Hollow carbon material coated ferrite absorber powder and preparation method and application thereof
By forming a hollow-structured carbon material coating layer on the ferrite microspheres, the problem of ferrite absorbing powder being difficult to balance between high absorption performance and low density is solved, achieving excellent absorption performance and low density in a wide frequency range. Stable chemical properties to meet the high performance requirements of absorbing materials.
Patent Information
- Application Number
- CN202111556756.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-17
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-12-17
AI Technical Summary
It is difficult for existing ferrite absorbing powder to balance high absorption performance, low density and stable chemical properties, and cannot meet the high performance requirements of absorbing materials.
The method for preparing hollow carbon material-coated ferrite absorber powder is to coat the surface of Fe3O4 microspheres with a SiO2 layer, and then form a polypyrrole layer through PVP surface modification and in-situ polymerization of pyrrole, and then in an inert gas. Calcination and carbonization, and finally etching in an alkaline solution to remove the SiO2 layer, forming a hollow structure of carbon material-coated ferrite absorber powder.
It has realized an absorbing material with excellent absorbing performance in a wide frequency band, taking into account high absorption performance, low density and stable chemical properties, meeting the high performance requirements of absorbing materials, and improving the corrosion resistance and corrosion resistance of ferrite. Oxidation resistance.
Smart Images

Figure CN116265559B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of absorbing materials, and in particular to a hollow carbon material-coated ferrite absorbing agent powder, a preparation method thereof and an application thereof. Background Art
[0002] With the rapid development of electronic information, electromagnetic radiation has become more and more serious. Electromagnetic pollution is more common than chemical pollution and has become a serious social hazard. Therefore, radar-absorbing stealth materials have attracted more and more attention at home and abroad.
[0003] Ferrite is the most studied, cheapest and most widely used traditional absorbing material. It has the characteristics of wide raw material supply, low price, simple manufacturing process, strong absorption, wide frequency band, strong corrosion resistance and low cost. Ferroferric oxide is its typical representative. It has the dual absorbing ability of magnetic loss and dielectric loss and is a commonly used absorbing material. However, ferrite has a large density and it is difficult to meet the principle of keeping the relative dielectric constant and relative magnetic permeability as close as possible, which makes it difficult to match the impedance. It makes it difficult for a single ferrite to simultaneously meet the requirements of high-performance absorbing materials such as strong absorption, wide frequency band, light weight and thin thickness. Carbon-based materials have excellent dielectric properties, good composite properties, special microstructures, low density, strong chemical stability, high resonance frequency and high magnetic permeability, which enhance the absorbing effect. They have broad applications in the field of radar absorbing and have become a hot topic of research at home and abroad.
[0004] There are many patents on the preparation process of ferroferric oxide loading, most of which use porous carbon and ferroferric oxide precursor solution as raw materials, mix the raw materials, heat the mixture in a water bath, age it, and dry it to obtain ferroferric oxide / porous carbon composite absorber. The preparation method of the composite absorber is simple, the raw material cost is low, and it is suitable for industrial production, but its absorption loss mechanism is single, the absorption efficiency and bandwidth need to be further improved, and the chemical performance is poorly stable, and low-density characteristics cannot be achieved.
[0005] Therefore, it is necessary to provide a new wave absorbing agent powder with good absorption performance, low density, stable chemical properties and better comprehensive performance. Summary of the invention
[0006] The main purpose of the present invention is to provide a hollow carbon material coated ferrite absorber powder and its preparation method and application, so as to solve the problems that the ferrite absorber powder in the prior art is difficult to have high absorption performance, low density and stable chemical properties.
[0007] In order to achieve the above-mentioned object, according to one aspect of the present invention, a method for preparing a hollow carbon material-coated ferrite absorber powder is provided, which comprises the following steps: step S1, coating a SiO2 layer on the surface of a Fe3O4 microsphere to form a Fe3O4 / SiO2 core-shell microsphere; step S2, dispersing the Fe3O4 / SiO2 core-shell microsphere in a first solvent, and then adding PVP to modify the surface of the Fe3O4 / SiO2 core-shell microsphere to form a PVP-modified Fe3O4 / SiO2 core-shell microsphere; step S3, adding the PVP-modified Fe3O4 / SiO2 core-shell microsphere to the Fe3O4 / SiO2 core-shell microsphere; 4 / SiO2 core-shell microspheres are dispersed in a second solvent, and then an oxidant and pyrrole are added and a polymerization reaction is carried out to further form a PPy coating layer on the surface of the PVP-modified Fe3O4 / SiO2 core-shell microspheres, thereby obtaining Fe3O4 / SiO2 / PPy core-shell microspheres; step S4, calcining the Fe3O4 / SiO2 / PPy core-shell microspheres in an inert gas to carbonize the PPy coating layer to obtain carbonized microspheres; step S5, placing the carbonized microspheres in an alkaline solution, etching and removing the SiO2 layer, thereby forming a hollow carbon material-coated ferrite absorber powder.
[0008] Furthermore, step S1 includes: dispersing Fe3O4 microspheres in a third solvent to form a dispersion; adjusting the pH value of the dispersion to 8-9, then adding tetraethyl orthosilicate thereto, reacting under stirring to obtain a reaction slurry; separating the solid in the reaction slurry, drying, and obtaining Fe3O4 / SiO2 core-shell microspheres; preferably, the particle size of the Fe3O4 microspheres is 200-800nm; preferably, the weight ratio of Fe3O4 microspheres to tetraethyl orthosilicate is (2-10):(1-6); preferably, the third solvent is a mixed solvent of ethanol and water, and the weight ratio of the two is (8-12):(2-5); preferably, the reagent for adjusting the pH value of the dispersion is ammonia water; preferably, after adding tetraethyl orthosilicate, the reaction is carried out for 3-6h at a stirring speed of 400-1000r / min and a temperature of 40-80°C.
[0009] Furthermore, Fe3O4 microspheres are prepared by the following method: divalent iron salt and trivalent iron salt are dispersed in a fourth solvent, and then a base is added to react, solid-liquid separation, and drying to obtain Fe3O4 microspheres; preferably, the divalent iron salt is ferrous chloride and / or ferrous sulfate, and the trivalent iron salt is ferric chloride and / or ferric sulfate; preferably, the base is anhydrous sodium acetate; preferably, the total weight of the divalent iron salt and the trivalent iron salt is recorded as m1, and the weight of the base is recorded as m2, then m1 / m2 is (1-6):(4-30); preferably, the fourth solvent is an ethylene glycol aqueous solution with a mass concentration of 96-99%; preferably, after adding the base, the reaction is carried out for 5-10 hours at a stirring speed of 1500-2500 r / min and a temperature of 150-250°C.
[0010] Furthermore, in step S2, the weight ratio of Fe3O4 / SiO2 core-shell microspheres to PVP is (1-6):(3-8); preferably, the first solvent is an ethanol aqueous solution, more preferably an ethanol aqueous solution with a mass concentration of 50-80%.
[0011] Furthermore, step S3 includes: dispersing PVP-modified Fe3O4 / SiO2 core-shell microspheres in a second solvent, then adding an oxidant and stirring for 30 to 80 minutes, and then adding pyrrole for polymerization reaction to obtain Fe3O4 / SiO2 / PPy core-shell microspheres; preferably, the weight ratio of PVP-modified Fe3O4 / SiO2 core-shell microspheres to the oxidant is (1 to 6):(5 to 10); preferably, the weight ratio of PVP-modified Fe3O4 / SiO2 core-shell microspheres to pyrrole is (1 to 6):(1 to 5); preferably, the temperature during the polymerization reaction is 30 to 50°C, the stirring speed is 400 to 800 r / min, and the reaction time is 6 to 12 hours; preferably, the oxidant is ferric chloride; preferably, the second solvent is water.
[0012] Furthermore, in step S4, during the calcination of Fe3O4 / SiO2 / PPy core-shell microspheres, the calcination temperature is 500-800°C and the calcination time is 2-6 hours.
[0013] Furthermore, in step S5, the alkaline solution is a sodium hydroxide aqueous solution with a concentration of 10 to 30 wt%.
[0014] Furthermore, in step S5, after placing the carbonized microspheres in an alkaline solution, the reaction is carried out for 10 to 20 hours at a stirring speed of 800 to 1500 r / min and a temperature of 40 to 80°C to etch and remove the SiO2 layer; preferably, in step S5, after the reaction is completed, the precipitate is separated and dried to obtain a hollow carbon material-coated ferrite absorber powder.
[0015] According to another aspect of the present invention, there is also provided a hollow carbon material-coated ferrite absorber powder, which is prepared by the above-mentioned preparation method.
[0016] According to another aspect of the present invention, there is provided an absorbing material, comprising absorbing powder, which is the above-mentioned carbon material-coated ferrite absorbing agent powder.
[0017] The preparation method of the present invention is used to prepare a hollow carbon material coated ferrite absorber powder, which is first coated with a SiO2 layer on the surface of the Fe3O4 microsphere, and then a further coated polypyrrole layer is formed by PVP surface modification and pyrrole in-situ polymerization to form Fe3O4 / SiO2 / PPy core-shell microspheres. Secondly, the present invention calcines in an inert gas to carbonize the polypyrrole layer to form Fe3O4 / SiO2 / C core-shell microspheres (carbonized microspheres), and then places the microspheres in an alkaline solution to etch and remove the middle SiO2 layer, thereby finally forming a carbon material coated ferrite absorber powder with a hollow structure. The absorbent powder has a hollow core-shell structure (the core layer is Fe3O4 microspheres, the shell layer is a carbon layer, and there is a hollow structure between the two). In addition to absorbing and reflecting lossy electromagnetic waves, it can also produce multiple reflections and multiple absorptions in the cavity, increase the propagation path of electromagnetic waves, form an effective conductive network structure, and increase the dielectric loss of the material, so that the prepared absorbent material can have good absorbent performance in a wider frequency band, meeting the high-performance requirements of the absorbent material. At the same time, the hollow structure and carbon layer coating also reduce the density of ferrite, improve the agglomeration of ferroferric oxide particles, and also have corrosion resistance, oxidation resistance and other properties, and stable chemical properties.
[0018] In conclusion, the hollow carbon material-coated ferrite absorber powder prepared by the present invention has a good balance of high absorption performance, low density and stable chemical properties, and has excellent comprehensive performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0020] Figure 1 A schematic flow chart of a method for preparing a hollow carbon material-coated ferrite absorber powder according to an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0021] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0022] As described in the background technology section, it is difficult for the ferrite absorbing powder in the prior art to have high absorption performance, low density and stable chemical properties. In order to solve the above problems, the present invention provides a method for preparing a hollow carbon material coated ferrite absorbing agent powder, such as Figure 1As shown, the preparation method comprises the following steps: step S1, coating the surface of Fe3O4 microsphere a with a SiO2 layer to form Fe3O4 / SiO2 core-shell microsphere b; step S2, dispersing the Fe3O4 / SiO2 core-shell microsphere b in a first solvent, and then adding PVP to modify the surface of the Fe3O4 / SiO2 core-shell microsphere to form PVP-modified Fe3O4 / SiO2 core-shell microsphere c; step S3, dispersing the PVP-modified Fe3O4 / SiO2 core-shell microsphere c in a second solvent, and then adding The oxidant and pyrrole are polymerized to further form a PPy coating layer (polypyrrole coating layer) on the surface of the PVP-modified Fe3O4 / SiO2 core-shell microspheres, thereby obtaining Fe3O4 / SiO2 / PPy core-shell microspheres d; step S4, calcining the Fe3O4 / SiO2 / PPy core-shell microspheres d in an inert gas to carbonize the PPy coating layer to obtain carbonized microspheres; step S5, placing the carbonized microspheres in an alkaline solution, etching away the SiO2 layer, thereby forming a hollow carbon material-coated ferrite absorber powder e.
[0023] The preparation method of the present invention is used to prepare a hollow carbon material-coated ferrite absorber powder, which is first coated with a SiO2 layer on the surface of the Fe3O4 microsphere, and then a further coated polypyrrole layer is formed by PVP surface modification and in-situ polymerization of pyrrole to form Fe3O4 / SiO2 / PPy core-shell microspheres. Secondly, the present invention calcines in an inert gas to carbonize the polypyrrole layer to form Fe3O4 / SiO2 / C core-shell microspheres (carbonized microspheres), and then places it in an alkaline solution to etch and remove the middle SiO2 layer, thereby finally forming a ferrite absorber powder coated with a carbon material having a hollow structure. It should be noted that Figure 1 What is shown is only a schematic diagram. After the SiO2 layer is finally removed, the outer carbon layer and the core Fe3O4 microspheres are not completely separated, but attached and fixed at some positions. However, there is a gap between the two layers, which is not dense enough, so there is a hollow structure.
[0024] The hollow carbon material coated ferrite absorber powder prepared by the above method not only has excellent dielectric properties and good matrix bonding, but also has low density, good corrosion resistance and oxidation resistance, and good chemical stability; at the same time, the carbon coating layer improves the agglomeration phenomenon of ferroferric oxide particles, and retains the dual absorbing ability of the ferrite itself with magnetic loss and dielectric loss; more importantly, in addition to absorbing and reflecting lossy electromagnetic waves, the hollow structure powder can also produce multiple reflections and multiple absorptions in the cavity, and the propagation path of the electromagnetic wave is increased, which can form an effective conductive network structure and increase the dielectric loss of the material, so that the prepared absorbing material can have good absorbing performance in a wider frequency band, so that the powder has good matching, strong absorption, and frequency band, which meets the high performance requirements of the absorbing material.
[0025] In summary, the hollow carbon material-coated ferrite absorber powder prepared by the present invention has a good balance of high absorption performance, low density and stable chemical properties, has excellent comprehensive performance, and may meet the different comprehensive performance requirements of absorbing materials in military fields such as electronic information products, aerospace, etc.
[0026] In a preferred embodiment, step S1 includes: dispersing Fe3O4 microspheres in a third solvent to form a dispersion; adjusting the pH value of the dispersion to 8-9, then adding tetraethyl orthosilicate thereto, reacting under stirring to obtain a reaction slurry; separating the solid in the reaction slurry, drying, and obtaining Fe3O4 / SiO2 core-shell microspheres. Under this process condition, a more complete SiO2 layer can be coated on the surface of the Fe3O4 microspheres, which is conducive to the subsequent formation of a hollow structure, and has a better effect on the absorbing performance, low density, and prevention of agglomeration of the absorbing powder.
[0027] Preferably, the particle size of the Fe3O4 microspheres is 200-800nm, more preferably the particle size of the Fe3O4 microspheres is 400-600nm; in order to make the SiO2 layer more complete and the thickness more suitable, preferably, the weight ratio of the Fe3O4 microspheres to ethyl orthosilicate is (2-10):(1-6). By controlling the weight ratio of the two within the above range, the SiO2 layer is more completely coated and the thickness is more suitable. On the one hand, it can better support the outer shell during the carbonization process of the PPy coating agent, making the final hollow structure of the powder more complete. On the other hand, it also makes the carbonized carbon layer better fixed, and the overall structural stability of the powder is higher, which is more beneficial to the stability of its performance in all aspects.
[0028] In a preferred embodiment, the third solvent is a mixed solvent of ethanol and water, and the weight ratio of the two is (8-12): (2-5). In this solvent, the Fe3O4 microspheres are better dispersed, which is more beneficial to the stability of the coating process and the coating effect of the SiO2 layer. Preferably, the reagent for adjusting the pH value of the dispersion is ammonia water. Preferably, after adding tetraethyl orthosilicate, the reaction is carried out for 3-6 hours at a stirring speed of 400-1000r / min and a temperature of 40-80°C. Reacting under the above conditions is conducive to further improving the coating effect of the SiO2 layer, and plays a better role in promoting the formation of the hollow structure and structural stability.
[0029] Exemplarily, the following steps can be used to coat the SiO2 layer: add 2 to 10 parts of Fe3O4 microspheres by weight to a mixed solvent of 800 to 1200 parts of anhydrous ethanol and 200 to 500 parts of deionized water, and perform ultrasonic treatment for 30 to 50 minutes to make the Fe3O4 microspheres more evenly dispersed in the solvent; use ammonia water as a pH regulating liquid to adjust the pH of the reaction liquid to 8 to 9, then drop 1 to 6 parts of ethyl orthosilicate therein, and stir continuously for 3 to 6 hours in a water bath at 40 to 80°C at a speed of 400 to 1000 r / min. After the reaction is completed, collect the precipitate with a magnet, pour out the supernatant, wash with ethanol 3 to 6 times, and place the precipitate in a 60 to 120°C blast oven for drying for 8 to 15 hours to complete the preparation of Fe3O4 / SiO2 core-shell microspheres.
[0030] In a preferred embodiment, Fe3O4 microspheres are prepared by the following method: dispersing a divalent iron salt and a trivalent iron salt in a fourth solvent, then adding a base to react, solid-liquid separation, and drying to obtain Fe3O4 microspheres. The Fe3O4 microspheres prepared using this method have better morphology and more uniform particle size. Preferably, the divalent iron salt is ferrous chloride and / or ferrous sulfate, and the trivalent iron salt is ferric chloride and / or ferrous sulfate. The use of the above types and amounts of divalent iron salts and trivalent iron salts can react more stably under the action of the base, and the Fe3O4 microspheres formed are more uniform. Preferably, the base is anhydrous sodium acetate; preferably, the total weight of the divalent iron salt and the trivalent iron salt is recorded as m1, and the weight of the base is recorded as m2, then m1 / m2 is (1-6): (4-30). Using the above type of base, controlling the amount within the above range is conducive to a more sufficient and efficient reaction, and will not cause excessive waste of raw materials.
[0031] In order to provide a more stable reaction environment and make the prepared Fe3O4 microspheres more uniform in morphology and particle size, preferably, the fourth solvent is an ethylene glycol aqueous solution with a mass concentration of 96-99%. Preferably, after adding the alkali, the reaction is carried out for 5-10 hours at a stirring speed of 1500-2500 r / min and a temperature of 150-250°C. Under the above conditions, the reaction is more complete, the magnetic properties of the prepared Fe3O4 microspheres are better, and the absorbing properties of the final absorbing powder are better promoted.
[0032] Exemplarily, the following steps can be used to prepare Fe3O4 microspheres: by weight, 5 to 30 parts of iron salt (divalent iron and trivalent iron) are dispersed in 400 to 800 parts of ethylene glycol solution, and after stirring evenly, 20 to 150 parts of anhydrous sodium acetate are added, and after continuous stirring evenly, the mixed solution is placed in an oil bath at 150 to 250°C and stirred at a speed of 1500 to 2500 r / min for 5 to 10 hours; after the reaction is complete, the precipitate is collected with a magnet, and after washing with water and ethanol for 3 to 6 times respectively, the obtained sample is dried in a 60 to 120°C forced air oven for 8 to 15 hours to obtain Fe3O4 microspheres with a particle size of 200 to 800 nm.
[0033] The Fe3O4 / SiO2 core-shell microspheres are surface-modified with PVP (polyvinyl pyrrolidone). On the one hand, it can promote the formation of good dispersion in the subsequent second solvent. On the other hand, it is also beneficial for the polypyrrole formed by polymerization to form a more complete coating on its surface during the in-situ polymerization process, and the polypyrrole coating layer is closely attached to its surface, which has a better promoting effect on the stability of the hollow structure after subsequent carbonization and etching. In order to further play this role, in a preferred embodiment, in step S2, the weight ratio of Fe3O4 / SiO2 core-shell microspheres to PVP is (1-6): (3-8). Preferably, the first solvent is an ethanol aqueous solution, more preferably an ethanol aqueous solution with a mass concentration of 50-80%. In this solvent, the dispersion and surface modification effects of Fe3O4 / SiO2 core-shell microspheres are better.
[0034] Exemplarily, the following steps can be used for PVP modification: by weight, 1 to 6 parts of Fe3O4 / SiO2 core-shell microspheres are dispersed in 50 to 400 parts of ethanol solution and ultrasonicated for 20 to 40 minutes, then 3 to 8 parts of PVP are added, and ultrasonication is continued for 40 to 60 minutes, and then the washed with distilled water for 3 to 6 times for standby use, and then the washed precipitate is placed in a 60 to 120°C forced air oven for drying for 8 to 15 hours to complete the PVP modification of the Fe3O4 / SiO2 core-shell microspheres.
[0035] In a preferred embodiment, the above step S3 includes: dispersing the Fe3O4 / SiO2 core-shell microspheres modified by PVP into a second solvent, then adding an oxidant and stirring for 30 to 80 minutes, and then adding pyrrole for polymerization to obtain Fe3O4 / SiO2 / PPy core-shell microspheres. Through the above process, under the action of the oxidant, pyrrole can be more stably completed on the surface of the Fe3O4 / SiO2 core-shell microspheres modified by PVP to complete in-situ polymerization, the coating effect is better, and the structural stability of the final hollow carbon material coated ferrite absorber powder is better promoted, which is beneficial to improve the comprehensive properties of the powder such as wave absorption performance, low density, and anti-agglomeration. Preferably, the weight ratio of Fe3O4 / SiO2 core-shell microspheres modified by PVP to the oxidant is (1 to 6): (5 to 10). In this way, the polymerization process of pyrrole is more stable. Preferably, the weight ratio of Fe3O4 / SiO2 core-shell microspheres modified by PVP to pyrrole is (1 to 6): (1 to 5). By controlling the amount of pyrrole within the above range, the thickness of the pyrrole is more suitable, and the thickness of the carbon coating layer finally formed is also more suitable. In addition to further reducing the powder density, increasing the dielectric constant and dielectric loss to further improve the absorption efficiency, it is also beneficial to avoid the problem of excessive reduction in magnetic permeability that is easily caused by the carbon coating, thereby improving the overall performance of the powder, such as matching and wave absorption.
[0036] To make the polymerization reaction more stable, in a preferred embodiment, the temperature during the polymerization reaction is 30-50°C, the stirring speed is 400-800 r / min, and the reaction time is 6-12 h. Preferably, the oxidant is ferric chloride; preferably, the second solvent is water.
[0037] Exemplarily, the preparation of Fe3O4 / SiO2 / PPy core-shell microspheres can be carried out by the following steps: by weight, 1 to 6 parts of PVP-modified Fe3O4 / SiO2 core-shell microspheres are dispersed in 100 to 400 parts of deionized water, 5 to 10 parts of ferric chloride are added after ultrasonic treatment for 15 to 30 minutes, 1 to 5 parts of pyrrole are added after stirring for 30 to 80 minutes, and the mixture is stirred in a water bath at 30 to 50°C at a speed of 400 to 800 r / min for 6 to 12 hours; after the reaction is completed, the precipitate is collected with a magnet, the supernatant is poured out, and the precipitate is washed with distilled water and ethanol for 3 to 6 times respectively, and the precipitate is dried in a blast oven at 40 to 80°C for 8 to 15 hours to obtain Fe3O4 / SiO2 / PPy core-shell microspheres with a particle size of 200 to 800 nm.
[0038] In order to make the polypyrrole layer carbonized more fully and make the carbon layer formed after calcination more stable, in a preferred embodiment, in step S4, during the calcination of Fe3O4 / SiO2 / PPy core-shell microspheres, the calcination temperature is 500-800°C and the calcination time is 2-6 hours. The inert gas used during this period includes but is not limited to nitrogen or argon. The specific calcination equipment can be a tubular furnace.
[0039] After calcination, the polypyrrole layer is carbonized to form a carbon layer with micropores, and the alkaline solution can penetrate the carbon layer into the interior and complete the etching of the SiO2 layer. In a preferred embodiment, in step S5, the alkaline solution is a sodium hydroxide aqueous solution with a concentration of 10 to 30 wt%, which has a better etching effect. Preferably, in step S5, after the carbonized microspheres are placed in the alkaline solution, the reaction is carried out for 10 to 20 hours at a stirring speed of 800 to 1500 r / min and a temperature of 40 to 80°C to etch and remove the SiO2 layer; preferably, in step S5, after the reaction is completed, the precipitate is separated and dried to obtain a hollow carbon material-coated ferrite absorber powder. Under the above conditions, the SiO2 layer can be etched more fully, and finally a hollow structure with a more complete and stable structure is formed.
[0040] Exemplarily, the following steps can be used to etch the SiO2 layer: disperse Fe3O4 / SiO2 / C microspheres (carbonized microspheres) in 100-400 parts by weight of a 10-30% sodium hydroxide aqueous solution for etching, stir at 800-1500 r / min at 40-80°C for 10-20 hours, collect the precipitate with a magnet, pour out the supernatant, wash with distilled water for 3-6 times, and dry the precipitate in a blast oven at 40-80°C for 8-15 hours to obtain the above hollow carbon material-coated ferrite absorber powder.
[0041] More preferably, in the above step S1, in the preparation process of Fe3O4 microspheres and Fe3O4 / SiO2 core-shell microspheres, the drying treatment time and temperature involved are preferably 80°C for 12 hours; the number of times the powder particles are washed is preferably 3 times. More preferably, in the above steps S2 to S5, the temperature during the drying process is preferably 60°C, the time is preferably 15 hours, and the number of times the powder particles are washed is 5 times.
[0042] According to another aspect of the present invention, there is also provided a hollow carbon material-coated ferrite absorber powder, which is prepared by the above-mentioned preparation method.
[0043] According to another aspect of the present invention, there is provided an absorbing material, comprising an absorbing powder, which is the above-mentioned hollow carbon material-coated ferrite absorber powder.
[0044] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0045] Comparative Example 1
[0046] A method for preparing Fe3O4 absorber powder comprises the following steps:
[0047] Preparation of Fe3O4 microspheres
[0048] Disperse 15 parts of iron salt (mass ratio FeCl3 / Fe(SO4)=6:5) into 600 parts of 99% ethylene glycol aqueous solution, stir evenly, then add 100 parts of anhydrous sodium acetate, continue stirring evenly, put the mixed solution into a 200°C oil bath and continue stirring at 2000r / min for 8h. After the reaction is complete, collect the precipitate with a magnet, wash it with water and ethanol for 5 times respectively, and then dry the obtained sample in a 80°C forced air oven for 12h to obtain Fe3O4 microspheres with a particle size of 400-600nm.
[0049] Example 1
[0050] A method for preparing a carbon-coated Fe3O4 absorber powder with a hollow core-shell structure comprises the following steps:
[0051] 1. Preparation of Fe3O4 microspheres
[0052] Disperse 15 parts of iron salt (mass ratio FeCl3 / Fe(SO4)=6:5) into 600 parts of 99% ethylene glycol aqueous solution, stir evenly, then add 100 parts of anhydrous sodium acetate, continue stirring evenly, put the mixed solution into a 200°C oil bath and continue stirring at 2000r / min for 8h. After the reaction is complete, collect the precipitate with a magnet, wash it with water and ethanol for 5 times respectively, and then dry the obtained sample in a 80°C forced air oven for 12h to obtain Fe3O4 microspheres with a particle size of 400-600nm.
[0053] 2. Preparation of Fe3O4 / SiO2 core-shell microspheres
[0054] Two parts of the prepared Fe3O4 microspheres were added to 1200 parts of anhydrous ethanol and 500 parts of deionized water, and ultrasonic treatment was performed for 30 minutes to uniformly disperse the Fe3O4 microspheres in the reaction solution. Dilute ammonia water was used as the pH adjusting liquid to control the pH of the reaction solution at about 8, and then 1 part of ethyl orthosilicate was dropped into the solution, and the mixture was stirred continuously for 3 hours at a speed of 500r / min in a water bath at 60°C. After the reaction was completed, the precipitate was collected with a magnet, the supernatant was poured out, and the mixture was washed with ethanol 5 times. The precipitate was placed in a 60°C blast oven and dried for 15 hours to complete the preparation of Fe3O4 / SiO2 core-shell microspheres.
[0055] 3. Modification of Fe3O4 / SiO2 core-shell microspheres
[0056] Disperse 1 part of Fe3O4 / SiO2 core-shell microspheres in 400 parts of ethanol solution and ultrasonicate for 20 minutes, then add 3 parts of PVP (polyvinyl pyrrolidone), continue ultrasonicate for 40 minutes, then wash with distilled water 5 times for standby use, then dry the washed precipitate in a 60°C forced air oven for 15 hours to complete the PVP modification of Fe3O4 / SiO2 core-shell microspheres.
[0057] 4. Preparation of Fe3O4 / SiO2 / PPy core-shell microspheres
[0058] Disperse 1 part of PVP-modified Fe3O4 / SiO2 core-shell microspheres in 400 parts of deionized water, add 5 parts of ferric chloride after ultrasonic treatment for 15 minutes, add 1 part of pyrrole after stirring for 30 minutes, and react at a speed of 400r / min for 8 hours under stirring in a 40°C water bath. After the reaction is completed, collect the precipitate with a magnet, pour out the supernatant, wash it with distilled water and ethanol for 5 times respectively, and dry the precipitate in a blast oven at 60°C for 15 hours to obtain Fe304 / SiO2 / PPy core-shell microspheres.
[0059] 5. Calcination
[0060] The Fe304 / SiO2 / PPy core-shell microspheres were calcined at 500°C for 3 h in a tubular furnace under nitrogen conditions to form carbonized microspheres.
[0061] 6. SiO2 layer etching
[0062] The carbonized microspheres were dispersed in 100 parts of a 10% sodium hydroxide aqueous solution for etching, stirred at 800 r / min at 40°C for 100 h, and the precipitate was collected with a magnet. The supernatant was poured out, washed with distilled water for 5 times, and the precipitate was dried in a blast oven at 60°C for 8 h to obtain Fe3O4 / C powder with a hollow core-shell structure.
[0063] Example 2
[0064] A method for preparing a carbon-coated Fe3O4 absorber powder with a hollow core-shell structure comprises the following steps:
[0065] 1. Preparation of Fe3O4 microspheres
[0066] Disperse 15 parts of iron salt (mass ratio FeCl3 / Fe(SO4)=6:5) into 600 parts of 99% ethylene glycol aqueous solution, stir evenly, then add 100 parts of anhydrous sodium acetate, continue stirring evenly, put the mixed solution into a 200°C oil bath and continue stirring at 2000r / min for 8h. After the reaction is complete, collect the precipitate with a magnet, wash it with water and ethanol for 5 times respectively, and then dry the obtained sample in a 80°C forced air oven for 12h to obtain Fe3O4 microspheres with a particle size of 400-600nm.
[0067] 2. Preparation of Fe3O4 / SiO2 core-shell microspheres
[0068] 5 parts of the prepared Fe3O4 microspheres were added to 1000 parts of anhydrous ethanol and 400 parts of deionized water, and ultrasonic treatment was performed for 40 minutes to make the Fe3O4 microspheres evenly dispersed in the reaction solution. Dilute ammonia water was used as the pH adjusting liquid to control the pH of the reaction solution at about 8, and then 3 parts of ethyl orthosilicate were dropped into the solution, and the mixture was stirred continuously for 4 hours at a speed of 800r / min in a water bath at 60°C. After the reaction was completed, the precipitate was collected with a magnet, the supernatant was poured out, and the precipitate was washed with ethanol 5 times. The precipitate was placed in an 80°C blast oven and dried for 12 hours to complete the preparation of Fe3O4 / SiO2 core-shell microspheres.
[0069] 3. Modification of Fe3O4 / SiO2 core-shell microspheres
[0070] Disperse 4 parts of Fe3O4 / SiO2 core-shell microspheres in 200 parts of ethanol solution and ultrasonicate for 30 minutes. Then add 6 parts of PVP (polyvinyl pyrrolidone). After continuous ultrasonication for 50 minutes, wash with distilled water for 5 times for standby use. Then, dry the washed precipitate in an 80°C forced air oven for 12 hours to complete the PVP modification of Fe3O4 / SiO2 core-shell microspheres.
[0071] 4. Preparation of Fe3O4 / SiO2 / PPy core-shell microspheres
[0072] Disperse 4 parts of PVP-modified Fe3O4 / SiO2 core-shell microspheres in 200 parts of deionized water, add 8 parts of ferric chloride after ultrasonic treatment for 20 minutes, add 3 parts of pyrrole after stirring for 60 minutes, and react at a speed of 600r / min for 10 hours under stirring in a 50°C water bath. After the reaction is completed, collect the precipitate with a magnet, pour out the supernatant, wash it with distilled water and ethanol for 5 times respectively, and dry the precipitate in a blast oven at 60°C for 15 hours to obtain Fe304 / SiO2 / PPy core-shell microspheres.
[0073] 5. Calcination
[0074] The Fe304 / SiO2 / PPy core-shell microspheres were calcined at 600°C for 4 h in a tubular furnace under nitrogen conditions to form carbonized microspheres.
[0075] 6. SiO2 layer etching
[0076] The carbonized microspheres were dispersed in 200 parts of a 20% sodium hydroxide aqueous solution for etching, stirred at 1000 r / min at 60°C for 15 hours, and the precipitate was collected with a magnet. The supernatant was poured out, washed with distilled water for 5 times, and the precipitate was dried in a blast oven at 60°C for 15 hours to obtain Fe3O4 / C powder with a hollow core-shell structure.
[0077] Example 3
[0078] A method for preparing a carbon-coated Fe3O4 absorber powder with a hollow core-shell structure includes the following two steps:
[0079] 1. Preparation of Fe3O4 microspheres
[0080] Disperse 15 parts of iron salt (mass ratio FeCl3 / Fe(SO4)=6:5) into 600 parts of 99% ethylene glycol aqueous solution, stir evenly, then add 100 parts of anhydrous sodium acetate, continue stirring evenly, put the mixed solution into a 200°C oil bath and continue stirring at 2000r / min for 8h. After the reaction is complete, collect the precipitate with a magnet, wash it with water and ethanol for 5 times respectively, and then dry the obtained sample in a 80°C forced air oven for 12h to obtain Fe3O4 microspheres with a particle size of 400-600nm.
[0081] 2. Preparation of Fe3O4 / SiO2 core-shell microspheres
[0082] 10 parts of the prepared Fe3O4 microspheres were added to 800 parts of anhydrous ethanol and 200 parts of deionized water, and ultrasonic treatment was performed for 50 minutes to uniformly disperse the Fe3O4 microspheres in the reaction solution. Dilute ammonia water was used as the pH adjusting liquid to control the pH of the reaction solution at about 9, and then 6 parts of ethyl orthosilicate were dropped into the solution, and the mixture was stirred continuously for 6 hours in a water bath at 80°C at a speed of 1000 r / min. After the reaction was completed, the precipitate was collected with a magnet, the supernatant was poured out, and the precipitate was washed with ethanol 5 times. The precipitate was placed in an 80°C blast oven and dried for 12 hours to complete the preparation of Fe3O4 / SiO2 core-shell microspheres.
[0083] 3. Modification of Fe3O4 / SiO2 core-shell microspheres
[0084] Disperse 6 parts of Fe3O4 / SiO2 core-shell microspheres in 50 parts of ethanol solution and ultrasonicate for 40 minutes, then add 8 parts of PVP (polyvinyl pyrrolidone), continue ultrasonication for 60 minutes, and then wash with distilled water for 5 times for standby use. Then, place the washed precipitate in an 80°C forced air oven and dry it for 12 hours to complete the PVP modification of Fe3O4 / SiO2 core-shell microspheres.
[0085] 4. Preparation of Fe3O4 / SiO2 / PPy core-shell microspheres
[0086] Disperse 6 parts of PVP-modified Fe3O4 / SiO2 core-shell microspheres into 100 parts of deionized water, add 10 parts of ferric chloride after ultrasonic treatment for 30 minutes, add 5 parts of pyrrole after stirring for 80 minutes, and react at a speed of 800r / min for 12 hours under stirring in a 50°C water bath. After the reaction is completed, collect the precipitate with a magnet, pour out the supernatant, wash it with distilled water and ethanol for 5 times respectively, and dry the precipitate in a blast oven at 60°C for 15 hours to obtain Fe304 / SiO2 / PPy core-shell microspheres.
[0087] 5. Calcination
[0088] The Fe304 / SiO2 / PPy core-shell microspheres were calcined at 800°C for 6 h in a tubular furnace under nitrogen conditions to form carbonized microspheres.
[0089] 6. SiO2 layer etching
[0090] The carbonized microspheres are dispersed in 100 parts of a 30% mass concentration sodium hydroxide aqueous solution for etching, stirred at 1500 r / min at 60°C for 20 hours, and the precipitate is collected with a magnet. The supernatant is poured out, washed with distilled water for 5 times, and the precipitate is placed in a blast oven at 60°C and dried for 15 hours to obtain Fe3O4 / C powder with a hollow core-shell structure.
[0091] Example 4
[0092] A method for preparing a carbon-coated Fe3O4 absorber powder with a hollow core-shell structure includes the following two steps:
[0093] 1. Preparation of Fe3O4 microspheres
[0094] Disperse 5 parts of iron salt (mass ratio FeCl3 / Fe(SO4)=6:5) into 800 parts of 99% ethylene glycol solution, stir evenly and add 150 parts of anhydrous sodium acetate. After continuous stirring, put the mixed solution into an oil bath at 250°C and stir continuously at 1500r / min for 5h. After the reaction is complete, collect the precipitate with a magnet, wash it with water and ethanol for 5 times respectively, and then dry the obtained sample in a blast oven at 80°C for 12h to obtain Fe3O4 microspheres with a particle size of 200-300nm.
[0095] 2. Preparation of Fe3O4 / SiO2 core-shell microspheres
[0096] 5 parts of the prepared Fe3O4 microspheres were added to 1000 parts of anhydrous ethanol and 400 parts of deionized water, and ultrasonic treatment was performed for 40 minutes to make the Fe3O4 microspheres evenly dispersed in the reaction solution. Dilute ammonia water was used as the pH adjusting liquid to control the pH of the reaction solution at about 8, and then 3 parts of ethyl orthosilicate were dropped into the solution, and the mixture was stirred continuously for 4 hours at a speed of 800r / min in a water bath at 60°C. After the reaction was completed, the precipitate was collected with a magnet, the supernatant was poured out, and the precipitate was washed with ethanol 5 times. The precipitate was placed in an 80°C blast oven and dried for 12 hours to complete the preparation of Fe3O4 / SiO2 core-shell microspheres.
[0097] 3. Modification of Fe3O4 / SiO2 core-shell microspheres
[0098] Disperse 4 parts of Fe3O4 / SiO2 core-shell microspheres in 200 parts of ethanol solution and ultrasonicate for 30 minutes. Then add 6 parts of PVP (polyvinyl pyrrolidone). After continuous ultrasonication for 50 minutes, wash with distilled water for 5 times for standby use. Then, dry the washed precipitate in an 80°C forced air oven for 12 hours to complete the PVP modification of Fe3O4 / SiO2 core-shell microspheres.
[0099] 4. Preparation of Fe3O4 / SiO2 / PPy core-shell microspheres
[0100] Disperse 4 parts of PVP-modified Fe3O4 / SiO2 core-shell microspheres in 200 parts of deionized water, add 8 parts of ferric chloride after ultrasonic treatment for 20 minutes, add 3 parts of pyrrole after stirring for 60 minutes, and react at a speed of 600r / min for 10 hours under stirring in a 50°C water bath. After the reaction is completed, collect the precipitate with a magnet, pour out the supernatant, wash it with distilled water and ethanol for 5 times respectively, and dry the precipitate in a blast oven at 60°C for 15 hours to obtain Fe304 / SiO2 / PPy core-shell microspheres.
[0101] 5. Calcination
[0102] The Fe304 / SiO2 / PPy core-shell microspheres were calcined at 600°C for 4 h in a tubular furnace under nitrogen conditions to form carbonized microspheres.
[0103] 6. SiO2 layer etching
[0104] The carbonized microspheres were dispersed in 200 parts of a 20% sodium hydroxide aqueous solution for etching, stirred at 1000 r / min at 60°C for 15 hours, and the precipitate was collected with a magnet. The supernatant was poured out, washed with distilled water for 5 times, and the precipitate was dried in a blast oven at 60°C for 15 hours to obtain Fe3O4 / C powder with a hollow core-shell structure.
[0105] Example 5
[0106] A method for preparing a carbon-coated Fe3O4 absorber powder with a hollow core-shell structure includes the following two steps:
[0107] 1. Preparation of Fe3O4 microspheres
[0108] Disperse 30 parts of iron salt (mass ratio (Fel3) / Fe(SO4)=6:5) into 400 parts of 99% ethylene glycol solution, stir evenly and add 20 parts of anhydrous sodium acetate. After continuous stirring, put the mixed solution into an oil bath at 150°C and stir at 2000r / min for 10 hours. After the reaction is complete, collect the precipitate with a magnet, wash it with water and ethanol for 5 times respectively, and then dry the obtained sample in a blast oven at 80°C for 12 hours to obtain Fe3O4 microspheres with a particle size of 600-800nm.
[0109] 2. Preparation of Fe3O4 / SiO2 core-shell microspheres
[0110] 5 parts of the prepared Fe3O4 microspheres were added to 1000 parts of anhydrous ethanol and 400 parts of deionized water, and ultrasonic treatment was performed for 40 minutes to make the Fe3O4 microspheres evenly dispersed in the reaction solution. Dilute ammonia water was used as the pH adjusting liquid to control the pH of the reaction solution at about 8, and then 3 parts of ethyl orthosilicate were dropped into the solution, and the mixture was stirred continuously for 4 hours at a speed of 800r / min in a water bath at 60°C. After the reaction was completed, the precipitate was collected with a magnet, the supernatant was poured out, and the precipitate was washed with ethanol 5 times. The precipitate was placed in an 80°C blast oven and dried for 12 hours to complete the preparation of Fe3O4 / SiO2 core-shell microspheres.
[0111] 3. Modification of Fe3O4 / SiO2 core-shell microspheres
[0112] Disperse 4 parts of Fe3O4 / SiO2 core-shell microspheres in 200 parts of ethanol solution and ultrasonicate for 30 minutes. Then add 6 parts of PVP (polyvinyl pyrrolidone). After continuous ultrasonication for 50 minutes, wash with distilled water for 5 times for standby use. Then, dry the washed precipitate in an 80°C forced air oven for 12 hours to complete the PVP modification of Fe3O4 / SiO2 core-shell microspheres.
[0113] 4. Preparation of Fe3O4 / SiO2 / PPy core-shell microspheres
[0114] Disperse 4 parts of PVP-modified Fe3O4 / SiO2 core-shell microspheres in 200 parts of deionized water, add 8 parts of ferric chloride after ultrasonic treatment for 20 minutes, add 3 parts of pyrrole after stirring for 60 minutes, and react at a speed of 600r / min for 10 hours under stirring in a 50°C water bath. After the reaction is completed, collect the precipitate with a magnet, pour out the supernatant, wash it with distilled water and ethanol for 5 times respectively, and dry the precipitate in a blast oven at 60°C for 15 hours to obtain Fe304 / SiO2 / PPy core-shell microspheres.
[0115] 5. Calcination
[0116] The Fe304 / SiO2 / PPy core-shell microspheres were calcined at 600°C for 4 h in a tubular furnace under nitrogen conditions to form carbonized microspheres.
[0117] 6. SiO2 layer etching
[0118] The carbonized microspheres were dispersed in 200 parts of a 20% sodium hydroxide aqueous solution for etching, stirred at 1000 r / min at 60°C for 15 hours, and the precipitate was collected with a magnet. The supernatant was poured out, washed with distilled water for 5 times, and the precipitate was dried in a blast oven at 60°C for 15 hours to obtain Fe3O4 / C powder with a hollow core-shell structure.
[0119] Performance characterization:
[0120] 8 portions of Fe3O4 particles and hollow Fe3O4 / C powders prepared in Comparative Example 1, Example 1 to Example 5 were prepared into 80% coaxial samples and tested. The main steps were: first, the powders were mixed with paraffin in a weight ratio of 8:2, placed in a high-temperature oven at 65°C and heated for 10 minutes, then quickly taken out and mixed and stirred evenly to form a viscous solid and filled into a coaxial ring mold (mold outer diameter 7mm, inner diameter 3.04mm), and 1-2mm thick samples were prepared respectively, and then the complex dielectric constant (ε′) and complex magnetic permeability (μ′) were measured by network vector analyzer, and then the reflection loss of the test sample at a thickness of 2.5mm was calculated by matlab simulation according to the electromagnetic field transmission line theory. The tap density of the powder was measured with a tap density meter. The powder was added to 25% dilute hydrochloric acid, and the time for the solution to produce bubbles or the solution color to change was observed. The characterization results are shown in Table 1:
[0121] Table 1
[0122] Comparative Example 1 Example 1 Example 2 Example 3 Example 4 Example 5 Average particle size 402nm 405nm 410nm 420nm 220nm 760nm ε′(6GHz) 10.64 8.23 9.77 10.88 9.15 11.32 μ′(6GHz) 1.39 1.61 1.56 1.44 1.42 1.66 Frequency(GHz) 6.93 6.71 6.56 6.43 6.31 6.48 Absorption peak(dB) -26 -32 -35 -28 -29 -31 Bandwidth (≤10dB) 2.6 3.8 3.9 3.5 3.3 3.4 Tap density 2.67 1.63 1.23 1.18 1.33 1.42 Acid corrosion resistance (color) 12min 106min 255min 294min 238min 267min
[0123] Generally, low dielectric constant and high magnetic permeability will form a better impedance match. The lower the absorption peak intensity, the better the absorption effect.
[0124] Through the above tests, it was found that: compared with the Fe3O4 microspheres prepared in Comparative Example 1, the hollow Fe3O4 / C prepared in Examples 1 to 5 of the present invention has a lower density, better absorption efficiency and bandwidth, and the hollow structure produces multiple reflections and multiple absorptions, the propagation path of electromagnetic waves is increased, and the acid and alkali corrosion resistance of the powder is greatly improved compared with the Fe3O4 microspheres; the hollow Fe3O4 / C powder in Examples 1 to 3, with the increase of carbon coating content, the powder density and magnetic permeability decrease accordingly, the dielectric constant increases, the dielectric loss inside the material is increased, and more It is easy to form an effective conductive network structure and increase the absorption efficiency, but the reduction of magnetic permeability will have some impact on the absorption efficiency; in the powder performance of Examples 4, 2, and 5, as the generated Fe3O4 particle size increases, the prepared hollow Fe3O4 / C particle size is too large, the dielectric effect increases significantly, which is not conducive to impedance matching, and the density will also increase accordingly; but the prepared hollow Fe3O4 / C particle size is too small, the magnetic loss effect will be reduced, which is not conducive to the improvement of the absorption efficiency intensity; therefore, finding a more suitable particle size range is conducive to obtaining better absorption performance. In Example 2, the powder density is significantly reduced, the acid and alkali corrosion resistance is significantly improved, and it can achieve better magnetic permeability and dielectric constant, has a more suitable particle size, and has better absorption efficiency and absorption bandwidth.
[0125] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a hollow carbon material-coated ferrite absorber powder, It is characterized in that The following steps are involved: Step S1, in Fe 3 O 4 The surface of the microspheres is coated with SiO 2 layer, forming Fe 3 O 4 / SiO 2 Core-shell microspheres; the Fe 3 O 4 The particle size of the microspheres is 200~800nm; Step S2, the Fe 3 O 4 / SiO 2 The core-shell microspheres are dispersed in a first solvent, and then PVP is added to the Fe 3 O 4 / SiO 2 The core-shell microspheres were surface modified to form PVP-modified Fe 3 O 4 / SiO 2 Core-shell microspheres; Step S3, the PVP-modified Fe 3 O 4 / SiO 2 The core-shell microspheres are dispersed in a second solvent, and then an oxidant and pyrrole are added and a polymerization reaction is performed to form a Fe 3 O 4 / SiO 2 The surface of the core-shell microspheres further forms a PPy coating layer, thereby obtaining Fe 3 O 4 / SiO 2 / PPy core-shell microspheres; the PVP-modified Fe 3 O 4 / SiO 2 The weight ratio of the core-shell microspheres to the pyrrole is 1:1 to 6:5; Step S4, calcining the Fe 3 O 4 / SiO 2 / PPy core-shell microspheres, so that the PPy coating layer is carbonized to obtain carbonized microspheres; Step S5, placing the carbonized microspheres in an alkaline solution to etch away the SiO 2 layer, thereby forming the hollow carbon material-coated ferrite absorber powder.
2. The preparation method according to claim 1, It is characterized in that The step S1 comprises: The Fe 3 O 4 The microspheres are dispersed in a third solvent to form a dispersion; The pH value of the dispersion is adjusted to 8-9, and then ethyl orthosilicate is added thereto, and reacted under stirring to obtain a reaction slurry; The solid in the reaction slurry is separated and dried to obtain the Fe 3 O 4 / SiO 2 Core-shell microspheres.
3. The preparation method according to claim 2, It is characterized in that The Fe 3 O 4 The weight ratio of the microspheres to the tetraethyl orthosilicate is (2-10):(1-6).
4. The preparation method according to claim 2, It is characterized in that The third solvent is a mixed solvent of ethanol and water, and the weight ratio of the two is (8-12): (2-5).
5. The preparation method according to claim 2, It is characterized in that Ammonia water is used as a reagent for adjusting the pH value of the dispersion.
6. The preparation method according to claim 2, It is characterized in that After adding the tetraethyl orthosilicate, the mixture is reacted for 3 to 6 hours at a stirring speed of 400 to 1000 r / min and a temperature of 40 to 80° C.
7. The preparation method according to any one of claims 2 to 6, It is characterized in that The Fe 3 O 4 The microspheres are prepared by the following method: dispersing a divalent iron salt and a trivalent iron salt in a fourth solvent, then adding a base to react, separating the solid and the liquid, and drying to obtain the Fe 3 O 4 Microspheres.
8. The preparation method according to claim 7, It is characterized in that The divalent iron salt is ferrous chloride and / or ferrous sulfate, and the trivalent iron salt is ferric chloride and / or ferric sulfate.
9. The preparation method according to claim 7, It is characterized in that The base is anhydrous sodium acetate.
10. The preparation method according to claim 7, It is characterized in that The total weight of the divalent iron salt and the trivalent iron salt is recorded as m1, and the weight of the base is recorded as m2, then m1 / m2 is (1-6):(4-30).
11. The preparation method according to claim 7, It is characterized in that The fourth solvent is an ethylene glycol aqueous solution with a mass concentration of 96-99%.
12. The preparation method according to claim 7, It is characterized in that After adding the base, the reaction is carried out for 5 to 10 hours at a stirring speed of 1500 to 2500 r / min and a temperature of 150 to 250° C.
13. The preparation method according to any one of claims 1 to 6, It is characterized in that In the step S2, the Fe 3 O 4 / SiO 2 The weight ratio of the core-shell microspheres to the PVP is (1-6): (3-8).
14. The preparation method according to claim 1, It is characterized in that The first solvent is an ethanol aqueous solution.
15. The preparation method according to claim 14, It is characterized in that The first solvent is an ethanol aqueous solution with a mass concentration of 50-80%.
16. The preparation method according to any one of claims 1 to 6, It is characterized in that The step S3 comprises: The PVP-modified Fe 3 O 4 / SiO 2 The core-shell microspheres are dispersed in a second solvent, and then the oxidant is added and stirred for 30 to 80 minutes, and then the pyrrole is added to carry out the polymerization reaction to obtain the Fe 3 O 4 / SiO 2 / PPy core-shell microspheres.
17. The preparation method according to claim 16, It is characterized in that The PVP-modified Fe 3 O 4 / SiO 2 The weight ratio of the core-shell microspheres to the oxidant is (1-6): (5-10).
18. The preparation method according to claim 16, It is characterized in that The temperature during the polymerization reaction is 30-50° C., the stirring speed is 400-800 r / min, and the reaction time is 6-12 h.
19. The preparation method according to claim 16, It is characterized in that The oxidant is ferric chloride; the second solvent is water.
20. The preparation method according to any one of claims 1 to 6, It is characterized in that In step S4, the Fe 3 O 4 / SiO 2 In the process of preparing / PPy core-shell microspheres, the calcination temperature is 500~800℃, and the calcination time is 2~6h.
21. The preparation method according to any one of claims 1 to 6, It is characterized in that In step S5, the alkaline solution is a sodium hydroxide aqueous solution with a concentration of 10-30 wt%.
22. The preparation method according to claim 21, It is characterized in that In step S5, after placing the carbonized microspheres in an alkaline solution, the reaction is carried out for 10 to 20 hours at a stirring speed of 800 to 1500 r / min and a temperature of 40 to 80° C. to etch and remove the SiO 2 layer.
23. The preparation method according to claim 22, It is characterized in that In the step S5, after the reaction is completed, the precipitate is separated and dried to obtain the hollow carbon material-coated ferrite absorber powder.
24. A hollow carbon material coated ferrite absorber powder, It is characterized in that The method is prepared according to any one of claims 1 to 23.
25. A wave absorbing material, comprising wave absorbing powder, It is characterized in that The absorbing powder is the hollow carbon material-coated ferrite absorber powder as described in claim 24.
Citation Information
Patent Citations
Preparation method of yolk type double-shell-layer hollow composite wave absorption material
CN108330471A
Fe3O4 / SiO2 / PPy composite microsphere of core-shell structure and preparing method thereof
CN108479732A
Ferroferric oxide / polypyrrole composite material and preparation method thereof
CN108976820A
Titanium dioxide coated ferroferric oxide hollow microsphere composite material as well as preparation method and application thereof
CN112094622A
Hollow microsphere core-shell structure wave-absorbing material as well as preparation method and application thereof
CN112226203A