A high-efficiency composite eluent for ion-exchange ammonium in weathering crust leaching type rare earth tailings and its preparation method
By using a mixed aqueous solution adjusted by complex metal salts and acids as the eluent, the problem of low elution efficiency and environmental pollution of ion-exchanged ammonium in rare earth tailings is solved, achieving an efficient, economical, and environmentally friendly elution effect, and preventing Geological disasters and environmental damage.
Patent Information
- Application Number
- CN202310084660.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-01-16
AI Technical Summary
When existing technologies deal with ion-exchanged ammonium remaining in rare earth tailings, the elution efficiency is low, the cost is high, and may lead to geological disasters and environmental pollution, making it difficult to develop efficient and environmentally friendly eluents.
A mixed aqueous solution formed of a complex metal salt and acid is used as an efficient eluent, including hydrochloric acid, oxalic acid, citric acid, etc. of metal elements such as K, Na, Li, Ca, Mg, Fe, and Al, and the pH value is adjusted to 3~ 6. Used for the elution of weathered crust leaching type rare earth tailings.
It achieves high removal rate and fast elution rate of ion-exchanged ammonium, reduces production costs, inhibits the expansion of clay minerals, prevents landslides, reduces back adsorption of ammonia nitrogen, and has good environmental protection effects.
Smart Images

Figure HDA0004068574140000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional materials, and in particular relates to a high-efficiency composite eluent for ionic ammonium in weathering crust leaching type rare earth tailings and a preparation method thereof. Background Art
[0002] Weathering crust leaching type rare earth ore (ion adsorption type rare earth ore) is rich in medium and heavy rare earths. The rare earths in this type of ore are mainly enriched in clay minerals such as kaolin in the form of hydrated or hydroxyl hydrated cations, and are usually mined by in situ leaching technology.
[0003] In the in-situ leaching process, ammonium salts are mainly used as leaching agents to leach rare earths. Ammonium salts enter the ore body through the injection hole, and undergo ion exchange reactions with rare earth ions adsorbed on the surface of clay minerals, thereby leaching rare earth ions. Among them, the in-situ leaching process using ammonium salts as leaching agents has the advantages of high leaching rate and no damage to the original topography and landforms of the mining area, and is widely used in the mining of weathering crust leaching type rare earth ores. However, the use of a large amount of leaching agents during the leaching process causes ammonium salts to remain in the tailings, and their slow release has a serious impact on the ecology of the mining area. According to statistics, 7-12 tons of ammonium sulfate are required to produce 1 ton of rare earth oxides. Therefore, the treatment of residual ammonium salts has become the key to green mining of rare earth mines. The existence of residual ammonium in rare earth ores can be divided into three forms: water-soluble ammonium, fixed ammonium and ion-exchange ammonium. Water-soluble ammonium in rare earth tailings is mainly adsorbed on clay minerals by weak forces such as hydrogen bonds and van der Waals forces; fixed ammonium is mainly adsorbed on the surface of clay minerals in a fixed state and then fixed between layers. Ion-exchange ammonium accounts for more than 80% of rare earth tailings, and is mainly adsorbed on the surface of clay minerals in an ion-exchange state. Ion-exchange ammonium adsorbed between clay mineral layers needs to be exchanged and eluted with metal ions of similar radius. Ion-exchange ammonium is the main cause of ammonia nitrogen pollution due to its high content.
[0004] In the actual process of treating ammonia nitrogen, the clay minerals in the rare earth tailings will undergo physical and chemical effects such as expansion and dispersion after adding low-permeability eluents, leading to geological disasters such as landslides; and the addition of eluents that are not suitable for plant growth will secondary damage the mining environment. Therefore, the development of efficient and environmentally friendly eluents will be of great significance to the ecological environment construction of rare earth mines. At present, the existing eluent work mainly focuses on total nitrogen elution, most of which use a single salt, with a large amount of eluent, low elution efficiency, high eluent cost, and complex elution process; and because the changes in clay minerals in rare earth tailings affect the content of ion-exchange ammonium, the composition and content of clay minerals in rare earth tailings of different depths and different particle sizes are very different. Therefore, from the perspective of reducing production costs and improving elution efficiency, it is very necessary to study the compounding ratio of compound eluents. Summary of the invention
[0005] The main purpose of the present invention is to provide a high-efficiency eluent for removing ion-exchange ammonium from weathering crust leaching type rare earth ore in view of the problems and shortcomings of the prior art. The eluent has a high removal rate for residual ion-exchange ammonium and a fast elution rate; it is low in cost, economical and environmentally friendly, and has broad application prospects; and the preparation method involved is simple, easy to operate, and suitable for popularization and application.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A highly efficient composite eluent for ion-exchange ammonium in weathering crust leaching type rare earth tailings, which is a mixed aqueous solution formed by a composite metal salt and an acid; wherein the metal elements corresponding to the composite metal salt are two or more of K, Na, Li, Ca, Mg, Fe, and Al; and the acid is one or more of hydrochloric acid, oxalic acid, citric acid, malic acid, etc.
[0008] In the above scheme, the pH value of the high-efficiency composite eluent is 3-6.
[0009] Furthermore, the metal elements corresponding to the composite metal salt are two of K, Na, Li, Ca, Mg, Fe, and Al, and their molar ratio is 1:4 to 4:1.
[0010] In the above scheme, the composite metal salt is one or more of soluble hydrochloride, nitrate, sulfate, phosphate, formates, acetates and the like.
[0011] In the above scheme, the concentration (total concentration) of the composite metal salt is 0.02 to 0.2 mol / L.
[0012] The above-mentioned method for preparing a highly efficient composite eluent for residual ammonium salt in weathering crust leaching type rare earth tailings comprises the following steps:
[0013] 1) preparing aqueous solutions of metal salts of different concentrations respectively;
[0014] 2) The obtained aqueous solutions of metal salts with different concentrations are mixed uniformly according to proportion to obtain a composite metal salt solution, and then an acid is added to adjust the pH value of the obtained mixed solution to obtain the composite salt high-efficiency eluent.
[0015] Preferably, the composite metal salt is potassium salt and magnesium salt.
[0016] Furthermore, the composite metal salt consists of potassium chloride and magnesium chloride.
[0017] Preferably, the molar ratio of potassium chloride to magnesium chloride is 7:(3-4).
[0018] Preferably, the pH value is 4-5.
[0019] The high-efficiency composite eluent described in the above scheme is applied to elute the residual ammonium salt in the ion exchange state in the weathering crust leaching type rare earth tailings. The removal rate of the residual ion exchange ammonium is high, the elution rate is fast, and a good swelling inhibition effect is shown.
[0020] The principle of the present invention is:
[0021] The residual ammonium salt exists in the ore body mainly in the form of water-soluble and exchangeable states. Aiming at the fact that the elution efficiency is affected by many factors (such as ion characteristics, permeability, diffusivity and exchange capacity of metal ions, etc.), the present invention utilizes the effect of the composite eluent on ion-exchange ammonium, and further uses a small amount of acid to adjust the pH value, which can effectively overcome the problems of low elution efficiency, low elution rate and complex composition of traditional eluents. The eluent of the present invention can realize the efficient elution of residual ammonium salt under simple formula conditions, and will not cause secondary pollution to the environment, so it is suitable for popularization and application.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1) The composite salt high-efficiency eluent of the present invention has low cost, high elution efficiency and simple elution process;
[0024] 2) It has good swelling suppression effect and will not cause the expansion of clay minerals in rare earth tailings, effectively preventing landslides and other problems;
[0025] 3) High permeability, which can effectively overcome the viscous resistance between ore bodies, increase diffusion and improve elution rate;
[0026] 4) It has various functions and can prevent the reverse adsorption of ammonia nitrogen under the action of concentration difference, and the amount of eluent used is small, which reduces the cost of eluent;
[0027] 5) The composite salt efficient eluent of the present invention is beneficial to the reclamation of tailings plants and has a good environmental protection effect;
[0028] 6) The composite eluent of the present invention can achieve efficient removal of residual ammonium salts in the ore body, significantly reduce the serious impact on the environment caused by the slow release of residual ammonium salts, and provide new ideas for the construction of green rare earth mines. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The swelling inhibition performance test results of the high-efficiency composite eluent obtained in Example 1 are shown in FIG. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0031] In the following embodiments, the rare earth tailings samples used were collected from the mountainside, top and bottom of the mountain where the rare earth ore was leached in situ, at a depth of 300-400 cm. In order to reduce the influence of some humus layers and impurities on the experimental treatment, the collected rare earth tailings were firstly cleaned, freeze-dried and sieved to obtain the required samples. Ionic ammonium accounts for the largest proportion in the form of ammonia. Through the continuous graded elution method, the water-soluble ammonium bound by hydrogen bonds and van der Waals forces is washed away with secondary water. Ionic ammonium mainly binds to a large number of hydroxyl active sites on the surface of clay minerals; it can be eluted by metal salt solution in the form of ion exchange, so the invention is mainly aimed at the elution of ion exchange ammonium.
[0032] Example 1
[0033] A high-efficiency composite eluent for ion-exchange ammonium in weathering crust leaching type rare earth tailings, the preparation method of which comprises the following steps:
[0034] 700 mL of 0.1 mol / L potassium chloride solution and 300 mL of 0.1 mol / L magnesium chloride solution were mixed evenly, and a few drops (about 5 mL) of 0.01 mol / L malic acid solution were added to the obtained composite metal salt solution, and the pH of the composite metal salt solution was adjusted to 5 to obtain the high-efficiency composite eluent.
[0035] Under simulated experimental conditions, the obtained high-efficiency composite eluent is used to elute ion-exchange ammonium in weathering crust leaching type rare earth tailings. The specific steps include:
[0036] Weigh 1 g of rare earth tailings with a particle size of 150-200 mesh obtained by continuous graded elution method, add the obtained high-efficiency composite eluent at a solid-liquid ratio of 1:30 (g:mL), shake in a shaker at a temperature of 25°C for 3 hours, put it into a centrifuge at 4000r / min for 5 minutes to obtain a supernatant, and measure the ammonium content in the supernatant by Nessler's reagent spectrophotometry.
[0037] Rare earth tailings were collected from the top, bottom and col of the rare earth mine and loaded into the dynamic column according to the quartering method. A certain loading height was set and the obtained high-efficiency composite eluent was used to control the flow rate to 3.0 mol / min with a peristaltic pump for dynamic experiments. Samples were collected at different times and the ammonium content in the sample solution was determined by the Nessler reagent method. The time to reach equilibrium was 30 minutes and the efficiency of the mixed salt solution in eluting ammonium in the rare earth tailings was 99%.
[0038] The free expansion rate method was further used to determine the effect of the obtained high-efficiency composite eluent on the swelling ratio of rare earth tailings. The swelling ratio was constructed using experimental data. The results are shown in Figure 1 The results show that the high-efficiency composite eluent obtained in this example has a good swelling inhibition effect on rare earth tailings.
[0039] Example 2
[0040] A highly efficient composite eluent for residual ammonium salt in weathering crust leaching type rare earth tailings, the preparation method of which comprises the following steps:
[0041] 800 mL of 0.1 mol / L potassium chloride solution and 200 mL of 0.1 mol / L calcium chloride solution were mixed evenly, and a few drops (about 5 mL) of 0.01 mol / L citric acid solution were added to the obtained composite metal salt solution, and the pH of the composite metal salt solution was adjusted to 5 to obtain the high-efficiency composite eluent.
[0042] Under simulated experimental conditions, the obtained high-efficiency composite eluent was used to elute residual ammonium salts in weathering crust leaching type rare earth tailings. The specific steps include:
[0043] Weigh 1 g of rare earth tailings with a particle size of 150-200 mesh obtained by continuous graded elution method, add the obtained high-efficiency composite eluent at a solid-liquid ratio of 1:30 (g:mL), shake in a shaker at a temperature of 25°C for 3 hours, put it into a centrifuge at 4000r / min for 5 minutes to obtain a supernatant, and measure the ammonium content in the supernatant by Nessler's reagent spectrophotometry.
[0044] The rare earth tailings were collected from the top, col and bottom of the rare earth mine, and loaded into the dynamic column according to the quartering method. A certain loading height was set, and the obtained high-efficiency composite eluent was used to control the flow rate of 2.5 mol / min with a peristaltic pump for dynamic experiments. The samples were collected at different times, and the ammonium content in the sample solution was determined by the Nessler reagent method. The time to reach equilibrium was 35 minutes, and the efficiency of the mixed salt solution in eluting ammonium in the rare earth tailings was 94%.
[0045] Example 3
[0046] A highly efficient composite eluent for residual ammonium salt in weathering crust leaching type rare earth tailings, the preparation method of which comprises the following steps:
[0047] 200 mL of a 0.1 mol / L magnesium chloride solution and 800 mL of a 0.1 mol / L calcium chloride solution were mixed evenly, and a few drops (about 5 mL) of a 0.01 mol / L oxalic acid solution were added to the resulting composite metal salt solution to adjust the pH value of the composite metal salt solution to 5, thereby obtaining the highly efficient composite eluent.
[0048] Under simulated experimental conditions, the obtained high-efficiency composite eluent was used to elute residual ammonium salts in weathering crust leaching type rare earth tailings. The specific steps include:
[0049] Weigh 1 g of rare earth tailings with a particle size of 150-200 mesh obtained by continuous graded elution method, add the obtained high-efficiency composite eluent at a solid-liquid ratio of 1:30 (g:mL), shake in a shaker at a temperature of 25°C for 3 hours, put it into a centrifuge at 4000r / min for 5 minutes to obtain a supernatant, and measure the ammonium content in the supernatant by Nessler's reagent spectrophotometry.
[0050] Collect rare earth tailings from the top, col and bottom of the rare earth mine, and load them into the dynamic column according to the quartering method. Set a certain sample loading height, and use a peristaltic pump to control the flow rate of the obtained high-efficiency composite eluent to 2.0 mol / min for dynamic experiments. Samples were collected at different times, and the ammonium content in the sample solution was determined by the Nessler reagent method. The time to reach equilibrium was 35 minutes, and the efficiency of the mixed salt solution in eluting ammonium in the rare earth tailings was 94%.
[0051] Example 4
[0052] A highly efficient composite eluent for residual ammonium salt in weathering crust leaching type rare earth tailings, the preparation method of which comprises the following steps:
[0053] 500 mL of 0.1 mol / L potassium chloride solution and 500 mL of 0.1 mol / L ferric chloride solution were mixed evenly, and a few drops (about 5 mL) of 0.01 mol / L hydrochloric acid were added to the obtained composite metal salt solution to adjust the pH value of the composite metal salt solution to 5, thereby obtaining the said high-efficiency composite eluent.
[0054] Under simulated experimental conditions, the obtained high-efficiency composite eluent was used to elute residual ammonium salts in weathering crust leaching type rare earth tailings. The specific steps include:
[0055] Weigh 1 g of rare earth tailings with a particle size of 150-200 mesh obtained by continuous graded elution method, add the obtained high-efficiency composite eluent at a solid-liquid ratio of 1:30 (g:mL), shake in a shaker at a temperature of 25°C for 3 hours, put it into a centrifuge and centrifuge it at 4000r / min for 5 minutes to obtain a supernatant, measure the ammonium content in the supernatant by Nessler's reagent spectrophotometry, and elute the ammonium in the rare earth tailings with a mixed salt solution.
[0056] Collect rare earth tailings from the top, col and bottom of the rare earth mine, and load them into the dynamic column according to the quartering method. Set a certain sample loading height, and use a peristaltic pump to control the flow rate of the obtained high-efficiency composite eluent to 1.5 mol / min for dynamic experiments. Samples are collected at different times, and the ammonium content in the sample solution is determined by the Nessler reagent method. The time to reach equilibrium is 35 minutes, and the efficiency of the mixed salt solution in eluting ammonium in the rare earth tailings is 95%.
[0057] Example 5
[0058] A highly efficient composite eluent for residual ammonium salt in weathering crust leaching type rare earth tailings, the preparation method of which comprises the following steps:
[0059] 500 mL of 0.1 mol / L magnesium chloride solution and 500 mL of 0.1 mol / L ferric chloride solution were mixed evenly, and a few drops (about 5 mL) of 0.01 mol / L malic acid were added to the obtained composite metal salt solution to adjust the pH value of the composite metal salt solution to 5, thereby obtaining the high-efficiency composite eluent.
[0060] Under simulated experimental conditions, the obtained high-efficiency composite eluent was used to elute residual ammonium salts in weathering crust leaching type rare earth tailings. The specific steps include:
[0061] Weigh 1 g of rare earth tailings with a particle size of 150-200 mesh obtained by continuous graded elution method, add the obtained high-efficiency composite eluent at a solid-liquid ratio of 1:30 (g:mL), shake in a shaker at a temperature of 25°C for 3 hours, put it into a centrifuge at 4000r / min for 5 minutes to obtain a supernatant, and measure the ammonium content in the supernatant by Nessler's reagent spectrophotometry.
[0062] Collect rare earth tailings from the top, col and bottom of the rare earth mine, and load them into the dynamic column according to the quartering method. Set a certain sample loading height, and use a peristaltic pump to control the flow rate of the obtained high-efficiency composite eluent to 1.0 mol / min for dynamic experiments. Samples were collected at different times, and the ammonium content in the sample solution was determined by the Nessler reagent method. The time to reach equilibrium was 40 minutes, and the efficiency of the mixed salt solution in eluting ammonium in the rare earth tailings was 92%.
[0063] Example 6
[0064] A highly efficient composite eluent for residual ammonium salt in weathering crust leaching type rare earth tailings, the preparation method of which comprises the following steps:
[0065] 500 mL of 0.1 mol / L calcium chloride solution and 500 mL of 0.1 mol / L ferric chloride solution were mixed evenly, and a few drops (about 5 mL) of 0.01 mol / L citric acid were added to the obtained composite metal salt solution to adjust the pH value of the composite metal salt solution to 5, thereby obtaining the high-efficiency composite eluent.
[0066] Under simulated experimental conditions, the obtained high-efficiency composite eluent was used to elute residual ammonium salts in weathering crust leaching type rare earth tailings. The specific steps include:
[0067] Weigh 1 g of rare earth tailings with a particle size of 150-200 mesh obtained by continuous graded elution method, add the obtained high-efficiency composite eluent at a solid-liquid ratio of 1:30 (g:mL), shake in a shaker at a temperature of 25°C for 3 hours, put it into a centrifuge at 4000r / min for 5 minutes to obtain a supernatant, and measure the ammonium content in the supernatant by Nessler's reagent spectrophotometry.
[0068] Collect rare earth tailings from the top, col and bottom of the rare earth mine, and load them into the dynamic column according to the quartering method. Set a certain sample loading height, and use a peristaltic pump to control the flow rate of the obtained high-efficiency composite eluent to 0.5 mol / min for dynamic experiments. Samples were collected at different times, and the ammonium content in the sample solution was determined by the Nessler reagent method. The time to reach equilibrium was 45 minutes, and the efficiency of the mixed salt solution in eluting ammonium in the rare earth tailings was 94%.
[0069] Comparative Example 1
[0070] A high-efficiency composite eluent for ion-exchange ammonium in weathering crust leaching type rare earth tailings, the preparation method of which comprises the following steps:
[0071] 170 mL of 0.1 mol / L potassium chloride solution and 830 mL of 0.1 mol / L magnesium chloride solution were mixed evenly, and a few drops (about 5 mL) of 0.01 mol / L malic acid solution were added to the obtained composite metal salt solution to adjust the pH value of the composite metal salt solution to 5, thereby obtaining the high-efficiency composite eluent.
[0072] Under simulated experimental conditions, the obtained high-efficiency composite eluent is used to elute ion-exchange ammonium in weathering crust leaching type rare earth tailings. The specific steps include:
[0073] Weigh 1 g of rare earth tailings with a particle size of 150-200 mesh obtained by continuous graded elution method, add the obtained high-efficiency composite eluent at a solid-liquid ratio of 1:30 (g:mL), shake in a shaker at a temperature of 25°C for 3 hours, put it into a centrifuge at 4000r / min for 5 minutes to obtain a supernatant, and measure the ammonium content in the supernatant by Nessler's reagent spectrophotometry.
[0074] The rare earth tailings were collected from the top, col and bottom of the rare earth mine, and loaded into the dynamic column according to the quartering method. A certain loading height was set, and the obtained high-efficiency composite eluent was used to control the flow rate of 3.0 mol / min with a peristaltic pump for dynamic experiments. The samples were collected at different times, and the ammonium content in the sample solution was determined by the Nessler reagent method. The time to reach equilibrium was 30 minutes, and the efficiency of the mixed salt solution in eluting ammonium in the rare earth tailings was 85%.
[0075] Comparative Example 2
[0076] A high-efficiency composite eluent for ion-exchange ammonium in weathering crust leaching type rare earth tailings, the preparation method of which comprises the following steps:
[0077] 700 mL of 0.1 mol / L potassium chloride solution and 300 mL of 0.1 mol / L magnesium chloride solution were mixed evenly, and a 0.01 mol / L malic acid solution (about 12 mL) was added dropwise to the obtained composite metal salt solution, and the pH of the composite metal salt solution was adjusted to 2 to obtain the high-efficiency composite eluent.
[0078] Under simulated experimental conditions, the obtained high-efficiency composite eluent is used to elute ion-exchange ammonium in weathering crust leaching type rare earth tailings. The specific steps include:
[0079] Weigh 1 g of rare earth tailings with a particle size of 150-200 mesh obtained by continuous graded elution method, add the obtained high-efficiency composite eluent at a solid-liquid ratio of 1:30 (g:ml), shake in a shaker at a temperature of 25°C for 3 hours, put it into a centrifuge at 4000r / min for 5 minutes to obtain a supernatant, and measure the ammonium content in the supernatant by Nessler's reagent spectrophotometry.
[0080] Rare earth tailings were collected from the top, col and bottom of the rare earth mine, loaded into the dynamic column according to the quartering method, and a certain loading height was set. The obtained high-efficiency composite eluent was used to control the flow rate of 3.0 mol / min with a peristaltic pump for dynamic experiments. Samples were collected at different times, and the ammonium content in the sample solution was determined by the Nessler reagent method. The time to reach equilibrium was 30 minutes, and the efficiency of the mixed salt solution in eluting ammonium in the rare earth tailings was 90%.
[0081] Comparative Example 3
[0082] An eluent for ion-exchange ammonium in weathering crust leaching type rare earth tailings, and an application method thereof comprises the following steps:
[0083] Weigh 1 g of rare earth tailings with a particle size of 150-200 mesh obtained by continuous graded elution method, add a 0.1 mol / L NaCl solution at a solid-liquid ratio of 1:30 (g:mL), shake in a shaker at a temperature of 25°C for 3 hours, put it into a centrifuge at 4000 r / min for 5 minutes to obtain a supernatant, and measure the ammonium content in the supernatant by Nessler's reagent spectrophotometry.
[0084] Collect rare earth tailings from the top, col and bottom of the rare earth mine, load them into the dynamic column according to the quartering method, set a certain sample loading height, add 0.1mol / L NaCl solution, and use a peristaltic pump to control the flow rate to 2.5mol / min for dynamic experiments. Samples are collected at different times, and the ammonium content in the sample solution is determined by the Nessler reagent method. The time to reach equilibrium is 55min, and the efficiency of NaCl solution eluting ammonium in rare earth tailings is 35%.
[0085] Comparative Example 4
[0086] An eluent for ion-exchange ammonium in weathering crust leaching type rare earth tailings, and an application method thereof comprises the following steps:
[0087] Weigh 1 g of rare earth tailings with a particle size of 150-200 mesh obtained by continuous graded elution method, add 0.1 mol / L of AICl at a solid-liquid ratio of 1:30 (g:mL). 3 The solution was shaken in a shaker at 25°C for 3 h, and centrifuged at 4000 r / min for 5 min to obtain the supernatant. The ammonium content in the supernatant was measured by Nessler's reagent spectrophotometry.
[0088] Collect rare earth tailings from the top, bottom and bottom of the rare earth mine, load them into the dynamic column according to the quartering method, set a certain loading height, and add AICl with a concentration of 0.1 mol / L 3 The solution was subjected to dynamic experiments with a peristaltic pump controlling the flow rate to 2.0 mol / min. Samples were collected at different times and the ammonium content in the sample solution was determined using Nessler's reagent method. The time to reach equilibrium was 50 min. AICI 3 The efficiency of the solution in eluting ammonium from rare earth tailings is 70%.
[0089] Comparative Example 5
[0090] An eluent for ion-exchange ammonium in weathering crust leaching type rare earth tailings, and an application method thereof comprises the following steps:
[0091] Weigh 1 g of rare earth tailings with a particle size of 150-200 mesh obtained by continuous graded elution method, add 0.1 mol / L FeCl at a solid-liquid ratio of 1:30 (g:mL). 3 The solution was shaken in a shaker at 25°C for 3 h, and centrifuged at 4000 r / min for 5 min to obtain the supernatant. The ammonium content in the supernatant was measured by Nessler's reagent spectrophotometry.
[0092] Collect rare earth tailings from the top, bottom and bottom of the rare earth mine, load them into the dynamic column according to the quartering method, set a certain loading height, and add FeCl with a concentration of 0.1 mol / L 3 The solution was subjected to a dynamic experiment with a peristaltic pump controlling the flow rate to 1.5 mol / min. Samples were collected at different times and the ammonium content in the sample solution was determined using Nessler's reagent method. The time to reach equilibrium was 50 min. FeCl 3 The efficiency of the solution in eluting ammonium from rare earth tailings is 65%.
[0093] Comparative Example 6
[0094] An eluent for ion-exchange ammonium in weathering crust leaching type rare earth tailings, and an application method thereof comprises the following steps:
[0095] Weigh 1 g of rare earth tailings with a particle size of 150-200 mesh obtained by continuous graded elution method, add 0.1 mol / L KCl solution at a solid-liquid ratio of 1:30 (g:mL), shake in a shaker at a temperature of 25°C for 3 hours, put it into a centrifuge at 4000 r / min for 5 minutes to obtain a supernatant, and measure the ammonium content in the supernatant by Nessler's reagent spectrophotometry.
[0096] Collect rare earth tailings from the top, col and bottom of the rare earth mine, and load them into the dynamic column according to the quartering method. Set a certain sample loading height, add KCl solution with a concentration of 0.1mol / L, and use a peristaltic pump to control the flow rate to 1.0mol / min for dynamic experiments. Samples are collected at different times, and the ammonium content in the sample solution is determined by the Nessler reagent method. The time to reach equilibrium is 50min, and the efficiency of KCl solution eluting ammonium in rare earth tailings is 82%.
[0097] Comparative Example 7
[0098] An eluent for ion-exchange ammonium in weathering crust leaching type rare earth tailings, and an application method thereof comprises the following steps:
[0099] Weigh 1 g of rare earth tailings with a particle size of 150-200 mesh obtained by continuous graded elution method, add 0.1 mol / L MgCl at a solid-liquid ratio of 1:30 (g:mL). 2 The solution was shaken in a shaker at 25°C for 3 h, and centrifuged at 4000 r / min for 5 min to obtain the supernatant. The ammonium content in the supernatant was measured by Nessler's reagent spectrophotometry.
[0100] Collect rare earth tailings from the top, bottom and bottom of the rare earth mine, load them into the dynamic column according to the quartering method, set a certain sample loading height, and add MgCl with a concentration of 0.1 mol / L 2 The solution was stirred at a flow rate of 0.5 mol / min using a peristaltic pump for dynamic experiments. Samples were collected at different times and the ammonium content in the sample solution was determined using the Nessler reagent method. The time to reach equilibrium was 50 min. MgCl 2 The efficiency of the solution in eluting ammonium from rare earth tailings is 80%.
[0101] The above embodiments are only examples for clear explanation, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, so the obvious changes or modifications derived are still within the protection scope of the invention.
Claims
1. A highly efficient composite eluent for ion-exchange ammonium in weathering crust leaching type rare earth tailings, characterized in that: It is a mixed aqueous solution formed by a composite metal salt and an acid; wherein the metal elements corresponding to the composite metal salt are two of K, Ca, Mg, and Fe, and the molar ratio thereof is 1:4 to 4:1; and the acid is one or more of hydrochloric acid, oxalic acid, citric acid, and malic acid; Adding acid dropwise to the composite metal salt solution to adjust the pH value of the high-efficiency composite eluent to 4-5; The composite metal salt is a soluble hydrochloride; The high-efficiency composite eluent has an efficiency of 99% in eluting ammonium from rare earth tailings.
2. The high-efficiency composite eluent according to claim 1, characterized in that: The composite metal salt is potassium salt and magnesium salt.
3. The high-efficiency composite eluent according to claim 2, characterized in that: The molar ratio of the potassium salt to the magnesium salt is 7:(3-4).
4. The high-efficiency composite eluent according to claim 1, characterized in that: The concentration of the composite metal salt is 0.02-0.2 mol / L.
5. The method for preparing the high-efficiency composite eluent according to any one of claims 1 to 4, comprising the following steps: 1) preparing aqueous solutions of metal salts of different concentrations respectively; 2) The obtained aqueous solutions of metal salts with different concentrations are mixed evenly according to proportion to obtain a composite metal salt solution, and then an acid is added to adjust the pH value of the obtained mixed solution to obtain the composite salt high-efficiency eluent.
Citation Information
Patent Citations
Ion absorpt deposit eluting agent and eluting method thereof
CN111088054A
Method for removing ionic rare earth ore ammonia nitrogen pollution in situ by using eluting agent
CN112813289A