A high yield strength cast Al-Si alloy and preparation method thereof

By adjusting the proportion of elements such as Si, Mg, Cu, Zn in the Al-Si casting alloy, and combining die-casting process and aging treatment, the problem of insufficient yield strength of the existing Al-Si casting alloy is solved, achieving high strength and high strength Cast Al-Si alloy with elongation, suitable for a variety of use states.

CN116254442BActive Publication Date: 2024-11-19SHENYANG AEROSPACE UNIVERSITY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202211671475.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-26
Publication Date
2024-11-19
Estimated Expiration
2042-12-26

AI Technical Summary

Technical Problem

The existing Al-Si cast alloys have insufficient yield strength under high Mg content, which is difficult to meet the needs of high strength and high elongation. The heat treatment process may lead to deformation of the castings, and the strength of non-heat treatment alloys is difficult to improve.

Method used

Si: 9.0-12.5%, Mg: 0.3-0.8%, Cu: 0.2-1.6%, Zn: 0.2-1.6%, Mn: 0-1.0%, Fe≤0.5%, Zr: 0-0.25%, Ti: Al-Si alloy with composition ratio of 0.05-0.25%, Cr: 0-0.25%, Re: 0-0.3%, Sr: 0.02-0.2%, and improved by die-casting process and aging treatment (T4, T5, T6 states) Strength and plasticity.

Benefits of technology

In the cast state, the room temperature tensile strength is achieved 289-336MPa, the yield strength is 132-187MPa, the elongation is 7.3-10.8%, the tensile strength is 335-385MPa, the yield strength is 243-278MPa, the elongation is 5.1-8.9%, At the same time, the negative impact of the relative elongation of eutectic Si is reduced and the mechanical properties of the alloy is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a high yield strength cast Al-Si alloy and a preparation method thereof. The cast Al-Si alloy comprises components and mass percentages of Si: 9.0-12.5%, but not equal to 9.0%, Mg: 0.3-0.8%, Cu: 0.2-1.6%, Zn: 0.2-1.6%, Mn: 0-1.0%, Fe≤0.5%, Zr: 0-0.25%, Ti: 0.05-0.25%, Cr: 0-0.25%, Re: 0-0.3%, Sr: 0.02-0.2%, and the balance is Al and unavoidable impurities. The total impurity content in the alloy is ≤1.0%, and the content of a single impurity is ≤0.15%. The ratio of each alloy element in the present invention makes the alloy have high strength and maintains high plasticity; the present invention increases the Si content and Mg content of the alloy, and at the same time, the alloy contains higher Cu and Zn, which enhances the solid solution strengthening effect of the alloy in the cast state and enhances the aging strengthening effect of the alloy in the aging state, improves the plasticity of the alloy, and reduces its negative impact on the elongation of the alloy; at the same time, other alloy elements are introduced to further increase the solid solution strengthening effect in the alloy, and effectively improve the strength and plasticity of the alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of cast aluminum alloys, and in particular relates to a high yield strength cast Al-Si alloy and a preparation method thereof. Background Art

[0002] In Al-Si casting alloys, Si is the main element and determines the fluidity of the alloy. Mg is an important strengthening element, which is dissolved in the matrix and plays a role of solid solution strengthening. As the Mg content increases, the eutectic phase Mg2Si will appear in the alloy. After T6 treatment, the strengthening phase precipitates to strengthen the alloy. However, as the Mg content further increases, the plasticity of the alloy decreases. Therefore, the Mg content is generally limited to a lower level. Copper is also an important strengthening element in aluminum alloys, mainly playing a role of aging strengthening. Zn is an important element in ultra-high strength aluminum alloys, forming ternary or quaternary aluminum-zinc alloys with alloying elements such as Mg, Cu, and Si. Adding an appropriate amount of magnesium to form a Mg2Zn strengthening phase can significantly improve the strength of the aluminum alloy. Therefore, it is also the main alloying element of alloys such as Al-Zn-Mg, Al-Zn-Si, and Al-Zn-Cu-Mg.

[0003] Al-Si casting alloys are very mature alloy systems, forming a large number of commercial alloy systems. There are both heat-treated strengthened alloys and non-heat-treated strengthened alloys. Heat-treated strengthened alloys are strengthened by solid solution aging treatment, and precipitation strengthening is performed in the alloy to strengthen the alloy, thereby obtaining higher tensile strength and yield strength. However, the heat treatment process inevitably causes deformation of the casting, affecting the use of the casting. Although non-heat-treated strengthened alloys do not have the problem of casting deformation, it is difficult to improve the strength of the alloy, especially the yield strength is generally low. Moreover, the network eutectic silicon structure greatly reduces the elongation of the alloy, making it difficult to obtain high-strength and high-elongation high-quality castings.

[0004] Patent application number CN202210897362X discloses a multi-purpose Al-Si casting alloy with good strength and plasticity, but its yield strength in F state is less than 150 MPa, which is difficult to meet the demand for high yield strength. It is of great significance to develop casting alloys with higher yield strength. Summary of the invention

[0005] The purpose of the present invention is to provide a high yield strength cast Al-Si alloy and a preparation method thereof, so that the cast Al-Si alloy has both high strength, especially high yield strength, and high plasticity.

[0006] The technical solution adopted by the present invention to solve the technical problem is: a high yield strength cast Al-Si alloy, comprising components and mass percentages of Si: 9.0-12.5%, but not equal to 9.0%, Mg: 0.3-0.8%, Cu: 0.2-1.6%, Zn: 0.2-1.6%, Mn: 0-1.0%, Fe≤0.5%, Zr: 0-0.25%, Ti: 0.05-0.25%, Cr: 0-0.25%, Re: 0-0.3%, Sr: 0.02-0.2%, and the balance is Al and unavoidable impurities, the total impurity content in the alloy is ≤1.0%, and the content of a single impurity is ≤0.15%.

[0007] Furthermore, the cast Al-Si alloy has a room temperature tensile strength of 289-336 MPa, a yield strength of 132-187 MPa, and an elongation of 7.3-10.8% in the F state (cast state); the cast Al-Si alloy is a T6 state, T5 state or T4 state Al-Si alloy, wherein, when in the T6 state, the room temperature tensile strength is 335-385 MPa, the yield strength is 243-278 MPa, and the elongation is 5.1-8.9%.

[0008] Furthermore, the cast Al-Si alloy is an Al-Si gravity casting (including low pressure casting) aluminum alloy, and the Al-Si gravity casting aluminum alloy includes components and mass percentages of Si: 9.0-12.5%, but not equal to 9.0%, Mg: 0.3-0.8%, Cu: 0.2-1.6%, Zn: 0.2-1.6%, Mn: 0-0.3%, Fe≤0.3%, Zr: 0-0.25%, Ti: 0.05-0.25%, Cr: 0-0.25%, Re: 0-0.3%, Sr: 0.02-0.2%, and the balance is Al and unavoidable impurities. The total impurity content in the alloy is ≤1.0%, and the content of a single impurity is ≤0.15%.

[0009] Furthermore, the Al-Si gravity casting aluminum alloy has an F-state tensile strength of 281-331 MPa, a yield strength of 124-180 MPa, and an elongation of 6.1-9.6%, and a T6-state tensile strength of 324-371 MPa, a yield strength of 231-266 MPa, and an elongation of 4.1-7.8%.

[0010] The method for preparing the above-mentioned high yield strength cast Al-Si alloy comprises the following steps:

[0011] Step 1: Prepare the raw materials of each component according to the content of each component of the alloy;

[0012] Step 2: Feeding the Al raw material into the preheated melting furnace for heating and melting;

[0013] Step 3: alloying, after the Al raw material is completely melted, add other alloying raw materials except Mg and Sr into the furnace, add raw material Mg after the alloying raw materials are melted, stir evenly after Mg is melted, and obtain aluminum alloy melt; determine the composition of the aluminum alloy melt to ensure that the alloy composition meets the requirements; in the above whole smelting process, control the temperature of the alloy melt to 680-750℃;

[0014] Step 4: Post-smelting treatment, adding a refining agent to the aluminum alloy melt for refining, then removing the aluminum slag from the furnace, and then adding an Sr modifier for modification to obtain a modified alloy melt;

[0015] Step 5: Transfer and degassing: transfer the molten aluminum to the transfer bag, use the degassing rotor to spray argon into the molten aluminum for degassing, then remove the slag, add grain refiner, and pour the molten aluminum into the machine-side furnace of the die casting machine or gravity casting machine;

[0016] Step 6: Casting: using a die casting machine or a gravity casting machine for casting, and obtaining an aluminum-silicon casting alloy casting, that is, a cast Al-Si alloy.

[0017] Furthermore, the preparation method further comprises:

[0018] Step 7: Solution aging treatment

[0019] (1) When it is necessary to prepare T6 state cast Al-Si alloy, the aluminum-silicon casting alloy casting is subjected to solid solution-aging treatment;

[0020] (2) When it is necessary to prepare T4 state cast Al-Si alloy, the aluminum-silicon casting alloy casting is subjected to solid solution treatment and then aging treatment at room temperature;

[0021] (3) When it is necessary to prepare T5 state cast Al-Si alloy, the aluminum-silicon casting alloy casting is directly subjected to aging treatment.

[0022] Furthermore, in step 7, the solution treatment process used for T4 and T6 treatments is: keeping warm at 500-550°C for 2-12 hours; the aging treatment process for T4 is placed at room temperature for more than 7 days; the aging treatment process for T5 and T6 is: keeping warm at 130-180°C for 2-12 hours.

[0023] Furthermore, in the step 1, the raw material Al is one or more of electrolytic aluminum ingots, remelted aluminum ingots or cast aluminum alloy ingots, or a mixture of return materials or recycled waste materials within the factory and Al ingots; the raw material Si is metallic silicon and / or aluminum-silicon master alloy; the raw material Cu is an aluminum-copper master alloy and / or a copper additive; the raw material Mg is an industrial pure magnesium ingot; the raw material Mn is an aluminum-manganese master alloy and / or a manganese additive; the raw material Zr is an aluminum-zirconium master alloy and / or a zirconium additive; the raw material Ti is an aluminum-titanium master alloy and / or a titanium additive; the raw material Cr is an aluminum-chromium master alloy and / or a chromium additive; the raw material Zn is an industrial pure zinc ingot; Re is La or / and Ce, and the raw material Re is an aluminum-lanthanum master alloy or an aluminum-cerium master alloy, or an aluminum-(lanthanum-cerium mixed rare earth) master alloy.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The alloy of the present invention can be used in the cast state or in the T4, T5 or T6 state.

[0026] (2) The iron content of the present invention is relatively high, so more waste materials can be used, thus achieving environmental protection and low carbon.

[0027] (3) The ratio of each alloying element in the present invention makes the alloy have high strength and maintains high plasticity; the present invention increases the Si content and Mg content of the alloy, and at the same time, the alloy contains higher Cu and Zn, which enhances the solid solution strengthening effect of the alloy in the cast state and enhances the aging strengthening effect of the alloy in the aged state, improves the plasticity of the alloy, and reduces its negative impact on the elongation of the alloy; at the same time, other alloying elements are introduced to further increase the solid solution strengthening effect in the alloy, effectively improving the strength and plasticity of the alloy. DETAILED DESCRIPTION

[0028] In the description of the present invention, it should be noted that, if the specific conditions are not specified in the examples, the experiments are carried out under conventional conditions or the conditions recommended by the manufacturer; if the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially. In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0029] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described below; the embodiments of the present invention provide an aluminum-silicon casting alloy, and the high-strength and high-plasticity aluminum-silicon casting alloy and the preparation method thereof of the present invention are described in detail through the following specific embodiments.

[0030] The remelting aluminum ingot selected in the embodiment of the present invention is Al99.70 in the national standard GB / T 1196-2008 "Remelting Aluminum Ingot", and its aluminum content is not less than 99.70wt%; it can also be a scrap remelting aluminum ingot; when adding the Mn element, Al-10Mn master alloy or 75Mn agent (aluminum alloy additive with a Mn mass percentage of 75%) is selected; when adding the Si element, Al-30Si master alloy is selected; when adding the Mg element, metallic magnesium is selected; when adding the Cu element, Al-50Cu master alloy is selected; when adding the Ti element, Al-10Ti master alloy or 75Ti agent (aluminum alloy additive with a Ti content of 75%) is selected; when adding the Zr element, Al-10Zr master alloy is selected; when adding the Cr element, Al-10Cr master alloy is selected. You can also use the pre-alloyed cast aluminum alloy ingots commonly used in the foundry industry, such as the aluminum ingots in the national standard GB / T 8733-2016 "Casting aluminum alloy ingots", and adjust the alloy composition on this basis to achieve the composition target. All raw materials such as Al-10Sr modifier are purchased from the market.

[0031] The invention provides a high yield strength casting Al-Si alloy, comprising components and mass percentages of Si: 9.0-12.5%, but not equal to 9.0%, Mg: 0.3-0.8%, Cu: 0.2-1.6%, Zn: 0.2-1.6%, Mn: 0-1.0%, Fe≤0.5%, Zr: 0-0.25%, Ti: 0.05-0.25%, Cr: 0-0.25%, Re: 0-0.3%, Sr: 0.02-0.2%, and the balance is Al and unavoidable impurities. The total impurity content in the alloy is ≤1.0%, and the content of a single impurity is ≤0.15%.

[0032] The method for preparing the above-mentioned high yield strength cast Al-Si alloy comprises the following steps:

[0033] Step 1: Prepare the raw materials of each component according to the content of each component of the alloy;

[0034] Step 2: Feeding the Al raw material into the preheated melting furnace for heating and melting;

[0035] Step 3: alloying, after the Al raw material is completely melted, add other alloying raw materials except Mg and Sr into the furnace, add raw material Mg after the alloying raw materials are melted, stir evenly after Mg is melted, and obtain aluminum alloy melt; determine the composition of the aluminum alloy melt to ensure that the alloy composition meets the requirements; in the above whole smelting process, control the temperature of the alloy melt to 680-750℃;

[0036] Step 4: post-smelting treatment, adding a refining agent to the aluminum alloy melt for refining, then scraping the aluminum slag out of the furnace, and then adding an Sr modifier for modification to obtain a modified alloy melt; the refining agent is a refining agent that can have a refining effect on the alloy melt, such as RJ-1 refining agent; the added mass of the refining agent is 0.2-0.8% of the total mass of the alloy melt, the refining temperature is 680-750°C, and the refining time is 20-60 minutes; the Sr modifier is specifically selected from Al-10Sr alloy modifier, and the amount of the modifier added is measured by the residual amount of Sr in the alloy melt after modification, ensuring that the mass percentage of the residual amount of Sr is 0.02%-0.2%;

[0037] Step 5: Transfer and degassing: transfer the molten aluminum to the transfer bag, use the degassing rotor to spray argon into the molten aluminum for degassing, then remove the slag, add grain refiner, and pour the molten aluminum into the machine-side furnace of the die casting machine or gravity casting machine; degassing is to use a degasser to pass argon into the modified alloy melt, and the argon flow rate is 0.2-0.3M 3 / h; the grain refiner is a commercial AlTiB or AlTiC alloy, and the addition amount is 0.05-0.25% of the total mass of the alloy melt;

[0038] Step 6: Casting: using a die casting machine or a gravity casting machine for casting, and obtaining an aluminum-silicon casting alloy casting, that is, a cast Al-Si alloy.

[0039] When preparing T4, T5, T6 state cast Al-Si alloy, it also includes:

[0040] Step 7: Solution aging treatment

[0041] (1) When it is necessary to prepare T6 state cast Al-Si alloy, the aluminum-silicon casting alloy casting is subjected to solid solution-aging treatment;

[0042] (2) When it is necessary to prepare T4 state cast Al-Si alloy, the aluminum-silicon casting alloy casting is subjected to solid solution treatment and then aging treatment at room temperature;

[0043] (3) When it is necessary to prepare T5 state cast Al-Si alloy, the aluminum-silicon casting alloy casting is directly subjected to aging treatment;

[0044] The solution treatment process used for T4 and T6 treatments is: keeping at 500-550℃ for 2-12h; the aging treatment process of T4 is placed at room temperature for more than 7 days; the aging treatment process of T5 and T6 is: keeping at 130-180℃ for 2-12h.

[0045] Wherein, when the Sr modifier is not added in step 4, it can be added to the aluminum melt together with Mg in step 3, or added to the aluminum melt together with other raw materials except Mg.

[0046] Wherein, in the step 6, the casting is performed by a die casting process, preferably high pressure die casting; vacuum high pressure die casting is performed for castings that require T4 and T6 treatments.

[0047] In the step 6, the casting is performed by gravity casting or low pressure casting process, the casting mold is a metal mold, the cooling speed of the metal liquid is increased, and the metal liquid is sub-fast cooled according to the size of the casting, and the cooling speed is between 10 0 -10 2 ℃ / s, so that the metal liquid solidifies under sub-rapid cooling state.

[0048] Example A1

[0049] A high yield strength cast Al-Si alloy, the chemical composition of which is shown in Table 1, and the preparation method comprises the following steps:

[0050] Step 1: Prepare the raw materials of each component according to the content of each component of the alloy;

[0051] Step 2: Feeding the Al raw material into the preheated melting furnace for heating and melting;

[0052] Step 3: Alloying. After the aluminum raw material is completely melted, add other alloying raw materials except Mg and Sr into the furnace. After the alloying raw materials are melted, add the raw material Mg. After Mg is melted, stir evenly to obtain an aluminum alloy melt. Determine the composition of the aluminum alloy melt to ensure that the alloy composition meets the requirements. During the entire smelting process, the temperature of the alloy melt is controlled at 710℃.

[0053] Step 4: post-smelting treatment, adding RJ-1 refining agent to the aluminum alloy melt for refining, the added amount is 0.4% of the total mass of the alloy melt, then the aluminum slag is removed from the furnace, and then Al-10Sr modifier is added for modification to obtain the modified alloy melt;

[0054] Step 5: Transfer and degassing: transfer the molten aluminum to the transfer bag, use the degassing rotor to spray argon into the molten aluminum for degassing, then skim the slag, add Al-5Ti-1B grain refiner, the addition amount is 0.1% of the total mass of the alloy melt; pour the molten aluminum into the die-casting machine side furnace.

[0055] Step 6: Casting: using a die-casting machine to die-cast the molten aluminum into a casting to obtain a cast Al-Si alloy.

[0056] Step 7: The prepared Al-Si alloy product is subjected to a room temperature tensile property test. The room temperature tensile property is shown in Table 1.

[0057] Examples A2-A9 and Examples A12 and A13 are the same as Example 1, except that the alloy compositions are different. The alloy compositions and room temperature tensile properties of the prepared castings are shown in Table 1.

[0058] Embodiments A10 and A11 and embodiments A14-A19 are the same as embodiment 1, except that the alloy composition is different, the casting process adopts vacuum high pressure die casting, and the casting needs to be subjected to solid solution aging heat treatment. The alloy composition, the solid solution aging treatment process of the casting after preparation, and the room temperature tensile properties are shown in Table 2.

[0059] Embodiments B1-B19 are the same as Embodiments A1-A19, except that:

[0060] (1) Alloy composition: Examples A1-A19 are die casting alloys with high Fe and Mn contents. Examples B1-B19 are gravity casting or low pressure casting alloys, which do not have mold sticking problems and do not need to increase the Fe and Mn contents to solve the mold sticking problem. Therefore, in these examples, Fe and Mn are impurity elements, and the lower the better. However, in order to maximize the use of aluminum alloy scrap with a high Fe content, the Fe and Mn content limits are intentionally increased.

[0061] (2) Casting process: Examples B1-B19 are aluminum-silicon casting alloys cast by a gravity casting machine or a low-pressure casting machine, wherein the casting mold is a metal mold;

[0062] (3) Alloy composition, solution treatment process of the castings after preparation, and room temperature tensile properties are shown in Tables 3 and 4.

[0063] Element Si is the main component of Al-Si alloy. Si precipitates in the form of eutectic Si during solidification to form a network structure. The higher the Si content, the coarser the eutectic Si phase and the tighter the network structure. For alloys used in the die-cast state (F state), this eutectic structure of the network structure cannot be broken by heat treatment, and the silicon particles cannot be spheroidized. It is generally believed that this eutectic Si structure of the network structure seriously damages the mechanical properties of the alloy. However, in order to improve fluidity, die-casting alloys need to be designed with a higher Si content. With the development of high-pressure die-casting, the demand for alloy fluidity has decreased, so the Si content in high-pressure die-cast aluminum alloys has a tendency to decrease. For example, the Si content in the invention with application number CN202210897362X is only 6-9%, and an elongation of up to 14.3% has been achieved, but the strength is slightly lower, and the yield strength does not exceed 150MPa. Although the present invention uses high pressure die casting, it still uses high silicon content, and achieves unexpected results: the strength of the alloy is greatly improved, especially the yield strength, which is up to 191MPa in the die casting state (F state), and the elongation is still maintained at 8.9%. Obviously, it has a broader application prospect.

[0064] The present invention uses high-pressure die casting, which is not only a production process, but also a means to improve mechanical properties. High-pressure die casting has high-pressure injection speed and injection pressure ratio, and die castings are often thin-walled parts. During die casting, molten aluminum is quickly pressed into the mold cavity and quickly solidified under high pressure. Under the multiple effects of Sr modification, grain refiner and rare earth elements, the grains of the die castings are very fine. This makes the eutectic Si phase and its network structure formed at the grain boundary very fine, so that their damage to mechanical properties is greatly reduced. In this case, the increased solid solution strengthening effect brought about by increasing the Si content becomes the dominant effect, thereby improving the strength of the alloy and maintaining a high elongation.

[0065] Mg is an important strengthening element in aluminum alloys, which can play a role in both solid solution strengthening and aging strengthening. In non-heat treatment strengthening alloys, such as 5000 series aluminum alloys, that is, Al-Mg alloys, Mg is the main solid solution strengthening element, and the Mg content can reach up to 6.0% (in 5059 alloy); in heat treatment strengthening alloys, such as 6000 series alloys, that is, Al-Mg-Si alloys, Mg is the main aging strengthening element, forming Mg2Si strengthening phase alloy strengthening. Although the solid solubility limit of Mg in Al is as high as 17.4%, and the eutectic composition of Al-Mg alloys is 34% Mg, Mg2Si eutectic phase is easy to appear in Al-Si-Mg alloys. According to the Al-Si-Mg alloy phase diagram, in high Si and low Mg alloys (such as cast Al-Si alloys), during the solidification process, the Al matrix is ​​first precipitated, and when the liquid composition at the interface front reaches the Al+Si eutectic line, the L→Al+Si eutectic reaction occurs. Then, the liquid composition at the interface front changes along the eutectic line. When the liquid component at the interface front reaches the ternary eutectic point, the L→Al+Si+Mg2Si ternary eutectic reaction occurs. The Mg2Si phase is in the shape of Chinese characters, which is detrimental to the mechanical properties of the alloy. Due to the large tendency of Mg to segregate, the Mg2Si eutectic phase will appear even if the Mg content is low. The higher the Mg content, the more and coarser the Mg2Si eutectic phase is in the cast structure, and the greater the damage to the mechanical properties. For alloys used in the cast state, the Chinese character-shaped Mg2Si eutectic phase cannot be eliminated because no heat treatment is performed. Therefore, it is necessary to limit the Mg content to a very low level, or even completely remove the Mg element to prevent the formation of coarse Mg2Si phase during casting. At present, the Mg content is often strictly limited for alloys used in the cast state. The Mg content is generally controlled below 0.2. Elemental Mg has a strong solid solution strengthening effect. If the adverse effects of the Mg2Si phase can be suppressed, the strength of the alloy can be improved by increasing the Mg content.

[0066] Cu is another important alloying element. But it mainly plays an aging strengthening role. At present, the Cu content in cast Al-Si alloys is generally above 3.5%, which plays an aging strengthening role of the Cu-rich phase. There is currently no solid solution strengthened alloy based on Cu. Cu combines with Mg to form Al2CuMg phase, and combines with Mg and Si to form Q-AlCuMgSi phase. Studies have shown that the formation of Q-AlCuMgSi phase can inhibit the formation of Mg2Si phase, and Q-AlCuMgSi is spherical, which greatly reduces the damage to mechanical properties. This result lays the foundation for the development of high-strength non-heat-treatable Al-Si alloys.

[0067] Zn is another important alloying element. On the one hand, Zn has a large solid solubility in aluminum, and on the other hand, the addition of Zn can promote the transformation of Mg2Si phase to Q-AlCuMgSi phase.

[0068] The present invention combines Si, Mg, Cu and Zn to achieve unexpected results. After adding Cu and Zn at the same time, on the one hand, the formation of coarse Mg2Si phase is suppressed, thereby avoiding the damage of Mg2Si phase to mechanical properties. In this way, the restriction on Mg content can be appropriately relaxed, thereby further improving the strength of the alloy. On the other hand, a small amount of Cu and Zn also has a solid solution strengthening effect. Therefore, the alloy of the present invention has very high strength.

[0069] The contents of Si, Mg, Cu and Zn determine the type, morphology, size and quantity of the phases in the solidified structure. In order to minimize the formation of the Mg2Si phase, they must maintain a suitable ratio. In particular, the ratio between Cu and Mg determines whether the Mg2Si phase or the Q-AlCuMgSi phase is formed. In high Si content alloys, for alloys used in the die casting state (F state), it is more appropriate to design the relationship between Cu and Mg to be Cu=2.5Mg-0.2, with a deviation of 0.1 above and below.

[0070] For Al-Si-Mg casting alloys used in the T6 state, it is necessary to precipitate Mg2Si strengthening phase during aging to strengthen the alloy. On the other hand, the coarse Mg2Si phase formed during solidification can be eliminated by solution treatment, so a certain amount of Mg2Si phase is allowed to exist in the solidified structure. Therefore, the amount of Cu and Zn should be reduced accordingly. For alloys used in the T4, T5 and T6 states, when the Mg2Si phase is required as a strengthening phase, it is more appropriate to design the relationship between Cu and Mg as Cu=2.5(Mg-0.2)-0.3, and a deviation of 0.1 above and below is allowed.

[0071] The addition of rare earth elements in the present invention has achieved good results and improved the mechanical properties of the alloy. After a large number of comparative experiments, it was found that Ce and La and their mixed rare earths have the best effect, refining grains, reducing gas and inclusions. Casting experiments show that the addition of rare earths can increase the fluidity of aluminum liquid, the process performance has obvious improvements, and the rare earth elements promote aging precipitation. More importantly, the Q-AlCuMgSi phase is refined, further reducing its damage to mechanical properties, thereby improving the mechanical properties. Example A3 shows that the mechanical properties of the alloy are improved by adding rare earths.

[0072] The elements Fe and Mn can effectively prevent the casting from sticking to the mold, which is very important for die casting production, so Fe and Mn are essential elements of die casting alloys. 15The (FeMn)3Si2 phase is in the form of coarse needles, laths or Chinese characters, which seriously damages the mechanical properties of the alloy. 15 The morphology of the (FeMn)3Si2 phase is greatly affected. When the ratio of Fe to Mn is close, Al 15 The morphology of the (FeMn)3Si2 phase is fishbone-like, which can alleviate the damage to the mechanical properties.

[0073] There is no mold sticking problem in ordinary casting alloys, so the content of Fe and Mn should be strictly limited in these alloys. On the other hand, Fe and Mn are common elements in aluminum alloy scrap and have a high content. In order to effectively utilize scrap and reduce production costs, as much scrap as possible should be used, which requires relaxing the restrictions on Fe and Mn content, and thus finding a balance between mechanical properties and the use of scrap.

[0074] Sr is a modifier of hypoeutectic Al-Si alloy, which can modify the eutectic Si phase and significantly refine the eutectic Si. The amount of Sr is generally controlled at 0.02-0.04%. High Sr content can effectively refine Al 15 (FeMn)3Si2 phase. Especially when the ratio of Fe and Mn is close, Al 15 The morphology of the (FeMn)3Si2 phase is fishbone-shaped. Under the modification of Sr, the fishbone-shaped fracture forms small blocks, which can further reduce the Al 15 Damage to the mechanical properties of (FeMn)3Si2 phase.

[0075] The chemical compositions of Example A3 and Example A4 are basically the same, except that Example A3 contains 0.16% of rare earth elements. Comparison shows that Example A3 has better mechanical properties. The same is true for Examples B3 and B4, indicating that rare earth elements play a role in improving mechanical properties.

[0076] The Fe content in Examples A6, A9, A12-A19 and Examples B5-B9, B12-B9 is very high, but by adding a relatively high amount of Sr to modify and refine the Fe-rich phase, the alloy still maintains relatively high strength and elongation.

[0077] Examples A12 and A13 are alloys used in the F state. The alloy components of the two are exactly the same except for the Cu content. The Cu content of Example A12 is determined according to the Cu content rule of the F state, and the Cu content of Example A13 is determined according to the Cu content rule of the T6 state, which is reduced by 0.5%, resulting in a large amount of Mg2Si eutectic phase in the solidified structure of the alloy, which impairs the mechanical properties. Therefore, the mechanical properties of Example A13 are lower than those of Example A12. The situation of Examples B12 and B13 is the same.

[0078] Examples A16 and A17 are alloys used in the T6 state. The alloy components of the two are exactly the same except for the Cu content. The Cu content of Example A16 is determined according to the Cu content rule of the T6 state, and the Cu content of Example A17 is determined according to the Cu content rule of the F state. It is increased by 0.5%, resulting in a significant reduction in the Mg2Si eutectic phase in the solidified structure of the alloy, thereby resulting in a significant reduction in the Mg2Si strengthening phase precipitated in the alloy during aging treatment, making the aging strengthening effect of the alloy much weaker. Therefore, the mechanical properties of Example A17 are lower than those of Example A16. The situation of Examples B16 and B17 is the same.

[0079] From the comparison between Examples A12 and A13, B12 and B13, A16 and A17, and B16 and B17, it can be seen that the ratio between Cu and Mg is very important. Only with a suitable ratio between the two can good mechanical properties be achieved.

[0080] Table 1 Chemical composition (wt%) and properties of die casting alloys

[0081]

[0082]

[0083] Table 2 Chemical composition (wt%) and properties of die casting alloys (continued)

[0084]

[0085]

[0086] Table 3 Chemical composition (wt%) and properties of gravity casting alloys

[0087]

[0088]

[0089] Table 4 Chemical composition (wt%) and properties of gravity casting alloys (continued)

[0090]

[0091] The above technical scheme explains the technical idea of ​​the present invention, which cannot be used to limit the protection scope of the present invention. Any changes and modifications made to the above technical scheme based on the technical essence of the present invention without departing from the content of the technical scheme of the present invention shall fall within the protection scope of the technical scheme of the present invention.

Claims

1. A high yield strength cast Al-Si alloy, characterized in that: The cast Al-Si alloy is a die-cast aluminum alloy, including components and mass percentages of Si: 9.0-12.5%, but not equal to 9.0%, Mg: 0.51-0.8%, Cu: 1.05-1.6%, Zn: 1.05-1.6%, Mn: 0-1.0%, Fe 0.15-0.45%, Zr: 0.08-0.25%, Ti: 0.05-0.25%, Cr: 0-0.25%, Re: 0-0.3%, Sr: 0.02-0.2%, Cu=2.5Mg-0.2%±0.1%, and the balance is Al and unavoidable impurities. The total impurity content in the alloy is ≤1.0%, and the content of a single impurity is ≤0.15%; The method for preparing the high yield strength cast Al-Si alloy comprises the following steps: Step 1: Prepare the raw materials of each component according to the content of each component of the alloy; Step 2: Feeding the Al raw material into the preheated melting furnace for heating and melting; Step 3: alloying, after the Al raw material is completely melted, add other alloying raw materials except Mg and Sr into the furnace, add raw material Mg after the alloying raw materials are melted, stir evenly after Mg is melted, and obtain aluminum alloy melt; determine the composition of the aluminum alloy melt to ensure that the alloy composition meets the requirements; in the above whole smelting process, control the temperature of the alloy melt to 680-750℃; Step 4: Post-smelting treatment, adding a refining agent to the aluminum alloy melt for refining, then removing the aluminum slag from the furnace, and then adding an Sr modifier for modification to obtain a modified alloy melt; Step 5: Transfer and degassing: transfer the molten aluminum to the transfer bag, use the degassing rotor to spray argon into the molten aluminum for degassing, then remove the slag, add grain refiner, and pour the molten aluminum into the machine-side furnace of the die-casting machine; Step 6: Casting, using a die-casting machine to cast, and after casting, an aluminum-silicon casting alloy casting is obtained, that is, a cast Al-Si alloy; The room temperature tensile strength of the cast Al-Si alloy is 316-336 MPa, the yield strength is 169-187 MPa, and the elongation is 7.7-9.5%.

2. A high yield strength cast Al-Si alloy, characterized in that: The cast Al-Si alloy is an Al-Si gravity cast aluminum alloy, and the Al-Si gravity cast aluminum alloy includes components and mass percentages of Si: 9.0-12.5%, but not equal to 9.0%, Mg: 0.51-0.8%, Cu: 1.05-1.6%, Zn: 1.05-1.6%, Mn: 0-0.3%, Fe 0.15-0.3%, Zr: 0.08-0.25%, Ti: 0.05-0.25%, Cr: 0-0.25%, Re: 0-0.3%, Sr: 0.02-0.2%, and the balance is Al and unavoidable impurities, and the total impurity content in the alloy is ≤1.0%, and the content of a single impurity is ≤0.15%; The method for preparing the high yield strength cast Al-Si alloy comprises the following steps: Step 1: Prepare the raw materials of each component according to the content of each component of the alloy; Step 2: Feeding the Al raw material into the preheated melting furnace for heating and melting; Step 3: alloying, after the Al raw material is completely melted, add other alloying raw materials except Mg and Sr into the furnace, add raw material Mg after the alloying raw materials are melted, stir evenly after Mg is melted, and obtain aluminum alloy melt; determine the composition of the aluminum alloy melt to ensure that the alloy composition meets the requirements; in the above whole smelting process, control the temperature of the alloy melt to 680-750℃; Step 4: Post-smelting treatment, adding a refining agent to the aluminum alloy melt for refining, then removing the aluminum slag from the furnace, and then adding an Sr modifier for modification to obtain a modified alloy melt; Step 5: Transfer and degassing: transfer the molten aluminum to the transfer bag, use the degassing rotor to spray argon into the molten aluminum for degassing, then remove the slag, add grain refiner, and pour the molten aluminum into the machine-side furnace of the gravity casting machine; Step 6: Casting: using a gravity casting machine to cast, and after casting, an aluminum-silicon casting alloy casting is obtained, that is, a cast Al-Si alloy.

3. A high yield strength cast Al-Si alloy according to claim 2, characterized in that: The Al-Si gravity casting aluminum alloy has a cast tensile strength of 281-331 MPa, a yield strength of 124-180 MPa, and an elongation of 6.1-9.6%.

Citation Information

Cited By

  • Al-Si-Mg series aluminum alloy and preparation method and application thereof

    CN121575277A

  • Al-si-mg aluminum alloy, method for preparing same, and use thereof

    CN121575277B