Method for producing propylene by direct dehydrogenation of propane and catalyst and preparation method thereof
By forming a MeOx semiconductor film layer on the SBA-15 support and anchoring the PtSn/@-MeOx/SBA-15 catalyst of Pt and Sn nanoparticles, the problems of easy deactivation and environmental impact of Pt-based catalysts are solved, and low-cost is achieved , efficient propane dehydrogenation maintains catalyst activity and propylene selectivity, and is suitable for industrial applications.
Patent Information
- Application Number
- CN202310269423.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-03-20
AI Technical Summary
In the existing direct propane dehydrogenation process, Pt-based catalysts are prone to deactivate, and Sn additives have various states that lead to a decrease in catalyst activity. The noble metal catalysts have an impact on the environment, and the reaction conditions require high purity of raw material gas and have high economic costs. .
PtSn/@-MeOx/SBA-15 platinum-tin hybrid nanostructured catalyst was used to form a MeOx semiconductor film layer by microwave heating, and Pt and Sn nanoparticles were anchored by photocatalytic reduction to form a synergistic catalyst. Sn was both SnOx The state exists, reducing the Pt content and improving the dehydrogenation activity and stability of propane.
It achieves low-cost and efficient propane dehydrogenation, the catalyst remains active during recycling, has high propylene selectivity, long and stable reaction time, and is suitable for industrial applications.
Smart Images

Figure CN116273137B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysts, and specifically relates to a method for preparing propylene by direct dehydrogenation of propane and a platinum-tin hybrid nanostructured catalyst and a preparation method thereof. Background Art
[0002] In the petrochemical industry, propylene is an important chemical intermediate and chemical raw material. There is a large market demand for downstream propylene products such as polypropylene, acrylic acid, and propylene oxide. With people's attention to and exploitation of shale gas, the output of propane has been greatly improved, and direct dehydrogenation of propane has naturally received more attention. At present, the industrial propane direct dehydrogenation process can be divided into two types: direct dehydrogenation of propane and propane oxidative dehydrogenation. The direct dehydrogenation processes of propane are the Oleflex process and the Catofin process, which account for more than 90% of the direct dehydrogenation capacity of propane that has been put into production worldwide. The reactor used in the Oleflex process is a moving bed, the reaction temperature is 580℃~650℃, the single-pass conversion rate is 30%~40%, the selectivity is 89%~91%, and the catalyst used is Pt-Sn / Al 2 O 3 The characteristics of this process technology are high selectivity and stability for propylene, but the Pt-based catalyst is expensive, the purity of the reaction raw gas is high, and the catalyst is prone to carbon deposition during the reaction. The reactor used in the Catofin process is a fixed bed, the reaction temperature is 560℃~650℃, the single-pass conversion rate is 48%~65%, the propylene selectivity is 85%~90%, and the catalyst used is CrOx / Al 2 O 3 This process technology is characterized by high dehydrogenation activity and relatively loose operating conditions, but Cr-based catalysts, as heavy metal catalysts, will have an impact on the environment.
[0003] There are two main reasons for the deactivation of precious metal Pt-based catalysts. One is that the coke produced by the side reactions during the reaction covers the active site Pt, resulting in a decrease in the dehydrogenation activity of the catalyst. The other is that the Pt particles are easily agglomerated and sintered during the reaction, resulting in a loss of catalytic activity. Sn is the most used and studied additive in dehydrogenation Pt-based catalysts. All industrial dehydrogenation Pt-based catalysts contain this transition metal. The addition of Sn can increase the dispersion of Pt particles to form smaller Pt particles, and can change the adsorption properties of Pt. However, Sn exists in multiple states. SnOx promotes the dehydrogenation of Pt-based catalysts, and Sn 0 It tends to adsorb on the surface of Pt particles, covering the catalyst surface and reducing the catalyst activity. Summary of the invention
[0004] The purpose of the present invention is to improve a catalyst with the expression of PtSn / @-MeOx / SBA-15, which is a hybrid nanostructured catalyst, has a simple preparation process, mild preparation conditions, a low Pt content in the catalyst, can reduce economic costs, and Sn is in the form of SnO x It exists in a state and has excellent propane dehydrogenation activity and stability.
[0005] In order to achieve the above object, the present invention provides a platinum-tin hybrid nanostructure catalyst for direct dehydrogenation of propane to propylene, comprising a composite carrier and an active component and an auxiliary agent supported on the composite carrier, wherein the active component is Pt, the auxiliary agent is Sn, and the composite carrier is MeO x / SBA-15, recorded as PtSn / @-MeOx / SBA-15, MeOx is CeO 2 or La 2 O 3 ; Wherein, the composite carrier MeO x / MeOx in SBA-15 is heated by microwaves to form MeO in a single layer or multiple layers on the SBA-15 molecular sieve. x Semiconductor film layer, the active component Pt and the auxiliary agent Sn in the catalyst PtSn / @-MeOx / SBA-15 are anchored on the composite carrier MeO in the form of nanoparticles through photocatalytic reduction method x / SBA-15, the active component Pt and the MeO x There is a synergistic effect among the semiconductor film layers.
[0006] Preferably, the catalyst PtSn / @-MeO x The mass content of Pt in the SBA-15 is 0.1-3%, and the molar ratio of the active component Pt to the auxiliary agent Sn is 1:(1 / 3-2); the composite carrier MeO x / The mass content of MeOx in SBA-15 is 5-20%.
[0007] More preferably, the mass content of Pt in the catalyst PtSn / @-MeOx / SBA-15 is 0.5-1.0%, and the molar ratio of the active component Pt to the auxiliary agent Sn is 1:1.
[0008] More preferably, the composite support CeO 2 CeO in SBA-15 2 The mass content of La is 5-15%, and the composite carrier La 2 O 3 / La in SBA-15 2 O 3 The mass content is 10-15%.
[0009] The present invention also provides a method for preparing a platinum-tin hybrid nanostructure catalyst for direct dehydrogenation of propane to propylene, the preparation method comprising the steps of:
[0010] (1) SBA-15 molecular sieve is uniformly dispersed in a cerium salt solution or a lanthanum salt solution, and then a precipitant is added to adjust the pH value to 7-10, and then stirring is continued for a first preset time. The resulting solution is placed in a microwave reaction device and heated under preset heating conditions for reaction, and then solid-liquid separation and drying are performed to obtain a composite carrier MeO x / SBA-15, of which MeO x CeO 2 or La 2 O 3 ;
[0011] (2) The active component Pt and the auxiliary agent Sn are anchored on the composite carrier MeOx / SBA-15 in the form of nanoparticles by photocatalytic reduction to obtain the catalyst PtSn / @-MeO x / SBA-15.
[0012] Preferably, the composite carrier MeO in step (1) x / MeO in SBA-15 x Mass content is 5-20% 3 ; The mass content of Pt in the catalyst PtSn / @-MeOx / SBA-15 in step (2) is 0.1 to 3%, and the molar ratio of the active component Pt to the auxiliary agent Sn is 1: (1 / 3 to 2).
[0013] More preferably, the mass content of Pt in the catalyst PtSn / @-MeOx / SBA-15 is 0.5-1.0%, and the molar ratio of the active component Pt to the auxiliary agent Sn is 1:1.
[0014] More preferably, the composite support CeO 2 CeO in SBA-15 2 The mass content of La is 5-15%, and the composite carrier La 2 O 3 / La in SBA-15 2 O 3 The mass content is 10-15%.
[0015] Preferably, the cerium salt solution is a cerium nitrate solution, and the lanthanum salt solution is a lanthanum nitrate solution.
[0016] More preferably, the composite carrier prepared in step (1) is CeO 2 / SBA-15, add a precipitant to adjust the pH value to 9-10; the composite carrier prepared in step (1) is La2 O 3 / SBA-15, add precipitant to adjust the pH value to 7-8.
[0017] Preferably, the precipitant is a 50 g / ml ammonia solution.
[0018] Preferably, the first preset time is 15 to 30 minutes.
[0019] Preferably, the preset heating conditions in step (1) include: a heating reaction time of 10 to 20 minutes and a microwave power of 200 to 600W.
[0020] Preferably, in step (1), the drying temperature is 60 to 120° C. and the drying time is 12 to 24 hours.
[0021] Preferably, the photocatalytic reduction method is specifically: the composite carrier MeO prepared in step (1) x / SBA-15 is added to water and anhydrous methanol, and ultrasonically dispersed evenly; then chloroplatinic acid solution and tin chloride solution are added, and ultrasonic oscillation is continued for a second preset time; then the catalyst is placed under an ultraviolet lamp and stirred under light conditions, and the stirred solution is filtered and vacuum dried to obtain the catalyst PtSn / @-MeOx / SBA-15.
[0022] More preferably, in the photocatalytic reduction method, the second preset time of ultrasonic oscillation is 10 to 20 minutes, and stirring is performed under ultraviolet light for 12 hours; the temperature of vacuum drying is 75° C. to 85° C., and the drying time is 8 to 12 hours.
[0023] Preferably, the catalyst is pretreated after step (2), specifically, the catalyst PtSn / @-MeO prepared in step 2) is treated with x / SBA-15 is filled into a micro fixed bed reactor, and an inert gas with a content of 10-40 vol% is introduced for pretreatment for 30-120 minutes, wherein the pretreatment temperature is 500-580°C.
[0024] The present invention also provides a platinum-tin hybrid nanostructure catalyst, which is prepared by the preparation method described above.
[0025] The present invention also provides a method for preparing propylene by direct dehydrogenation of propane, which comprises using a pretreated catalyst PtSn / @-MeOx / SBA-15 to catalyze the dehydrogenation reaction of propane gas to produce propylene, the reaction pressure is normal pressure, and the reaction temperature is 550° C. The catalyst PtSn / @-MeOx / SBA-15 comprises a composite carrier and an active component and an auxiliary agent loaded on the composite carrier, wherein the active component is Pt, the auxiliary agent is Sn, and the composite carrier is MeOx / SBA-15. The catalyst PtSn / @-MeOx / SBA-15 is prepared by the following method, including:
[0026] The SBA-15 molecular sieve is uniformly dispersed in a cerium salt solution or a lanthanum salt solution, and then a precipitant is added to adjust the pH value to 7-10, and then the stirring is continued for a first preset time. The obtained solution is placed in a microwave reaction device and heated to react under preset heating conditions, and then the composite carrier MeO is obtained by solid-liquid separation and drying. x / SBA-15, of which MeO x CeO 2 or La 2 O 3 ;
[0027] The active component Pt and the auxiliary agent Sn are anchored on the composite carrier MeOx / SBA-15 in the form of nanoparticles by photocatalytic reduction to obtain the catalyst PtSn / @-MeO x / SBA-15.
[0028] Preferably, the propane content in the propane gas is 20-100 vol%, and the gas weight hourly space velocity of the propane is 5-18 h -1 .
[0029] Preferably, the pretreatment method of the catalyst PtSn / @-MeOx / SBA-15 is: fill the catalyst PtSn / @-MeOx / SBA-15 into a micro fixed bed reactor, introduce an inert gas with a content of 10 to 40 vol% for pretreatment for 30 to 120 minutes, wherein the pretreatment temperature is 500 to 580°C.
[0030] More preferably, the inert gas is argon.
[0031] Preferably, the composite carrier MeO x / MeO in SBA-15 x The mass content is 5-20%; more preferably, the composite carrier CeO 2 CeO in SBA-15 2 The mass content of La is 5-15%, and the composite carrier La 2 O 3 / La in SBA-15 2 O 3 The mass content is 10-15%.
[0032] Preferably, the mass content of Pt in the catalyst PtSn / @-MeOx / SBA-15 is 0.1-3%, and the molar ratio of the active component Pt to the auxiliary agent Sn is 1:(1 / 3-2). More preferably, the mass content of Pt in the catalyst PtSn / @-MeOx / SBA-15 is 0.5-1.0%, and the molar ratio of the active component Pt to the auxiliary agent Sn is 1:1.
[0033] Preferably, the cerium salt solution is a cerium nitrate solution, and the lanthanum salt solution is a lanthanum nitrate solution.
[0034] More preferably, the prepared composite carrier is CeO 2 / SBA-15, adding a precipitant to adjust the pH value to 9-10; the prepared composite carrier is La 2 O 3 / SBA-15, add precipitant to adjust the pH value to 7-8.
[0035] Preferably, the precipitant is a 50 g / ml ammonia solution.
[0036] Preferably, the first preset time is 15 to 30 minutes.
[0037] Preferably, the preset heating conditions include: heating reaction time of 10 to 20 minutes, and microwave power of 200 to 600W.
[0038] Preferably, the composite carrier MeO is prepared x / The corresponding drying temperature of SBA-15 is 60-120℃ and the drying time is 12-24h.
[0039] Preferably, the photocatalytic reduction method is specifically: the composite carrier MeO x / SBA-15 is added to water and anhydrous methanol, and ultrasonically dispersed uniformly; then chloroplatinic acid solution and tin chloride solution are added, and ultrasonic oscillation is continued for a second preset time; then placed under an ultraviolet lamp, stirred under light conditions, and the stirred solution is filtered and vacuum dried to obtain the catalyst PtSn / @-MeO x / SBA-15.
[0040] More preferably, in the photocatalytic reduction method, the second preset time of ultrasonic oscillation is 10 to 20 minutes, and stirring is performed under ultraviolet light for 12 hours; the temperature of vacuum drying is 75° C. to 85° C., and the drying time is 8 to 12 hours.
[0041] The beneficial effects of the present invention include at least:
[0042] 1. The catalyst PtSn / @-MeOx / SBA-15 provided by the present invention comprises Pt as an active component, Sn as an auxiliary agent, and CeO 2 / SBA-15 or La 2 O 3 / SBA-15 is a composite carrier, composite carrier MeO x / MeO in SBA-15 x MeO was formed by microwave heating reaction in the form of single layer or multilayer on SBA-15 molecular sieve x Semiconductor film layer, active component Pt and auxiliary agent Sn in the form of nanoparticles are anchored on the composite carrier MeO by photocatalytic reduction method x / SBA-15, the active component Pt and the MeO x The semiconductor film layer has a synergistic effect; thus, the present invention makes full use of the semiconductor metal oxide MeO x The photocatalytic reduction properties of the catalyst are such that Pt and Sn are uniformly loaded on the composite carrier in the form of nanoparticles under the irradiation of ultraviolet light to form a hybrid composite nanostructured catalyst with low loading of the active component Pt and small dosage, and Sn is in the form of SnO x The existence of the catalyst in this state makes the catalyst have excellent propane dehydrogenation activity and stability.
[0043] 2. The catalyst PtSn / @-MeOx / SBA-15 provided by the present invention has a simple preparation process, mild preparation conditions, high efficiency and environmental protection, and has good industrial application prospects.
[0044] 3. The catalyst PtSn / @-MeOx / SBA-15 provided by the present invention has high stability. Specifically, on the one hand, it can be recycled for 4 times and still maintain good activity without obvious deactivation; on the other hand, when the reaction time is 1200 min, the propane conversion rate is still high and the propylene selectivity is high. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 The catalyst prepared in Example 1 is PtSn / @-10%CeO 2 / XPS chart of SBA-15;
[0046] Figure 2 The catalyst prepared in Example 5 is PtSn / @-10%La 2 O 3 / XPS chart of SBA-15;
[0047] Figure 3 Catalysts prepared in Example 1 and Example 5 PtSn / @-10% MeO x / TEM image of SBA-15;
[0048] Figure 4 Catalysts prepared in Example 1 and Example 5 PtSn / @-10% MeO x / SBA-15 and carrier CeO 2 / SBA-15, La 2 O 3 / XRD patterns of SBA-15 and SBA-15;
[0049] Figure 5 The propane conversion rate and propane selectivity of the catalysts prepared in Examples 1 to 4 and Comparative Example 1 in the catalytic direct dehydrogenation of propane to propylene reaction versus time are plotted;
[0050] Figure 6 The propane conversion rate and propane selectivity of the catalysts prepared in Examples 5 to 8 and Comparative Example 2 in the catalytic direct dehydrogenation of propane to propylene reaction versus time are plotted;
[0051] Figure 7 The propylene yield and propane selectivity versus time curve of the catalysts prepared in Example 1, Examples 9-10 and Comparative Examples 3 to 4 in the catalytic direct dehydrogenation of propane to propylene reaction;
[0052] Figure 8 The propylene yield and propane selectivity versus time curve of the catalysts prepared in Example 5, Examples 11-12, and Comparative Examples 3 and 5 in the catalytic direct dehydrogenation of propane to propylene reaction;
[0053] Fig. 9 This is a graph showing the cycle performance of the catalyst prepared in Example 1 for direct dehydrogenation of propane;
[0054] Fig.10 This is a graph showing the cycle performance of the catalyst prepared in Example 5 for direct dehydrogenation of propane;
[0055] Fig.11 This is a graph showing the stability performance of the catalyst prepared in Example 1 for direct dehydrogenation of propane;
[0056] Fig.12 This is a graph showing the stability performance of the catalyst prepared in Example 5 for the direct dehydrogenation reaction of propane. DETAILED DESCRIPTION
[0057] The present invention is described in detail below with reference to the accompanying drawings and embodiments, but the present invention can be implemented in many different ways as limited and covered by the claims.
[0058] Example 1
[0059] 1. CeO2 Preparation of SBA-15 composite carrier:
[0060] Step 1.1, weigh a certain amount of ammonia solution, and prepare it into a 50g / ml ammonia solution as a precipitant;
[0061] Step 1.2, add 150ml of deionized water into a three-necked flask, weigh 0.2803g Ce(NO 3 ) 3 6H 2 O is dissolved in deionized water and stirred to obtain a cerium nitrate solution;
[0062] Step 1.3, weigh 1g SBA-15 carrier (CeO 2 Theoretical calculated mass content is 10%) dispersed in cerium nitrate solution, stirred evenly, slowly added the precipitant solution prepared in step 1.1, adjusted the pH to 9-10, and continued stirring for more than 15 minutes after the pH adjustment was completed;
[0063] Step 1.4, the stirred solution was transferred to a microwave reaction device, the power of the microwave reaction device was adjusted to 400 W, and the microwave heating reaction was performed for 16 min. The reaction solution was taken out and cooled to room temperature, and then solid-liquid separation was performed. The solid was washed with anhydrous ethanol and deionized water until the pH was neutral, and then placed in an 80°C drying oven for 12 h to obtain a composite carrier, which was recorded as 10% CeO 2 / SBA-15;
[0064] 2. Catalyst PtSn / @-CeO 2 Preparation of SBA-15:
[0065] Step 2.1: Prepare the composite support 10% CeO 2 / SBA-15 (0.366 g) was dissolved in 10 ml of anhydrous methanol, and about 90 ml of deionized water was added, stirred evenly at room temperature, and ultrasonically vibrated for 10 min to obtain a mixed solution;
[0066] Step 2.2: After the ultrasound is completed, use a pipette to take 0.5 ml of chloroplatinic acid solution (containing 0.0074 g / ml platinum) (molecular formula H 2 PtCl 6 ), and 3 ml of tin chloride solution (0.0014 g / ml) were dropped into the mixed solution, the mixed solution was fixed to 100 ml, and ultrasonic shaking was continued for 20 min;
[0067] Step 2.3: The mixed solution after ultrasonic oscillation was irradiated with ultraviolet light for 12 hours under magnetic stirring. After 12 hours, the mixed solution was taken out and filtered, washed until the filtrate was neutral, and placed in a vacuum drying oven and dried at 80°C for 12 hours to obtain the catalyst PtSn / @-10%CeO 2 / SBA-15, i.e. catalyst PtSn / @-10%CeO 2 The molar ratio of Pt to Sn in / SBA-15 is 1:1, and the mass content of Pt is 1%.
[0068] Embodiment 2:
[0069] Same as Example 1, except that the volume of the tin chloride solution added in step 2.2 is 1 ml, and the molar ratio of platinum to tin is 3:1, denoted as Pt 3 Sn / @-10%CeO 2 / SBA-15.
[0070] Embodiment 3:
[0071] Same as Example 1, except that the volume of the tin chloride solution added in step 2.2 is 1.5 ml, and the molar ratio of platinum to tin is 2:1, denoted as Pt 2 Sn / @-10%CeO 2 / SBA-15.
[0072] Embodiment 4:
[0073] Same as Example 1, except that the volume of the tin chloride solution added in step 2.2 is 6 ml, and the molar ratio of platinum to tin is 1:2, denoted as PtSn 2 / @-10%CeO 2 / SBA-15.
[0074] Comparative Example 1:
[0075] Same as Example 1, except that no tin chloride solution is added in step 2.2, denoted as Pt / @-10%CeO 2 / SBA-15.
[0076] Example 5
[0077] 1. La 2 O 3 Preparation of SBA-15 composite carrier:
[0078] Step 1.1, weigh a certain amount of ammonia solution, and prepare it into a 50g / ml ammonia solution as a precipitant;
[0079] Step 1.2, add 150ml of deionized water to a three-necked flask, weigh 0.2953g La(NO 3 ) 3 6H2 O is dissolved in deionized water and stirred to obtain a lanthanum nitrate solution;
[0080] Step 1.3, weigh 1g SBA-15 carrier (CeO 2 Theoretical calculated mass content is 10%) dispersed in lanthanum nitrate solution, stirred evenly, slowly added the precipitant solution prepared in step 1.1, adjusted the pH to 9-10, and continued stirring for more than 15 minutes after the pH adjustment was completed;
[0081] Step 1.4, the stirred solution was transferred to a microwave reaction device, the power of the microwave reaction device was adjusted to 400W, and the microwave heating reaction was performed for 16 minutes. The reaction solution was taken out and cooled to room temperature, and then solid-liquid separation was performed. The solid was washed with anhydrous ethanol and deionized water until the pH was neutral, and then placed in an 80°C drying oven for 12 hours to obtain a composite carrier, which was recorded as 10% La 2 O 3 / SBA-15;
[0082] 2. Catalyst PtSn / @-La 2 O 3 Preparation of SBA-15:
[0083] Step 2.1: The composite carrier 10% La prepared in step 1.4 2 O 3 / SBA-15 (0.366 g) was dissolved in 10 ml of anhydrous methanol, and about 90 ml of deionized water was added, stirred evenly at room temperature, and ultrasonically vibrated for 10 min to obtain a mixed solution;
[0084] Step 2.2: After the ultrasound is completed, use a pipette to take 0.5 ml of chloroplatinic acid solution (containing 0.0074 g / ml platinum) (molecular formula H 2 PtCl 6 ), and 3 ml of tin chloride solution (0.0014 g / ml) were dropped into the mixed solution, the mixed solution was fixed to 100 ml, and ultrasonic shaking was continued for 20 min;
[0085] Step 2.3, the mixed solution after ultrasonic oscillation was irradiated with ultraviolet light for 12 hours under magnetic stirring, and then taken out and filtered after 12 hours, washed until the filtrate was neutral, and placed in a vacuum drying oven and dried at 80°C for 12 hours to obtain the catalyst PtSn / @-10%La 2 O 3 / SBA-15, i.e. catalyst PtSn / @-10%La 2 O 3 The molar ratio of Pt to Sn in / SBA-15 is 1:1, and the mass content of Pt is 1%.
[0086] Embodiment 6:
[0087] Same as Example 5, except that the volume of the tin chloride solution added in step 2.2 is 1 ml, and the molar ratio of platinum to tin is 3:1, denoted as Pt 3 Sn / @-10%La 2 O 3 / SBA-15.
[0088] Embodiment 7:
[0089] Same as Example 5, except that the volume of the tin chloride solution added in step 2.2 is 1.5 ml, and the molar ratio of platinum to tin is 2:1, denoted as Pt 2 Sn / @-10%La 2 O 3 / SBA-15.
[0090] Embodiment 8:
[0091] Same as Example 5, except that the volume of the tin chloride solution added in step 2.2 is 6 ml, and the molar ratio of platinum to tin is 1:2, denoted as PtSn 2 / @-10%La 2 O 3 / SBA-15.
[0092] Comparative Example 2:
[0093] Same as Example 5, except that no tin chloride solution is added in step 2.2, recorded as Pt / @-10%La 2 O 3 / SBA-15.
[0094] It should be noted that in the above embodiment, CeO 2 and La 2 O 3 The mass fraction of 10% refers to its content in the composite carrier MeO x / Mass fraction in SBA-15.
[0095] Catalyst activity evaluation
[0096] In this example, the effect of different molar ratios of platinum and tin in the catalyst on the performance of direct dehydrogenation of propane was investigated. All the direct dehydrogenation reactions of propane in the reaction examples were carried out in a micro fixed bed reactor at normal pressure, with pure propane as the reaction gas, and analyzed using an Agilent 6820 gas chromatograph.
[0097] 100 mg of the catalyst was used to test the direct dehydrogenation of propane in a micro fixed bed reactor. The propane reaction gas flow rate was 12 ml / min, i.e., the weight hourly space velocity was 14 h -1Before the reaction performance test, the sample was pretreated by passing a mixed gas of hydrogen and argon. The pretreated catalyst was switched to propane raw gas for reaction under the protection of argon. The pretreatment conditions were as follows: the pretreatment temperature was 550°C (programmed temperature control was used in the reaction), the pretreatment time was 1h, and the volume ratio of hydrogen and argon in the pretreatment gas was 1:4, that is, 20% H 2 / 80%Ar.
[0098] The catalyst activity is expressed by propane conversion and propylene selectivity or propylene yield and propylene selectivity:
[0099] in:
[0100]
[0101]
[0102]
[0103] Refers to propane conversion rate;
[0104] S j (%): refers to the selectivity of the generated product;
[0105] Y j (%): refers to propylene yield;
[0106] z j and n j are the number of carbon atoms and the number of moles of gaseous carbon-containing product j, respectively. propane is the number of moles of unconverted propane in the product stream.
[0107] z j and n j : are the number of carbon atoms and the number of moles of gaseous carbon-containing product j, respectively.
[0108] The initial activity data of the catalysts prepared in Examples 1 to 8 and Comparative Examples 1 and 2 in the direct dehydrogenation reaction of propane are summarized to obtain Table 1.
[0109] Table 1 Activity data corresponding to the catalysts prepared in Examples 1 to 8 and Comparative Examples 1 and 2
[0110] catalyst Propane conversion rate (%) Propylene selectivity (%) Comparative Example 1 <![CDATA[1%Pt / @-10%CeO 2 / SBA-15]]> 14.51 85.10 Example 1 <![CDATA[PtSn / @-10%CeO 2 / SBA-15]]> 27.09 97.16 Example 2 <![CDATA[Pt 3 Sn / @-10%CeO 2 / SBA-15]]> 25.91 94.60 Example 3 <![CDATA[Pt 2 Sn / @-10%CeO 2 / SBA-15]]> 25.47 96.27 Example 4 <![CDATA[PtSn 2 / @-10%CeO 2 / SBA-15]]> 22.44 97.23 Comparative Example 2 <![CDATA[1%Pt / @-10%La 2 SHE 3 / SBA-15]]> 17.33 82.38 Example 5 <![CDATA[PtSn / @-10%La 2 SHE 3 / SBA-15]]> 26.95 93.57 Example 6 <![CDATA[Pt 3 Sn / @-10%La 2 SHE 3 / SBA-15]]> 26.32 90.82 Example 7 <![CDATA[Pt 2 Sn / @-10%La 2 SHE 3 / SBA-15]]> 25.74 91.47 Example 8 <![CDATA[PtSn 2 / @-10%La 2 SHE 3 / SBA-15]]> 22.43 96.47
[0111] By comparing the experimental results of Comparative Example 1 with those of Examples 1 to 4, and by comparing the experimental results of Comparative Example 2 with those of Examples 5 to 8, it can be seen that the addition of Sn effectively improves the catalyst activity, and when the platinum-tin ratio is 1:1, the highest propane conversion rate is achieved.
[0112] Figure 1 The catalyst prepared in Example 1 is PtSn / @-10%CeO 2 / XPS graph of SBA-15, Figure 2 The catalyst prepared in Example 5 is PtSn / @-10%La 2 O 3 / XPS graph of SBA-15, from Figure 1 and Figure 2 It can be seen that the proportion of electron-deficient Pt is very high, indicating that x There is a strong interfacial electronic effect between them; and Sn only exists in one valence state of +4, indicating that Sn plays a good promoting role in the catalyst and exists stably.
[0113] Figure 3 The catalyst prepared in Example 1 is PtSn / @-10%CeO 2 / SBA-15 and catalyst PtSn / @-10%La prepared in Example 5 2 O 3 / TEM image of SBA-15, from Figure 3 It can be seen that the pore structure of SBA-15 has not changed, and Pt and Sn are evenly dispersed on the catalyst.
[0114] Figure 4 The catalyst prepared in Example 1 and Example 5 and MeO x XRD patterns of SBA-15 composite support and SBA-15 molecular sieve. Figure 4 It can be seen that the spectrum has not changed significantly and MeO x The diffraction peaks of Pt and Sn indicate that the pore structure of SBA-15 has not changed and MeO x Does not exist in crystalline form.
[0115] The relationship between the propane conversion rate and propane selectivity calculated in the direct dehydrogenation reaction of propane by the catalysts prepared in Examples 1 to 4 and the catalyst prepared in Comparative Example 1 and time is plotted into a curve graph, as shown in FIG. Figure 5 As shown; the relationship between the propane conversion rate and propane selectivity calculated in the direct dehydrogenation reaction of propane by the catalysts prepared in Examples 5 to 8 and the catalyst prepared in Comparative Example 2 and time is plotted into a curve graph, as shown Figure 6 shown; from Figure 5 and Figure 6 It can be seen that the propane conversion rate and propylene selectivity corresponding to each catalyst change little with the increase of time; at the same time, when the molar ratio of Pt to Sn is 1:, the corresponding propane conversion rate and propylene selectivity data are the best.
[0116] Example 9
[0117] Same as Example 1, except that the catalyst is PtSn / @-CeO 2 / CeO in SBA-15 2 The mass fraction of PtSn is 5%, recorded as PtSn / @-5%CeO 2 / SBA-15.
[0118] Example 10
[0119] Same as Example 1, except that the catalyst is PtSn / @-CeO 2 / CeO in SBA-15 2 The mass fraction of PtSn is 15%, recorded as PtSn / @-15%CeO 2 / SBA-15.
[0120] Comparative Example 3
[0121] Same as Example 1, except that the catalyst is PtSn / @-CeO 2 / CeO in SBA-15 2 The mass fraction of is 0, recorded as PtSn / / SBA-15.
[0122] Comparative Example 4
[0123] Same as Example 1, except that the catalyst is PtSn / @-CeO 2 The mass fraction of SBA-15 in PtSn / CeO is 0, which is recorded as PtSn / CeO 2 .
[0124] Embodiment 11
[0125] Same as Example 5, except that the catalyst is PtSn / @-La 2 O 3 / SBA-15 Medium La 2 O 3 The mass fraction of La is 5%, recorded as PtSn / @-5%La 2 O 3 / SBA-15.
[0126] Example 12
[0127] Same as Example 5, except that the catalyst is PtSn / @-La 2 O 3 / SBA-15 Medium La 2 O 3 The mass fraction of La is 15%, recorded as PtSn / @-15%La 2 O 3 / SBA-15.
[0128] Comparative Example 5
[0129] Same as Example 5, except that the catalyst is PtSn / @-La 2 O 3 The mass fraction of SBA-15 in PtSn / @-La is 0, which is recorded as 2 O 3 ; At the same time, the precipitant used in step 1.1 is 0.4 mol / L ammonium bicarbonate solution.
[0130] The same catalyst activity evaluation method as above was used to evaluate the activities of the catalysts prepared in Examples 9 to 12 and Comparative Examples 3 to 5. The activity evaluation results are shown in Table 2.
[0131] Table 2 Propylene yield and propylene selectivity corresponding to the catalysts prepared in each example
[0132] catalyst Propylene yield (%) Propylene selectivity (%) Comparative Example 3 PtSn / SBA-15 7.74 92.37 Comparative Example 4 <![CDATA[PtSn / CeO 2 ]]> 7.73 76.80 Example 1 <![CDATA[PtSn / @-10%CeO 2 / SBA-15]]> 25.84 96.90 Example 9 <![CDATA[PtSn / @-5%CeO 2 / SBA-15]]> 24.37 95.85 Example 10 <![CDATA[PtSn / @-15%CeO 2 / SBA-15]]> 24.57 97.33 Comparative Example 5 <![CDATA[PtSn / @-La 2 THE 3 ]]> 10.07 87.16 Example 5 <![CDATA[PtSn / @-10%La 2 SHE 3 / SBA-15]]> 25.73 94.55 Embodiment 11 <![CDATA[PtSn / @-5%La 2 SHE 3 / SBA-15]]> 25.28 96.85 Example 12 <![CDATA[PtSn / @-15%La 2 SHE 3 / SBA-15]]> 25.31 90.56
[0133] By comparing the experimental results of Example 1, Examples 9-10 with Comparative Examples 3 and 4, and comparing the experimental results of Example 5, Examples 11-12 with Comparative Example 5, it can be seen that the synergistic effect between the metal and the metal semiconductor effectively improves the catalyst activity, and when the oxide loading is 10%, the highest propylene yield is achieved.
[0134] The relationship between the propylene yield and propylene selectivity calculated in the direct dehydrogenation reaction of propane using the catalysts prepared in Example 1, Examples 9-10 and Comparative Examples 3 and 4 and time is plotted as a curve, as shown in FIG. Figure 7 The relationship between the propylene yield and propylene selectivity and time calculated in the direct dehydrogenation reaction of propane by the catalysts prepared in Example 5, Example 11-12 and Comparative Examples 3 and 5 is plotted as a curve, as shown in FIG. Figure 8 shown; from Figure 7 and Figure 8 It can be seen that the propylene yield and propylene selectivity corresponding to each catalyst change little with the increase of time; at the same time, when the oxide loading is 10%, the corresponding propylene yield and propylene selectivity data are the best.
[0135] Embodiment 13
[0136] The catalyst prepared in Example 1 was subjected to a cyclic stability test.
[0137] According to the catalyst activity evaluation method provided above, the catalyst PtSn / @-10%CeO prepared in Example 1 was used. 2 / SBA-15 was used for multiple cycles, each time for 7 hours. After the experiment, the catalyst was collected and calcined in a muffle furnace at 500℃ for 2 hours to eliminate carbon deposits. The results of multiple cycles are detailed in Fig. 9 ,from Fig. 9 It can be seen that the catalyst PtSn / @-10%CeO 2 / SBA-15 has good regenerative performance for direct dehydrogenation of propane and can be reused.
[0138] Embodiment 14
[0139] The catalyst prepared in Example 5 was subjected to a cyclic stability test.
[0140] According to the catalyst reaction activity method provided above, the catalyst PtSn / @-10%La prepared in Example 5 was used. 2 O 3 / SBA-15 was used for multiple cycles, each time for 7 hours. After the experiment, the catalyst was collected and calcined in a muffle furnace at 500℃ for 2 hours to eliminate carbon deposits. The results of multiple cycles are detailed in Fig.10 ,from Fig.10 It can be seen that the catalyst PtSn / @-10%La 2 O 3 / SBA-15 has good regenerative performance for direct dehydrogenation of propane and can be reused.
[0141] Embodiment 15
[0142] The stability of the catalyst prepared in Example 1 was tested
[0143] According to the catalyst activity evaluation method provided above, the catalyst PtSn / @-10%CeO prepared in Example 1 was used. 2 / SBA-15 was used for catalytic reaction, and the reaction time was 1200 minutes. Fig.11 It can be seen that the catalyst PtSn / @-10%CeO 2 / SBA-15 has good stability performance and still maintains good catalytic activity after the catalytic reaction time reaches 1200 minutes.
[0144] Example 16
[0145] The stability of the catalyst prepared in Example 5 was tested
[0146] According to the catalyst activity evaluation method provided above, the catalyst prepared in Example 1 was used. 2 O 3 / SBA-15 was used for catalytic reaction, and the reaction time was 1200 minutes. Fig.12 It can be seen that the catalyst PtSn / @-10%La 2 O 3 / SBA-15 has good stability performance and still maintains good catalytic activity after the catalytic reaction time reaches 1200 minutes.
[0147] The conversion rate of propane, selectivity of propylene and deactivation coefficient of the catalyst prepared in Example 1 and the catalyst prepared in Example 5 and the catalyst reported in the published literature in the direct dehydrogenation reaction of propane are summarized, and the summary results are shown in Table 3;
[0148] Table 3 Comparison of activity data of several reported optimal catalysts in direct dehydrogenation of propane
[0149]
[0150]
[0151] a The above data comes from, Stable and selective catalysts for propanedehydrogenation operating at thermodynamic limit, Science, 373, 217–222 (2021)
[0152] The calculation formula for the inactivation coefficient in Table 3 is:
[0153]
[0154] Among them, con Final Refers to the final conversion rate;
[0155] Con Initial Refers to the initial conversion rate.
[0156] As can be seen from Table 3, the PtSn hybrid nanostructured catalyst PtSn / @-CeO 2 / SBA-15 has a very high catalytic activity for propane dehydrogenation to propylene; when pure propane is fed, the reaction temperature is 550℃ and the high space velocity (WHSV = 14h -1 ) can reach equilibrium conversion rate of 86%, propylene selectivity> 97%, and deactivation coefficient is small (k d Only 0.011h -1 ; 1 / k d (h) = 90.91) (~ reached the limit); and has good stability and reproducibility.
[0157] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions and substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention.
Claims
1. A platinum-tin hybrid nanostructured catalyst for direct dehydrogenation of propane to propylene, It is characterized in that The invention comprises a composite carrier and an active component and an auxiliary agent loaded on the composite carrier, wherein the active component is Pt, the auxiliary agent is Sn, and Sn is in the form of SnO x The composite carrier is MeO x / SBA-15, denoted as PtSn / @-MeO x / SBA-15, MeO x CeO 2 or La 2 O 3 ; Wherein, the composite carrier MeO x / MeO in SBA-15 x MeO was formed by microwave heating reaction in the form of single layer or multilayer on SBA-15 molecular sieve x Semiconductor film layer, the catalyst PtSn / @-MeO x The active component Pt and the auxiliary agent Sn in SBA-15 are anchored on the composite support MeO in the form of nanoparticles through photocatalytic reduction. x / SBA-15, the active component Pt and the MeO x There is a synergistic effect among the semiconductor film layers.
2. The platinum-tin hybrid nanostructured catalyst for direct dehydrogenation of propane to propylene according to claim 1, It is characterized in that The catalyst PtSn / @-MeO x The mass content of Pt in the SBA-15 is 0.1-3%, and the molar ratio of the active component Pt to the auxiliary agent Sn is 1:(1 / 3-2); the composite carrier MeO x / MeO in SBA-15 x The mass content is 5-20%.
3. A method for preparing a platinum-tin hybrid nanostructured catalyst for direct dehydrogenation of propane to propylene, It is characterized in that The steps include: (1) SBA-15 molecular sieve is uniformly dispersed in a cerium salt solution or a lanthanum salt solution, and then a precipitant is added to adjust the pH value to 7-10, and then stirring is continued for a first preset time. The resulting solution is placed in a microwave reaction device and heated under preset heating conditions for reaction, and then solid-liquid separation and drying are performed to obtain a composite carrier MeO x / SBA-15, of which MeO x CeO 2 or La 2 O 3 ; (2) The active component Pt and the auxiliary agent Sn are anchored on the composite carrier MeO in the form of nanoparticles by photocatalytic reduction. x / SBA-15, and the catalyst PtSn / @-MeO was obtained x / SBA-15, in which Pt is the active component, Sn is the auxiliary agent and Sn is in the form of SnO x The state exists.
4. The method for preparing the platinum-tin hybrid nanostructured catalyst for direct dehydrogenation of propane to propylene according to claim 3, It is characterized in that The composite carrier MeO in step (1) x / MeO in SBA-15 x The mass content is 5 to 20%; the mass content of Pt in the catalyst PtSn / @-MeOx / SBA-15 in step (2) is 0.1 to 3%, and the molar ratio of the active component Pt to the auxiliary agent Sn is 1: (1 / 3 to 2).
5. The method for preparing the platinum-tin hybrid nanostructured catalyst for direct dehydrogenation of propane to propylene according to claim 3, It is characterized in that The preset heating conditions include: heating reaction time of 10 to 20 minutes and microwave power of 200 to 600W.
6. The method for preparing the platinum-tin hybrid nanostructured catalyst for direct dehydrogenation of propane to propylene according to claim 3, It is characterized in that The photocatalytic reduction method is specifically as follows: adding the composite carrier MeOx / SBA-15 prepared in step (1) to water and anhydrous methanol, and uniformly dispersing by ultrasonication; then adding chloroplatinic acid solution and tin chloride solution, and continuing ultrasonic oscillation for a second preset time; then placing under an ultraviolet lamp, stirring under light conditions, filtering the stirred solution, and vacuum drying to obtain the catalyst PtSn / @-MeOx / SBA-15.
7. A platinum-tin hybrid nanostructure catalyst, It is characterized in that The catalyst is prepared by the preparation method according to any one of claims 3 to 6.
8. A method for preparing propylene by direct dehydrogenation of propane, It is characterized in that The method comprises using a pretreated catalyst PtSn / @-MeO x / SBA-15 catalyzes direct dehydrogenation of propane gas to produce propylene, the reaction pressure is normal pressure, and the reaction temperature is 500-580°C; the catalyst PtSn / @-MeO x / SBA-15 comprises a composite carrier and an active component and an auxiliary agent loaded on the composite carrier, wherein the active component is Pt, the auxiliary agent is Sn, and Sn is in the form of SnO x The composite carrier is MeO x / SBA-15, the catalyst PtSn / @-MeO x / SBA-15 is prepared by the following method, comprising: The SBA-15 molecular sieve is uniformly dispersed in a cerium salt solution or a lanthanum salt solution, and then a precipitant is added to adjust the pH value to 7-10, and then the stirring is continued for a first preset time. The obtained solution is placed in a microwave reaction device and heated to react under preset heating conditions, and then solid-liquid separation and drying are performed to obtain a composite carrier MeOx / SBA-15, wherein MeO x CeO 2 or La 2 O 3 ; The active component Pt and the auxiliary agent Sn are anchored on the composite carrier MeOx / SBA-15 in the form of nanoparticles by photocatalytic reduction to obtain the catalyst PtSn / @-MeO x / SBA-15.
9. The method for preparing propylene by direct dehydrogenation of propane according to claim 8, It is characterized in that The propane content of the propane gas is 20-100 vol%, and the weight hourly space velocity of the propane gas is 5-18 h -1 .
10. The method for preparing propylene by direct dehydrogenation of propane according to claim 9, It is characterized in that The pretreatment method of the catalyst PtSn / @-MeOx / SBA-15 is as follows: the catalyst PtSn / @-MeOx / SBA-15 is filled into a micro fixed bed reactor, and an inert gas with a content of 10 to 40 vol% is introduced for pretreatment for 30 to 120 minutes, wherein the pretreatment temperature is 500 to 580°C.