driving the phase transition was 120MPa, and the stress hysteresis was 110MPa.
[0053] Table 1 below shows a comparison of the caloric elastic properties of the Ti-Zr-Nb-Sn alloy caloric elastic materials prepared by Examples 1-5 and Comparative Example 1.
[0054] Table 1 Performance comparison of various embodiments
[0055] Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Adiabatic temperature change / K 10.7 9.4 8.4 10.2 9.5 2.8 Critical stress / MPa 50 100 75 80 108 120 Stress hysteresis / MPa 12 20 15 19 30 110
[0056] Compared with the Ti-Zr-Nb-Sn alloy prepared by the prior art in Comparative Example 1, the elastocaloric effect of the Ti-Zr-Nb-Sn alloys provided in Examples 1-5 is greatly improved, and the adiabatic unloading temperature change value can reach up to 10.7 K. At the same time, the Ti-Zr-Nb-Sn alloys provided in Examples 1-5 also have the advantages of low stress driving field, small stress hysteresis and excellent elastocaloric cycle stability, which meet the application requirements of solid-state refrigeration and are elastocaloric refrigeration materials with great development potential.
[0057] The embodiments of the present invention are given for the purpose of illustration and description, and are not intended to be exhaustive or to limit the invention to the disclosed forms. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described in order to better illustrate the principles and practical applications of the present invention and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for specific uses.
Claims
1. A method for preparing a Ti-Zr-Nb-Sn alloy with high elastic thermal effect, characterized in that: The steps include: S1. According to the atomic percentage configuration of the raw materials of the Ti-Zr-Nb-Sn alloy; the chemical formula of the Ti-Zr-Nb-Sn alloy is Ti 97-x-y Zr x Nb y Sn3, with 16 ≤ x ≤ 20, 10 ≤ y ≤ 12; S2. The raw materials configured in step S1 are subjected to high vacuum melting to obtain an alloy ingot having a uniform composition; S3. The alloy ingot prepared in step S2 is subjected to annealing heat treatment in a high vacuum or inert gas environment; S4. The alloy ingot after the heat treatment in step S3 is quenched by using an extremely rapid cooling process to obtain the Ti-Zr-Nb-Sn alloy having a β single phase.
2. The method for preparing a Ti-Zr-Nb-Sn alloy with high elasto-thermal effect according to claim 1, characterized in that: In step S1, the chemical formula of the Ti-Zr-Nb-Sn alloy is Ti 68 Zr 18 Nb 11 Sn3.
3. The method for preparing a Ti-Zr-Nb-Sn alloy with high elasto-thermal effect according to claim 1, characterized in that: In step S2, the vacuum degree is first drawn to 1×10 -2 Pa, high-purity Ar gas was introduced for gas washing and repeated several times; after the gas washing was completed, the vacuum degree was drawn to 3×10 -3 Pa, prepare to smelt the raw materials; before smelting the raw materials, melt the high-purity titanium ingot in a high-purity Ar gas environment and cool it to remove the residual oxygen in the furnace.
4. The method for preparing a Ti-Zr-Nb-Sn alloy with high elasto-thermal effect according to claim 1, characterized in that: In step S2, the raw material is turned over for no less than 4 times during the smelting process, and magnetic stirring is applied during the smelting process.
5. The method for preparing a Ti-Zr-Nb-Sn alloy with high elasto-thermal effect according to claim 1, characterized in that: In step S2, during the alloy smelting process, the smelting furnace is cooled by circulating water, and the circulating water temperature is 20-25°C.
6. The method for preparing a Ti-Zr-Nb-Sn alloy with high elasto-thermal effect according to claim 1, characterized in that: In step S3, the inert gas includes any one of helium and argon with a purity of more than 99.99%, or a combination of the two.
7. The method for preparing a Ti-Zr-Nb-Sn alloy with high elasto-thermal effect according to claim 1, characterized in that: In the step S3, the annealing heat treatment temperature is 900-1100°C, and the annealing time is 2-6 hours.
8. The method for preparing a Ti-Zr-Nb-Sn alloy with high elasto-thermal effect according to claim 1, characterized in that: In the step S4, the alloy ingot after heat treatment is extremely rapidly quenched in ice-salt water.
9. A Ti-Zr-Nb-Sn alloy with high elasto-thermal effect prepared by the preparation method according to any one of claims 1 to 8.